Steel ingot isothermal forging process

Through isothermal forging technology, thermal insulation paint and lubricant are used to maintain the constant temperature of the steel ingot, which solves the problem of uneven grain size in the forging of high alloy steel ingots, and improves the forging efficiency and finished product quality.

CN118989204APending Publication Date: 2024-11-22ZUNYI XINLITE METAL MATERIAL TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411192618.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the forging process, the grain size of the forged steel ingots is uneven at both ends, which affects the quality and is low forging efficiency.

Method used

Isothermal forging technology, including heating, brushing insulation paint, wrapping insulation cotton and adding lubricants, ensuring that the steel ingot maintains a constant temperature during forging, and through the composition of insulation paint and the use of lubricants, the material deformation resistance and the plastic flow capacity are reduced.

Benefits of technology

The temperature consistency of the head, tail, surface and core of the ingot is achieved, the deformation time is extended, the dimensional accuracy and tissue uniformity are improved, and the mechanical properties and grain size uniformity are improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a steel ingot isothermal forging process in the technical field of metal forging, which comprises the following steps: step 1, heating: heating a steel ingot in a heating furnace until the steel ingot reaches a specified temperature; (2) paint brushing is conducted, specifically, the surface of the steel ingot heated in the step (1) is coated with heat preservation paint; the steel ingot is wrapped with heat preservation cotton after the heat preservation paint is brushed on the steel ingot, and a lubricating agent is added between the heat preservation cotton and the steel ingot when the steel ingot is wrapped so as to increase the lubricity; and fourthly, forging is conducted, specifically, the steel ingot wrapped with the heat preservation cotton in the third step is subjected to heat preservation for a certain time and then placed in a forging and pressing machine to be forged. According to the scheme, the problem that in the existing steel ingot forging process, due to temperature loss, the grain size difference of the two ends of the forged steel ingot is large is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal forging, and in particular to an isothermal forging process for steel ingots. Background Art

[0002] Ingots are a crucial intermediate product in the steelmaking process. They are formed by cooling and solidifying molten steel into a solid block of a specific shape and size. Ingot processing typically involves heating raw materials to a molten state in a steelmaking furnace to form molten steel. The molten steel then undergoes further processing to remove impurities and adjust its chemical composition to achieve the desired steel grade specifications. The refined molten steel is poured into pre-prepared molds, known as ingot molds. The shape and size of the ingot molds determine the final form of the ingot. Once the molten steel cools and forms within the molds, it is demolded and subsequently subjected to heat treatment, forging, and other processing steps.

[0003] During the forging process, the steel ingot undergoes plastic deformation at high temperature, which can refine the grains and eliminate dendritic segregation and porosity that may occur during casting, thereby improving the microstructure of the steel and improving its mechanical properties, such as strength, toughness, plasticity and fatigue strength.

[0004] In the forging of high-alloy steel ingots, the forging temperature range of some high-alloy steel ingots is relatively narrow, which may only be a few tens of degrees. Therefore, when forging such high-alloy steel ingots, the temperature will drop below the forging temperature range after a short period of time after being struck by the forging hammer. Therefore, it is necessary to heat it again to a suitable temperature before forging. This operation is cumbersome, inconvenient, and inefficient. Moreover, when forging the high-alloy steel ingot, the temperature of the rear end gradually decreases as the front end is forged. When forging to the rear end, the temperature is relatively low, which results in a large difference in grain size at both ends of the forged high-alloy steel ingot, making the grain size at both ends of the forged high-alloy steel ingot uneven, affecting the quality of the steel ingot. Summary of the Invention

[0005] The present invention aims to provide an isothermal forging process for steel ingots to solve the problem of large grain size difference between the two ends of the forged steel ingots due to temperature loss during the current steel ingot forging process.

[0006] To solve the above technical problems, the present invention provides the following technical solution: an isothermal forging process for a steel ingot, comprising the following steps:

[0007] Step 1: Heating: Place the steel ingot in a heating furnace and heat it until the ingot reaches the specified temperature;

[0008] Step 2: Paint: Apply thermal insulation paint to the surface of the steel ingot after heating in step 1;

[0009] Step 3: Wrapping with cotton: After the steel ingot is painted with thermal insulation paint, wrap the steel ingot with thermal insulation cotton. When wrapping the steel ingot, add lubricant between the thermal insulation cotton and the steel ingot to increase lubricity.

[0010] Step 4: Forging: The steel ingot wrapped with insulation cotton in step 3 is kept warm for a certain period of time before being placed in a forging machine for forging.

[0011] Furthermore, the thermal insulation paint comprises Al2O3 85-93%, Cr2O3 7-15% and Na2SiO3 in terms of mass percentage, and the mass percentage of Na2SiO3 is 10% of the mass of the mixture of Al2O3 and Cr2O3.

[0012] Furthermore, when preparing the thermal insulation paint, Al2O3 powder and Cr2O3 powder are evenly mixed according to mass percentage, and then 10% of the mass of Na2SiO3 is added to the evenly mixed Al2O3 powder and Cr2O3 powder, and then fully stirred to obtain the thermal insulation paint.

[0013] Furthermore, the thermal insulation paint comprises 92% Al2O3, 8% Cr2O3 and Na2SiO3 by mass, and the mass percentage of Na2SiO3 is 10% of the mass of the mixture of Al2O3 and Cr2O3.

[0014] Furthermore, the lubricant is iron oxide or quartz sand.

[0015] Furthermore, the thermal insulation wool is made of asbestos.

[0016] Beneficial effects of the present invention:

[0017] 1. Reduce the deformation resistance of the material, so that the temperature of the head, tail, surface and core of the steel ingot is basically the same, and the steel ingot cools down very slowly due to the covering of the thermal insulation material, so that the softening process of the material is more complete, and the deformation time of the material is extended at a lower deformation speed.

[0018] 2. Improve the plastic flow ability of the material. Since the surface of the billet is covered with insulation material, the billet cools down very slowly and the overall temperature of the ingot is uniform, which can fully carry out the material softening process, thereby improving the plastic flow ability of the material and healing the defects.

[0019] 3. Improve the dimensional accuracy of material forming, achieve good surface quality, uniform structure, and excellent performance. During isothermal forging, since the billet deformation temperature remains essentially constant, the heating temperature can be 50-100°C lower than that of conventional deformation. Therefore, the material's start forging temperature can be appropriately lowered, and single-fire forming can be used while increasing the material deformation. The increased deformation and lower forging temperature can improve material performance. Before forging, quartz sand or iron oxide can be sprinkled on the surface of the insulation material to improve lubrication conditions and make the billet deformation more uniform. This results in a uniform structure after forming, and more uniform overall mechanical properties and grain size. DETAILED DESCRIPTION

[0020] The following is further described in detail through specific implementation methods:

[0021] Example 1

[0022] A steel ingot isothermal forging process comprises the following steps:

[0023] Step 1: Heating: Place the steel ingot in a heating furnace and heat it until the ingot reaches the specified temperature;

[0024] Step 2: Paint: Apply thermal insulation paint to the surface of the steel ingot after heating in step 1;

[0025] The thermal insulation paint comprises, by mass percentage, 85% Al2O3, 15% Cr2O3, and Na2SiO3, with the mass percentage of Na2SiO3 being 10% of the mass of the mixture of Al2O3 and Cr2O3. During preparation, the Al2O3 powder and Cr2O3 powder are uniformly mixed according to mass percentages. Then, Na2SiO3, which accounts for 10% of the total mass of the mixed Al2O3 and Cr2O3 powders, is added to the uniformly mixed Al2O3 and Cr2O3 powders, and the mixture is thoroughly stirred to obtain the thermal insulation paint.

[0026] Step 3: Wrapping: After the steel ingot is painted with insulation paint, wrap it with insulation cotton made of asbestos. When wrapping the steel ingot, add lubricant between the insulation cotton and the steel ingot to increase lubricity. The lubricant is iron oxide or quartz sand.

[0027] Step 4: Forging: The steel ingot wrapped with insulation cotton in step 3 is kept warm for a certain period of time before being placed in a forging machine for forging.

[0028] Example 2

[0029] A steel ingot isothermal forging process comprises the following steps:

[0030] Step 1: Heating: Place the steel ingot in a heating furnace and heat it until the ingot reaches the specified temperature;

[0031] Step 2: Paint: Apply thermal insulation paint to the surface of the steel ingot after heating in step 1;

[0032] The thermal insulation paint comprises, by mass percentage, 93% Al2O3, 7% Cr2O3, and Na2SiO3, with the mass percentage of Na2SiO3 being 10% of the mass of the combined Al2O3 and Cr2O3. During preparation, the Al2O3 powder and the Cr2O3 powder are uniformly mixed according to mass percentages. Then, Na2SiO3, representing 10% of the total mass of the mixed Al2O3 and Cr2O3 powders, is added to the uniformly mixed Al2O3 and Cr2O3 powders, and the mixture is thoroughly stirred to produce the thermal insulation paint.

[0033] Step 3: Wrapping: After the steel ingot is painted with insulation paint, wrap it with insulation cotton made of asbestos. When wrapping the steel ingot, add lubricant between the insulation cotton and the steel ingot to increase lubricity. The lubricant is iron oxide or quartz sand.

[0034] Step 4: Forging: The steel ingot wrapped with insulation cotton in step 3 is kept warm for a certain period of time before being placed in a forging machine for forging.

[0035] Example 3

[0036] A steel ingot isothermal forging process comprises the following steps:

[0037] Step 1: Heating: Place the steel ingot in a heating furnace and heat it until the ingot reaches the specified temperature;

[0038] Step 2: Paint: Apply thermal insulation paint to the surface of the steel ingot after heating in step 1;

[0039] The thermal insulation paint comprises, by mass percentage, 92% Al2O3, 8% Cr2O3, and Na2SiO3, with the mass percentage of Na2SiO3 being 10% of the mass of the combined Al2O3 and Cr2O3. During preparation, the Al2O3 powder and the Cr2O3 powder are uniformly mixed according to mass percentages. Then, Na2SiO3, representing 10% of the total mass of the mixed Al2O3 and Cr2O3 powders, is added to the uniformly mixed Al2O3 and Cr2O3 powders, and the mixture is thoroughly stirred to produce the thermal insulation paint.

[0040] Step 3: Wrapping: After the steel ingot is painted with insulation paint, wrap it with insulation cotton made of asbestos. When wrapping the steel ingot, add lubricant between the insulation cotton and the steel ingot to increase lubricity. The lubricant is iron oxide or quartz sand.

[0041] Step 4: Forging: The steel ingot wrapped with insulation cotton in step 3 is kept warm for a certain period of time before being placed in a forging machine for forging.

Claims

1. A steel ingot isothermal forging process, characterized in that: The following steps are involved: Step 1, heating: placing the steel ingot into a heating furnace for heating until the steel ingot reaches a specified temperature; Step 2, painting: apply heat-insulating paint on the surface of the steel ingot after heating in step 1; Step 3, wrapping with cotton: After the steel ingot is painted with thermal insulation paint, wrap the steel ingot with thermal insulation cotton. When wrapping the steel ingot, add lubricant between the thermal insulation cotton and the steel ingot to increase lubricity; Step 4: Forging: The steel ingot wrapped with the insulation cotton in step 3 is kept warm for a certain period of time and then placed in a forging machine for forging.

2. The isothermal forging process for steel ingots according to claim 1, characterized in that: The thermal insulation paint comprises 85-93% of Al2O3, 7-15% of Cr2O3 and Na2SiO3 by mass percentage, wherein the mass percentage of Na2SiO3 is 10% of the mass of the mixture of Al2O3 and Cr2O3.

3. The isothermal forging process for steel ingots according to claim 2, characterized in that: When preparing the thermal insulation paint, Al2O3 powder and Cr2O3 powder are uniformly mixed according to mass percentage, and then 10% of the mass of Na2SiO3 is added to the uniformly mixed Al2O3 powder and Cr2O3 powder, and then the mixture is fully stirred to obtain the thermal insulation paint.

4. The isothermal forging process for steel ingots according to claim 3, characterized in that: The thermal insulation paint comprises 92% Al2O3, 8% Cr2O3 and Na2SiO3 by mass percentage, and the mass percentage of Na2SiO3 is 10% of the mass of the mixture of Al2O3 and Cr2O3.

5. The isothermal forging process for steel ingots according to claim 4, characterized in that: The lubricant is iron oxide or quartz sand.

6. The isothermal forging process for steel ingots according to claim 5, characterized in that: The thermal insulation wool is made of asbestos.

Citation Information

Patent Citations

  • Heat-processing temperature-cntrolled heat-insulation material, its preparing method and use

    CN101070223A

  • GH864 high-temperature alloy die forging method

    CN105478643A

  • Forming method of 718 plus special-shaped ring forge piece

    CN109530607A

  • Steel ingot or billet heat preservation device used in high-temperature alloy forging process and method of steel ingot or billet heat preservation device

    CN110947899A

  • TiAl-based alloy stator blade isothermal forming manufacturing method and device thereof

    CN112122523A