Method for improving crushing pressure of jet mill in silver powder preparation process

By coating silver powder with liquid unsaturated fatty acids and increasing the crushing pressure in the airflow mill, the problems of insufficient crushing pressure and powder back spraying in the prior art are solved, and more efficient crushing and plasticizing are achieved, which improves the product Surface smoothness and mass.

CN118989338APending Publication Date: 2024-11-22SHENZHEN HASHEN TECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411106574.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The crushing pressure of existing silver powder during the airflow grinding process usually can only reach 0.6-0.8Mpa, and powder backspray is prone to occur at higher pressures, resulting in poor crushing effect and product quality.

Method used

By mixing silver powder with liquid unsaturated fatty acids for coating, and mechanically crushing in subsequent airflow mills, the crushing pressure is increased to more than 0.8Mpa, and the liquid droplet and surface tension of liquid unsaturated fatty acids can make the silver powder larger Effective crushing under pressure.

Benefits of technology

Achieve a larger range of crushing and shaping of silver powder in airflow grinding, improve the surface smoothness and related properties of the powder, enhance the crushing pressure threshold, avoid powder back spraying, and improve product uniformity and quality stability. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989338A_ABST
    Figure CN118989338A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of silver powder preparation, and discloses a method for improving jet mill crushing pressure in the silver powder preparation process. The method for improving the crushing pressure of the jet mill in the silver powder preparation process comprises the steps that silver powder and liquid unsaturated fatty acid are mixed and coated, coated silver powder is obtained, the coated silver powder is mechanically crushed, then the powder is crushed and dispersed through the jet mill, and the crushing pressure of the jet mill reaches 0.8 Mpa or above. According to the method, a small amount of liquid unsaturated fatty acid is added into the silver powder, so that the silver powder can be coated, the surface of the silver powder is flat and smooth, and meanwhile, the crushing pressure of jet mill crushing can be increased during subsequent jet mill crushing, so that shaping in a larger range is realized; therefore, the adjusting range of the morphology, the viscosity of the slurry prepared from the powder and other properties is larger.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silver powder preparation, in particular to a method for improving the pulverizing pressure of a jet mill in a silver powder preparation process. Background Art

[0002] Metal micro-nano powders have many unique physical, chemical and material properties, and therefore have a wide range of applications in materials science, energy, biomedicine, electronic devices and other fields. In the field of materials science, metal powders can be used to prepare high-performance composite materials, micro-nano coatings, etc., with excellent mechanical properties and surface properties. In the energy field, metal micro-nano powders can be used to prepare energy materials such as catalysts, fuel cells, and lithium-ion batteries to improve energy conversion efficiency and energy storage performance. In the field of biomedicine, metal micro-nano powders can be used in bioimaging, drug carriers, biosensors, etc., with the advantages of biocompatibility and drug delivery. In the field of electronic devices, metal micro-nano powders can be used in conductive inks, flexible electronic devices, sensors, etc., with excellent electrical and conductive properties.

[0003] Metal micro-nano powders, including silver powder and silver-coated copper conductive powders, are widely used in photovoltaic conductive pastes. The powders need to have good conductive properties to ensure high conversion efficiency of photovoltaic cells. Secondly, micro-nano powders need to have good dispersibility and stability to ensure uniform distribution in the conductive paste and maintain stable performance. In addition, for silver-coated copper powders, they also need to have good corrosion resistance to ensure that no corrosion occurs during the long-term use of photovoltaic cells. In summary, the application of metal micro-nano powders in photovoltaic conductive pastes needs to meet multiple requirements such as conductivity, dispersibility, stability and corrosion resistance. The preparation method, post-treatment and dispersion method of metal micro-nano powders have an important influence on their application performance.

[0004] The preparation methods of metal micro-nano powders include physical methods and chemical methods. Physical methods include inert gas condensation, mechanical alloying, laser thermal evaporation, etc., which mainly aggregate metal atoms or clusters into micro-nano-scale powders by physical means. Chemical methods include wet reduction, solvent thermal method, chemical vapor deposition, sol-gel method, etc., which synthesize metal micro-nano powders through chemical reactions. Post-treatment methods of metal micro-nano powders include surface modification, heat treatment, functionalization, and crushing and dispersion. Surface modification is to change the surface properties of metal micro-nano powders by coating organic matter, oxides or other functional compounds to improve their dispersibility and stability. Heat treatment is to change the crystal structure and grain size of metal micro-nano powders by temperature treatment to improve their thermal stability and mechanical properties. Functionalization is to change the surface chemical properties of metal micro-nano powders by introducing functional groups, changing surface charges and other functionalization methods to improve their application performance in various materials. Since metal micro-nano powders often have agglomeration problems during the preparation process, crushing and dispersion are needed to improve their dispersibility in order to better obtain the properties of their single particle powders. The dispersion and crushing methods of metal micro-nano powders include mechanical dispersion and chemical dispersion. Mechanical dispersion is to directly disperse metal micro-nano powders or disperse and crush them in solvents by mechanical means such as ultrasound, grinding, stirring, etc., so that the agglomerated clusters become particles with smaller particle sizes. Chemical dispersion is to improve the dispersibility and stability of metal micro-nano powders in solvents by chemical means such as surfactants and dispersants.

[0005] Metal micro-nano powders are widely used in many product fields including photovoltaics. Their preparation methods, post-treatment and dispersion and crushing methods have an important impact on their application performance and need to be reasonably selected and optimized in combination with specific application requirements. The more common post-treatment and dispersion and crushing methods of silver micro-nano powders commonly used in the photovoltaic field include powder surface modification, coating, shaping and dispersion and crushing. After the powder is treated by air flow milling or crushing, the surface becomes smoother, which is conducive to reducing the friction resistance between powders, improving the fluidity of silver powder in the slurry, reducing the viscosity of the slurry, and improving its printing performance. At the same time, the flat and smooth surface is conducive to the dispersion between silver powder particles, making it easier for silver powder to be evenly dispersed in liquid or solid matrices, which is conducive to improving the uniformity and quality stability of the product. In addition, the flat and smooth surface after crushing and dispersion is conducive to improving the reactivity and reaction stability of silver powder, making the chemical reaction activity of the powder more balanced and stable, and for silver powder, its sintering reaction temperature changes significantly.

[0006] However, when the silver powder is currently being jet milled, the pulverizing pressure of the jet mill can usually only reach 0.6-0.8Mpa, and some silver powders cannot even reach a pressure of 0.6Mpa. When the pulverizing pressure continues to increase, the powder feed pressure will not be able to suppress the pulverizing pressure, that is, powder backsplash frequently occurs. The low pulverizing pressure and unstable process lead to poor pulverizing effect and product quality of the jet mill.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The object of the present invention is to provide a method for improving the pulverizing pressure of a jet mill in the process of preparing silver powder.

[0009] The present invention is achieved in that:

[0010] In a first aspect, the present invention provides a method for improving the crushing pressure of a jet mill during the preparation of silver powder, comprising: mixing silver powder with liquid unsaturated fatty acid for coating to obtain coated silver powder, mechanically crushing the coated silver powder, and then crushing and dispersing the powder using a jet mill, wherein the crushing pressure of the jet mill reaches above 0.8 MPa.

[0011] In an optional embodiment, the liquid unsaturated fatty acid includes at least one of oleic acid, palmitoleic acid, trans-oleic acid, ricinoleic acid, erucic acid, linoleic acid, linolenic acid and omega-7 fatty acids.

[0012] In an optional embodiment, the liquid unsaturated fatty acid and the silver powder are dry coated, and the mass ratio of the silver powder to the liquid unsaturated fatty acid is 100:0.1-0.2.

[0013] In an optional embodiment, the liquid unsaturated fatty acid and the silver powder are wet coated. During the wet coating, the liquid unsaturated fatty acid is first mixed with a solvent to form a liquid unsaturated fatty acid solution, and then the silver powder is mixed with the liquid unsaturated fatty acid solution. The mass ratio of the silver powder to the liquid unsaturated fatty acid solution is 100:1-2.

[0014] Preferably, the mass ratio of the liquid unsaturated fatty acid to the solvent in the liquid unsaturated fatty acid solution is 10-20:100;

[0015] Preferably, the solvent is ethanol.

[0016] In an optional embodiment, the wet coating further comprises drying the coated silver powder;

[0017] Preferably, the drying comprises drying at 45-80°C.

[0018] In an optional embodiment, the coating is carried out under stirring, with a stirring speed of 100-400RPM and a stirring time of 3-10min.

[0019] In an optional embodiment, the mechanical pulverization includes using a crushing blade to pulverize the coated silver powder to a particle size of 0.5-3 μm.

[0020] In an optional embodiment, the feed rate of the jet mill is 20-60 kg / h, and the gas flow rate of the jet mill is 1.5-7.5 m 3 / min.

[0021] In an optional embodiment, the preparation method of the silver powder comprises: mixing a silver salt solution, a dispersant base solution and a reducing agent solution to react, stirring after the reaction is completed and adding a flocculant to flocculate, then separating the solid from the liquid, washing the solid until the conductivity of the washing liquid is reduced to 50 μS / cm, and then stopping washing to obtain silver powder;

[0022] Preferably, the flocculant includes at least one of polyacrylamide, polyacryl alcohol, polyacryl ether, fatty acid and fatty acid salt.

[0023] In an optional embodiment, the method for mixing the silver salt solution, the dispersant base solution and the reducing agent solution comprises: injecting the silver salt solution and the reducing agent solution into the dispersant base solution respectively through a peristaltic pump, the injection time is 5-12 minutes, maintaining a water bath condition of 15-40° C. during the reaction, and using a mechanical stirring paddle to stir at a speed of 100-300RPM;

[0024] Preferably, the concentration of the silver salt solution is 0.1-3 mol / L, the concentration of the dispersant base solution is 2-10wt%, the concentration of the reducing agent is 0.1-15 mol / L, and the amount of the dispersant in the dispersant base solution is 10-50% of the mass of the silver particles;

[0025] Preferably, the silver salt in the silver salt solution includes at least one of silver nitrate and silver sulfate;

[0026] Preferably, the dispersant in the dispersant base solution comprises at least one of polyvinyl pyrrolidone, polyethylene glycol, gum arabic, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum and polyethylene glycol esters of fatty acids;

[0027] Preferably, the reducing agent comprises at least one of ascorbic acid, hydrazine hydrate, sodium borohydride and formalin.

[0028] The present invention has the following beneficial effects:

[0029] The method for improving the crushing pressure of the airflow mill in the process of preparing silver powder provided by the present invention can not only realize the coating of the silver powder to make its surface flat and smooth by adding a small amount of liquid unsaturated fatty acid to the silver powder, but also help to increase the crushing pressure of the airflow mill during the subsequent airflow mill crushing. The reason is that the liquid unsaturated fatty acid itself is in the form of droplets, and its surface tension acts on the silver powder particles, so that it tends to aggregate to reduce the specific surface area. This increases the mutual force between the silver powders attached to it, and can withstand a greater crushing pressure in the feeding device of the airflow mill without producing a back-spray effect. Therefore, the kinetic energy of mutual collision in the silver powder airflow mill is greater, and the mutual collision is more sufficient, which ultimately leads to the improvement of the surface morphology and related properties of the silver powder. On the other hand, the liquid coating agent has better fluidity and may have better dispersion and coating effects on the surface of the silver powder. By increasing the crushing pressure, a larger range of crushing pressure can be achieved for shaping, so the adjustment range of its morphology, the viscosity of the slurry prepared by the powder and other properties is larger.

[0030] For the jet mill, its working state needs to roughly meet the formula of "feed optimization pressure A + feed pressure B ≥ crushing pressure C" to ensure normal operation, otherwise powder back-spray is very likely to occur. For a determined jet mill working pipeline, the feed pressure B is a certain value, and its value is related to the output pressure of the air compressor and gas tank and the line structure, and can be adjusted to a certain extent through the valve. However, generally the feed pressure and crushing pressure come from the same main gas pipeline (otherwise, another set of air compressors and gas system needs to be set up, which is more expensive), so the feed pressure and crushing pressure are controlled and mutually restricted by the total pipeline gas volume, air pressure and each branch valve. The feed optimization pressure A is a parameter related to the powder state, feed speed, and feed device structure. Among them, the powder state involves factors such as the density and dispersion of the powder material. The powder feeding speed is positively correlated with the A parameter within a certain range, and can be adjusted and affect the A parameter to a certain extent, but too high a feeding speed will lead to blockage of the feeding pipeline and the powder blockage in the airflow mill cavity, which will lead to insufficient powder collision. The present invention affects the microscopic dispersion state of the powder through the coating method, increases the feed optimization pressure, and thus increases the threshold of the crushing pressure. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0032] Figure 1This is a SEM image of the silver powder obtained in step S1 of the method for improving the crushing pressure of the airflow mill in the preparation process of silver powder provided in Example 1 of the present application;

[0033] Figure 2 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverizing pressure of the airflow mill in the preparation process of silver powder provided in Example 1 of the present application at a pulverizing pressure of 0.6 MPa;

[0034] Figure 3 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the airflow mill crushing pressure in the silver powder preparation process provided in Example 1 of the present application at a crushing pressure of 0.8 MPa;

[0035] Figure 4 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverizing pressure of a jet mill in the preparation process of silver powder provided in Example 1 of the present application at a pulverizing pressure of 1 MPa;

[0036] Figure 5 This is a SEM image of the silver powder obtained in step S1 of the method for improving the crushing pressure of the airflow mill in the preparation process of silver powder provided in Example 2 of the present application;

[0037] Figure 6 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the airflow mill crushing pressure in the silver powder preparation process provided in Example 2 of the present application at a crushing pressure of 0.6 MPa;

[0038] Figure 7 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the airflow mill crushing pressure in the silver powder preparation process provided in Example 2 of the present application at a crushing pressure of 0.8 MPa;

[0039] Figure 8 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverizing pressure of the airflow mill in the preparation process of silver powder provided in Example 2 of the present application at a pulverizing pressure of 1 MPa;

[0040] Fig. 9 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverizing pressure of the airflow mill in the preparation process of silver powder provided in Example 3 of the present application at a pulverizing pressure of 0.6 MPa;

[0041] Fig.10 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the airflow mill crushing pressure in the silver powder preparation process provided in Example 3 of the present application at a crushing pressure of 0.8 MPa;

[0042] Fig.11This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverizing pressure of a jet mill in the preparation process of silver powder provided in Example 3 of the present application at a pulverizing pressure of 1 MPa;

[0043] Fig.12 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the airflow mill crushing pressure in the silver powder preparation process provided in Example 4 of the present application at a crushing pressure of 0.6 MPa;

[0044] Fig.13 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverizing pressure of the airflow mill in the preparation process of silver powder provided in Example 4 of the present application at a pulverizing pressure of 0.8 MPa;

[0045] Fig.14 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverizing pressure of the airflow mill in the preparation process of silver powder provided in Example 4 of the present application at a pulverizing pressure of 1 MPa;

[0046] Fig.15 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the airflow mill crushing pressure in the silver powder preparation process provided in Example 5 of the present application at a crushing pressure of 0.6 MPa;

[0047] Fig.16 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the airflow mill crushing pressure in the silver powder preparation process provided in Example 5 of the present application at a crushing pressure of 0.8 MPa;

[0048] Fig.17 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverizing pressure of the airflow mill in the preparation process of silver powder provided in Example 5 of the present application at a pulverizing pressure of 1 MPa;

[0049] Fig.18 This is a SEM image of the silver powder obtained by the method step S1 provided in Comparative Example 1 of the present application;

[0050] Fig.19 This is a SEM image of a product prepared by crushing and pressing the initial sample obtained by the method provided in Comparative Example 1 of the present application at 0.6 MPa;

[0051] Fig. 20 This is a SEM image of the silver powder obtained by the method step S1 provided in Comparative Example 2 of the present application;

[0052] Fig.21 This is a SEM image of a product prepared by crushing and pressing the initial sample obtained by the method provided in Comparative Example 2 of the present application at 0.6 MPa;

[0053] Fig. 22 This is a SEM image of the silver powder obtained by preparing step S1 of the method provided in Comparative Example 3 of the present application;

[0054] Fig.23 This is a SEM image of a product prepared by crushing and pressing the initial sample obtained by the method provided in Comparative Example 3 of the present application at 0.6 MPa;

[0055] Fig.24 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverization pressure of the airflow mill in the preparation process of silver powder provided in Comparative Example 4 of the present application at a pulverization pressure of 0.6 MPa;

[0056] Fig.25 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverizing pressure of the airflow mill in the preparation process of silver powder provided in Comparative Example 4 of the present application at a pulverizing pressure of 0.8 MPa;

[0057] Fig.26 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverization pressure of the airflow mill in the preparation process of silver powder provided in Comparative Example 4 of the present application at a pulverization pressure of 1 MPa;

[0058] Fig. 27 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverization pressure of the airflow mill in the preparation process of silver powder provided in Comparative Example 5 of the present application at a pulverization pressure of 0.6 MPa;

[0059] Fig.28 This is a SEM image of a product prepared by the initial preparation sample prepared by the method for improving the pulverizing pressure of the airflow mill in the preparation process of silver powder provided in Comparative Example 5 of the present application at a pulverizing pressure of 0.8 MPa;

[0060] Fig.29 This is a SEM image of the product prepared by the initial preparation sample prepared by the method for improving the airflow mill pulverizing pressure in the silver powder preparation process provided in Comparative Example 5 of the present application at a pulverizing pressure of 1 MPa. DETAILED DESCRIPTION

[0061] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0062] The present invention provides a method for improving the crushing pressure of a jet mill in a silver powder preparation process, comprising: mixing silver powder with liquid unsaturated fatty acid for coating to obtain coated silver powder, mechanically crushing the coated silver powder, and then crushing and dispersing the powder by a jet mill, wherein the crushing pressure of the jet mill can reach above 0.8Mpa.

[0063] In the present invention, by coating the silver powder with liquid unsaturated fatty acid, the final grinding pressure of the air flow mill can be significantly increased, so that the silver powder can be ground and shaped under a greater pressure, and the silver powder is spherical after grinding and has a smooth surface.

[0064] Specifically, the method includes the following steps:

[0065] S1. Preparation of silver powder.

[0066] The silver salt solution, the dispersant base solution and the reducing agent solution are mixed to react. After the reaction is completed, stirring is maintained and a flocculant is added for flocculation. Subsequently, the solid and the liquid are separated. The solid is washed until the conductivity of the washing liquid decreases to 50 μS / cm, and then the washing is stopped to obtain silver powder.

[0067] The method for mixing the silver salt solution, the dispersant base solution and the reducing agent solution comprises: injecting the silver salt solution and the reducing agent solution into the dispersant base solution respectively through a peristaltic pump, the injection time is 5-12 minutes, maintaining a water bath condition of 15-40°C during the reaction, and using a mechanical stirring paddle to stir at a speed of 100-300RPM.

[0068] The concentration of the silver salt solution is 0.1-3 mol / L, the concentration of the dispersant base solution is 2-10wt%, the concentration of the reducing agent is 0.1-15 mol / L, and the amount of the dispersant in the dispersant base solution is 10-50% of the mass of the silver particles.

[0069] In the present invention, the silver salt in the silver salt solution includes but is not limited to at least one of silver nitrate and silver sulfate; the dispersant in the dispersant base solution includes but is not limited to at least one of polyvinyl pyrrolidone, polyethylene glycol, gum arabic, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum and fatty acid polyethylene glycol ester; the reducing agent includes but is not limited to at least one of ascorbic acid, hydrazine hydrate, sodium borohydride and formalin. The flocculant includes but is not limited to at least one of polyacrylamide, polyacryl alcohol, polyacryl ether, fatty acid and fatty acid salt.

[0070] S2. Coating.

[0071] The silver powder is mixed with liquid unsaturated fatty acid for coating to obtain coated silver powder.

[0072] The liquid unsaturated fatty acids include at least one of oleic acid, palmitoleic acid, trans-oleic acid, ricinoleic acid, erucic acid, linoleic acid, linolenic acid and omega-7 fatty acids.

[0073] In the present invention, liquid unsaturated fatty acid is selected as the coating agent instead of the conventional solid coating agent. The difference between the two coating agents is mainly that the liquid unsaturated fatty acid itself is in the form of a droplet, and its surface tension acts on the silver powder particles, causing them to tend to aggregate to reduce the specific surface area. This increases the mutual force between the silver powders attached to it, and can withstand a larger crushing pressure in the feed device of the airflow mill without generating a back-spray effect. Therefore, the kinetic energy of the silver powders colliding with each other in the airflow mill is greater, and the mutual collision is more sufficient, which ultimately leads to the improvement of the surface morphology and related properties of the silver powder. Although the coating agent, which is solid in itself, is dissolved by solvents such as ethanol, it is solid and coated on the surface of the silver powder after the alcohol evaporates. Although the isolation effect between the silver powders is good, the powder is very easy to scatter during the process of entering the feed device of the airflow mill, and back-spray may occur under low crushing pressure conditions, and frequent back-spraying causes the airflow mill to shut down. On the other hand, the liquid coating agent has better fluidity, and the dispersion and coating effect on the surface of the silver powder are more uniform.

[0074] Furthermore, liquid unsaturated fatty acids are more likely to form droplets as coating agents than solid coating agents. This is because the intermolecular forces of liquids are relatively weak, and they are fluid, so the molecules can move more freely, which allows the liquid to flow and change shape, and easily aggregate into droplets. However, the intermolecular forces of solids are stronger, the molecules are closely arranged, and the positions are relatively fixed. Their molecules are confined in a fixed lattice structure and lack fluidity. Therefore, the solid coating agent is not fully and uniformly coated on the surface of the powder, and it is easier to form localized coating and difficult to form droplets.

[0075] Moreover, the surface tension of the liquid acts on the molecules, making the liquid tend to reduce its surface area, thus forming round droplets. Solids do not have this tendency to minimize the surface area because their surface is determined by a fixed molecular structure. In a higher energy state, the molecular motion of the liquid is more active, and the molecules in the liquid are more likely to overcome the interaction force and gather into droplets. In solids, the energy state of the molecules is low, which is not enough to enable them to overcome the interaction force and move freely.

[0076] Due to the combined effect of the above factors, liquid unsaturated fatty acids as coating agents are more likely to form droplets than solid coating agents, which is beneficial to increase the interaction force between the coated silver powders and can withstand greater crushing pressure in the feeding device of the air flow mill without producing a back-spray effect.

[0077] The liquid unsaturated fatty acid in the present invention can be mixed with silver powder by dry mixing or wet mixing. When the liquid unsaturated fatty acid and silver powder are dry coated, the mass ratio of silver powder to liquid unsaturated fatty acid is 100:0.1-0.2. When the liquid unsaturated fatty acid and silver powder are wet coated, the liquid unsaturated fatty acid and solvent are first mixed to form a liquid unsaturated fatty acid solution, and then the silver powder and the liquid unsaturated fatty acid solution are mixed, and the mass ratio of the silver powder to the liquid unsaturated fatty acid solution is 100:1-2; preferably, the mass ratio of the liquid unsaturated fatty acid to the solvent in the liquid unsaturated fatty acid solution is 10-20:100; preferably, the solvent is ethanol.

[0078] It can be seen that no matter whether the liquid unsaturated fatty acid and the silver powder are mixed by dry method or wet method, the amount of liquid unsaturated fatty acid added is small, and no liquid phase mixing is formed during the mixing process, but solid phase mixing or solid phase wetting and then mixing, and after wet mixing, the coated silver powder needs to be dried. The drying operation can dry the solvent in the wet mixing to make it volatilize. Specifically, the drying includes drying at 45-80°C.

[0079] Furthermore, in the present invention, the coating is carried out under stirring, and stirring can make the coating more uniform, wherein the stirring speed is 100-400RPM and the stirring time is 3-10min.

[0080] S3. Mechanical crushing.

[0081] The coated silver powder is mechanically crushed.

[0082] In the present invention, mechanically crushing the coated silver powder can further control the particle size of the silver powder. The method of mechanical crushing mainly includes crushing the coated silver powder with a crushing blade to a particle size of 0.5-3 μm.

[0083] S4, air flow mill.

[0084] The air jet mill is used to crush and disperse the powder, and the crushing pressure of the air jet mill can reach above 0.8Mpa.

[0085] The feed rate of the jet mill is 20-60kg / h, and the gas flow rate of the jet mill is 1.5-7.5m 3 / min.

[0086] In the present invention, the silver powder is coated with liquid unsaturated fatty acid so that the silver powder is formed into balls or agglomerates during the mixing process, and the particle size of the silver powder can be controlled after subsequent mechanical pulverization. The pulverization pressure of the final air flow mill can be significantly increased during the subsequent air flow milling, so that the silver powder can be pulverized and shaped under a greater pressure, and the silver powder is spherical after pulverization with a smooth surface.

[0087] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0088] Example 1

[0089] This embodiment provides a method for improving the grinding pressure of a jet mill in the process of preparing silver powder, which comprises the following steps:

[0090] S1. Preparation of silver powder.

[0091] (1) Weigh 10 kg of silver nitrate solid and dissolve it in 100 kg of water to form a clear and transparent silver salt solution, which serves as the silver source, namely system A;

[0092] (2) Weigh 2 kg of polyvinyl pyrrolidone and dissolve it in 100 kg of water for later use as the dispersant base liquid, which is system B;

[0093] (3) Weigh 6 kg of ascorbic acid solid and dissolve it in 100 kg of water for later use as a reducing agent, which is system C;

[0094] (4) System A and system C were slowly injected into system B through a peristaltic pump for 10 minutes. During the process, the water bath condition at room temperature of 25°C was maintained, and the stirring speed was 200RPM using a mechanical stirring paddle. After the reaction was completed, the stirring was maintained for 5 minutes, 1g of lauric acid was added to form flocculation, and the stirring was continued for 5 minutes. Then, the powder was washed with deionized water by suction filtration. The washing was stopped after the conductivity of the washing solution was reduced to 50μS / cm, and the silver powder was obtained.

[0095] S2. Coating.

[0096] 45g of ethanol was used as solvent, and 5g of palmitic acid was added as coating agent to prepare coating agent solution. 50g of coating agent solution was added to 5kg of powder, and mechanical stirring was used to stir for 5min to achieve coating. Afterwards, the powder was filtered and placed in an oven to bake at 75°C to obtain coated silver powder.

[0097] S3. Mechanical crushing.

[0098] The coated silver powder is mechanically crushed with a crushing blade to a particle size of 0.5-3 μm to obtain an initial prepared sample.

[0099] S4, air flow mill.

[0100] The powder is crushed and dispersed by air jet mill. The feed rate of the air jet mill is 40kg / h and the gas flow rate of the air jet mill is 4.5m 3 / min, control the grinding pressure of the jet mill to obtain the final powder product.

[0101] Example 2

[0102] The basic operation of this embodiment is the same as that of Embodiment 1, except that in this embodiment, formalin is used as a reducing agent in step 1 instead of ascorbic acid in Embodiment 1, and oleic acid is used as a coating agent in step S2 instead of palmitoleic acid in Embodiment 1.

[0103] This embodiment provides a method for improving the grinding pressure of a jet mill in the process of preparing silver powder, which comprises the following steps:

[0104] S1. Preparation of silver powder.

[0105] (1) 10 kg of silver nitrate solid was weighed and dissolved in 100 kg of water, and 6 kg of ammonia solution was added, the concentration of the ammonia solution was 10 wt %, and a clear and transparent silver ammonia solution was formed, which served as a silver source and an oxidant, namely, system A;

[0106] (2) Weigh 2 kg of polyvinyl pyrrolidone and dissolve it in 100 kg of water for later use as the dispersant base liquid, which is system B;

[0107] (3) Weigh 5 kg of formalin solution with a concentration of 37 wt % and dissolve it in 100 kg of water for later use as a reducing agent, which is system C;

[0108] (4) System A and System C were slowly injected into System B through a peristaltic pump for 10 min. During the process, the water bath condition was maintained at room temperature of 25°C and the stirring speed was 200 RPM using a mechanical stirring paddle. After the reaction was completed, stirring was continued for 5 min, 1 g of lauric acid was added to form flocculation, stirring was continued for 5 min, and then the powder was washed with deionized water by suction filtration. The washing was stopped after the conductivity of the washing solution was reduced to 50 μS / cm.

[0109] S2. Coating.

[0110] 45g of ethanol was used as solvent, and 5g of oleic acid was added as coating agent to prepare coating agent solution. 50g of coating agent solution was added to 5kg of powder, and mechanical stirring was used to stir for 5min to achieve coating. Afterwards, the powder was filtered and placed in an oven to bake at 75°C to obtain coated silver powder.

[0111] S3. Mechanical crushing.

[0112] The coated silver powder is mechanically crushed with a crushing blade to a particle size of 0.5-3 μm to obtain an initial prepared sample.

[0113] S4, air flow mill.

[0114] The powder is crushed and dispersed by air jet mill. The feed rate of the air jet mill is 40kg / h and the gas flow rate of the air jet mill is 4.5m 3 / min, control the grinding pressure of the jet mill to obtain the final powder product.

[0115] Example 3

[0116] This embodiment is substantially the same as embodiment 1, except that the palmitoleic acid in embodiment 1 is replaced by erucic acid in this embodiment.

[0117] Example 4

[0118] This example is basically the same as Example 1, except that in this example, the palmitoleic acid in Example 1 is replaced with linoleic acid and linolenic acid in a ratio of 1:1.

[0119] Example 5

[0120] This embodiment is basically the same as the embodiment 1, except that, in this embodiment, step S2 includes: adding 10 g of oleic acid to the medium powder, mixing, and stirring for 5 minutes by mechanical stirring to achieve coating, thereby obtaining coated silver powder.

[0121] Comparative Example 1

[0122] This comparative example is basically the same as Example 1, except that in this comparative example, the palmitoleic acid in Example 1 is replaced by lauric acid, which is a solid saturated fatty acid.

[0123] Comparative Example 2

[0124] This comparative example is basically the same as Example 2, except that in this comparative example, the oleic acid in Example 2 is replaced by lauric acid, which is a solid saturated fatty acid.

[0125] Comparative Example 3

[0126] This comparative example is substantially the same as Example 1, except that the palmitoleic acid in Example 1 is omitted in this comparative example.

[0127] Step S2 of this comparative example 1 is: using 50g of ethanol as a solvent, without adding a coating agent, placing the powder in the ethanol, and stirring for 5 minutes by mechanical stirring. Afterwards, the powder is filtered and placed in an oven to bake at 75°C to obtain silver powder.

[0128] Comparative Example 4

[0129] This comparative example is basically the same as Example 1, except that the mass ratio of the powder to the coating agent solution in this comparative example is 1:3. (That is, 3 kg of the coating agent solution is added to 1 kg of the powder for pure wet coating.)

[0130] Comparative Example 5

[0131] This comparative example is basically the same as Example 1, except that the mass ratio of the powder to the coating agent solution in this comparative example is 100:5.

[0132] Experimental example

[0133] The powders prepared in the above embodiments and comparative examples were jet milled at 0.6 MPa, 0.8 MPa and 1 MPa crushing pressures, respectively, and the particle size D50, specific surface area, slurry viscosity and powder characteristics were respectively detected. The detection methods included laser particle size analyzer (PSD), rotational viscometer (the viscosity test method adopted the rotational viscosity test method in the national standard GB / T 17473.5-2008), scanning electron microscope (SEM), etc. The test results are shown in Table 1.

[0134] Table 1. Statistical table of the pulverization results of the powders of the embodiments and comparative examples at different pulverization pressures by jet mill

[0135]

[0136]

[0137] The results of Example 1 are shown in Figure 1 (Powder original image), Figure 2 , Figure 3 and Figure 4 It can be seen that after the powder is treated with a lower air flow mill pressure of 0.6MPa, the angular parts of the powder surface disappear and the powder is relatively round; after the air flow mill pressure is treated with 0.8MPa, the angular parts of the powder surface basically disappear and the powder is spherical; after the air flow mill pressure is treated with 1.0MPa, the powder surface becomes very smooth and the powder is spherical.

[0138] The results of Example 2 are shown in Figure 5 (Powder original image), Figure 6 and Figure 7 and Figure 8 It can be seen that after the powder is treated with a lower air flow mill pressure of 0.6MPa, the fine protrusions on the powder surface disappear and the powder tends to be round; after the air flow mill pressure of 0.8MPa, the powder becomes more round, and some powders combine together to form larger spherical powders; after the air flow mill pressure of 1.0MPa, the powder surface becomes smoother, the powder is spherical, and has larger aggregated particles.

[0139] The results of Example 3 are shown in Fig. 9 , Fig.10 and Fig.11 It can be seen that after the powder is treated with a lower air flow mill pressure of 0.8MPa, the angular parts of the powder surface disappear and the powder is relatively round; after the air flow mill pressure of 0.6MPa, the angular parts of the powder surface basically disappear and the powder is spherical; after the air flow mill pressure of 1.0MPa, the powder surface becomes very smooth and the powder is spherical.

[0140] The results of Example 4 are shown in Fig.12 , Fig.13 and Fig.14 It can be seen that after the powder is treated with a lower air flow mill pressure of 0.6MPa, the angular parts of the powder surface disappear and the powder is relatively round; after the air flow mill pressure is treated with 0.8MPa, the angular parts of the powder surface basically disappear and the powder is spherical; after the air flow mill pressure is treated with 1.0MPa, the powder surface becomes very smooth and the powder is spherical.

[0141] The results of Example 5 are shown in Fig.15 , Fig.16 and Fig.17 It can be seen that after the powder is processed by the lower airflow mill crushing pressure of 0.6MPa, the angular parts of the powder surface disappear and the powder is relatively round; after the airflow mill crushing pressure of 0.8MPa, the angular parts of the powder surface basically disappear and the powder presents a spherical shape; after the airflow mill crushing pressure of 1.0MPa, the powder surface becomes very smooth and the powder presents a spherical shape. The effects of Examples 3, 4, and 5 are similar to those of Example 1.

[0142] The results of Comparative Example 1 can be found in Fig.18 and Fig.19 It can be seen that after the powder is processed at a lower air flow mill crushing pressure of 0.6 MPa, the angular parts of the powder surface disappear and the powder is relatively round, but further increasing the crushing pressure will cause back spray, so the powder cannot reach the smoothness of the embodiment.

[0143] The results of Comparative Example 2 are shown in Fig. 20 and Fig.21 It can be seen that after the powder is treated with a lower air flow mill crushing pressure of 0.6MPa, the fine protrusions on the surface of the powder partially disappear, there are obvious impact marks but the impact is not sufficient, the powder tends to be round, and some parts are deformed.

[0144] The results of Comparative Example 3 are shown in Fig. 22 and Fig.23 It can be seen that after the powder is processed at a lower air flow mill crushing pressure of 0.6 MPa, the angular parts of the powder surface disappear and the powder is relatively round, but further increasing the crushing pressure will cause back spray, so the powder cannot reach the smoothness of the embodiment.

[0145] The results of Comparative Example 4 are shown in Fig.24 , Fig.25 and Fig.26It can be seen that after the powder is treated with a relatively low airflow mill crushing pressure of 0.6MPa, the angular parts of the powder surface disappear, and the powder is relatively round; after the airflow mill crushing pressure is 0.8MPa, the angular parts of the powder surface basically disappear, and the powder presents a quasi-spherical shape; after the airflow mill crushing pressure is 1.0MPa, the powder surface becomes very smooth, and the powder presents a quasi-spherical shape. Generally, the coating agent for pure wet coating is usually a solid coating agent such as lauric acid, which requires a large amount of solvent to dissolve the solid coating agent such as lauric acid, while the liquid unsaturated fatty acid provided by the present invention does not require a large amount of solvent to dissolve. Excessive use of solvent will cause waste of solvent and relatively high cost, so it is not recommended.

[0146] The results of Comparative Example 5 can be found in Fig. 27 , Fig.28 and Fig.29 It can be seen that after the powder is processed by the lower airflow mill crushing pressure of 0.6MPa, the angular parts of the powder surface disappear and the powder is relatively round; after the airflow mill crushing pressure of 0.8MPa, the angular parts of the powder surface basically disappear, and the powder is spherical; after the airflow mill crushing pressure of 1.0MPa, the powder surface becomes very smooth and the powder is spherical. However, this method leads to excessive residual coating agent, which affects the subsequent measurement of impurity content of the powder, and causes the powder to adhere too strongly in the airflow mill pipe and cavity, increasing the risk of blockage and difficulty in cleaning, so it is not recommended.

[0147] From the viscosity of the slurry prepared by the powder, it can be seen that as the crushing pressure is increased, the smoothness of the powder surface increases and the viscosity of the slurry decreases. In addition, when the surface of the powder itself is relatively rough, the viscosity of the slurry is also correspondingly higher (such as Example 2 and Comparative Example 2).

[0148] Combining the above table with Figure 1-29 It can be seen that after being crushed and dispersed by the airflow mill, the morphology of the powder has undergone a significant change, and the surface has become relatively flatter and smoother. Generally, its dispersibility can be better achieved under a lower crushing pressure, that is, the agglomeration of organic matter bonding during the synthesis process can be opened. After increasing the crushing pressure, the particle size dispersion state does not change much (that is, the laser particle size analyzer test results do not change much), but the morphology begins to change, and the edges and corners of the surface basically tend to disappear, becoming flatter and smoother. In the selection and use of coating agents, powders coated with liquid unsaturated fatty acids such as palmitic acid and oleic acid can withstand greater crushing pressure, so a wider range of crushing pressure can be achieved for shaping, so the adjustment range of its morphology, viscosity of the slurry prepared by the powder and other properties is larger.

[0149] In summary, the method for improving the crushing pressure of the airflow mill during the preparation of silver powder provided by the present invention, by adding a small amount of liquid unsaturated fatty acids to the silver powder, can not only realize the coating of the silver powder to make its surface smooth and flat, but also help to increase the crushing pressure of the airflow mill during the subsequent airflow mill crushing. The reason is that the liquid unsaturated fatty acids themselves are in the form of droplets, and their surface tension acts on the molecules, so that they tend to aggregate to reduce the specific surface area. This increases the interaction between the silver powders attached to it, and can withstand a greater crushing pressure in the feeding device of the airflow mill without producing a back-spray effect. Therefore, the kinetic energy of the mutual collision in the silver powder airflow mill is greater, and the mutual collision is more sufficient, which ultimately leads to the improvement of the surface morphology and related properties of the silver powder. On the other hand, the liquid coating agent has better fluidity and may have better dispersion and coating effects on the surface of the silver powder. By increasing the crushing pressure, a larger range of crushing pressure can be achieved for shaping, so the adjustment range of its morphology, the viscosity of the slurry prepared by the powder and other properties is larger.

[0150] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for improving the grinding pressure of a jet mill in the process of preparing silver powder, characterized in that: It includes: Silver powder is mixed with liquid unsaturated fatty acid for coating to obtain coated silver powder, the coated silver powder is mechanically crushed, and then the powder is crushed and dispersed by a jet mill, and the crushing pressure of the jet mill reaches above 0.8Mpa.

2. The method for improving the crushing pressure of a jet mill in the process of preparing silver powder according to claim 1, characterized in that: The liquid unsaturated fatty acid comprises at least one of oleic acid, palmitoleic acid, trans-oleic acid, ricinoleic acid, erucic acid, linoleic acid, linolenic acid and omega-7 fatty acids.

3. The method for improving the crushing pressure of a jet mill in the process of preparing silver powder according to claim 2, characterized in that: The liquid unsaturated fatty acid and the silver powder are dry coated, and the mass ratio of the silver powder to the liquid unsaturated fatty acid is 100:0.1-0.

2.

4. The method for improving the crushing pressure of a jet mill in the process of preparing silver powder according to claim 2, characterized in that: The liquid unsaturated fatty acid and the silver powder are wet coated. During the wet coating, the liquid unsaturated fatty acid is first mixed with a solvent to form a liquid unsaturated fatty acid solution, and then the silver powder is mixed with the liquid unsaturated fatty acid solution, and the mass ratio of the silver powder to the liquid unsaturated fatty acid solution is 100:1-2; Preferably, the mass ratio of the liquid unsaturated fatty acid to the solvent in the liquid unsaturated fatty acid solution is 10-20:100; Preferably, the solvent is ethanol.

5. The method for improving the crushing pressure of a jet mill in the process of preparing silver powder according to claim 4, characterized in that: The wet coating further comprises drying the coated silver powder; Preferably, the drying comprises drying at 45-80°C.

6. The method for improving the crushing pressure of a jet mill in the process of preparing silver powder according to any one of claims 1 to 5, characterized in that: The coating is carried out under stirring, with a stirring speed of 100-400RPM and a stirring time of 3-10min.

7. The method for improving the crushing pressure of a jet mill in the process of preparing silver powder according to any one of claims 1 to 5, characterized in that: The mechanical pulverization includes using a crushing blade to pulverize the coated silver powder to a particle size of 0.5-3 μm.

8. The method for improving the crushing pressure of a jet mill in the process of preparing silver powder according to any one of claims 1 to 5, characterized in that: The feed rate of the jet mill is 20-60 kg / h, and the gas flow rate of the jet mill is 1.5-7.5 m 3 / min.

9. The method for improving the crushing pressure of a jet mill in the process of preparing silver powder according to any one of claims 1 to 5, characterized in that: The preparation method of the silver powder comprises: mixing a silver salt solution, a dispersant base liquid and a reducing agent solution to react, stirring after the reaction is completed and adding a flocculant to flocculate, then separating the solid from the liquid, washing the solid until the conductivity of the washing liquid is reduced to 50 μS / cm, and then stopping washing to obtain the silver powder; Preferably, the flocculant includes at least one of polyacrylamide, polyacryl alcohol, polyacryl ether, fatty acid and fatty acid salt.

10. The method for improving the crushing pressure of a jet mill in the process of preparing silver powder according to claim 9, characterized in that: The method for mixing the silver salt solution, the dispersant base solution and the reducing agent solution comprises: injecting the silver salt solution and the reducing agent solution into the dispersant base solution respectively through a peristaltic pump, the injection time is 5-12 minutes, maintaining a water bath condition of 15-40° C. during the reaction process, and using a mechanical stirring paddle to stir at a speed of 100-300RPM; Preferably, the concentration of the silver salt solution is 0.1-3 mol / L, the concentration of the dispersant base solution is 2-10wt%, the concentration of the reducing agent is 0.1-15 mol / L, and the amount of the dispersant in the dispersant base solution is 10-50% of the mass of the silver particles; Preferably, the silver salt in the silver salt solution includes at least one of silver nitrate and silver sulfate; Preferably, the dispersant in the dispersant base solution comprises at least one of polyvinyl pyrrolidone, polyethylene glycol, gum arabic, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum and polyethylene glycol esters of fatty acids; Preferably, the reducing agent comprises at least one of ascorbic acid, hydrazine hydrate, sodium borohydride and formalin.

Citation Information

Cited By

  • Dry modification method of silver powder, dry modified silver powder and application

    CN121004267A

  • A dry method for modifying silver powder, dry modified silver powder and application

    CN121004267B