Manufacturing process method and system of inner runner part

By decomposing the complex inner flow channel structure into multiple split parts and using a process of combining laser selection melting and forming and vacuum diffusion welding, the problems of long manufacturing cycle and difficulty in powder cleaning in traditional processes are solved, and efficient inner flow channel is achieved Part manufacturing avoids the risk of excess and welding defects, and improves processing efficiency and part performance.

CN118989687APending Publication Date: 2024-11-22SHANGHAI SPACE PRECISION MACHINERY RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411242455.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the manufacturing process of complex inner runner structure parts, traditional methods have problems such as long manufacturing cycle, high difficulty and low efficiency in cleaning internal powder after melting and forming of laser selections, resulting in low design freedom and risk of excess.

Method used

By decomposing the three-dimensional model of the phase change energy storage heat exchanger into multiple split parts, and using a manufacturing process combining laser selection melting and forming and vacuum diffusion welding, the preset process standards and welding surface treatment of split parts are ensured. Achieve efficient forming and connection of parts.

Benefits of technology

It effectively reduces the difficulty of cleaning metal powder in the runner, avoids welding defects, realizes stable connection between internal and multi-point and large-area parts, and improves processing efficiency and performance of parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989687A_ABST
    Figure CN118989687A_ABST
Patent Text Reader

Abstract

The invention provides a manufacturing process method of an internal flow channel part, which comprises the following steps: a decomposition step: decomposing a three-dimensional model of a phase change energy storage heat exchanger into n split parts according to requirements, and setting process parameters to ensure that the split parts reach a preset selective laser melting process standard; the preparation method comprises the following steps: preparing n split parts according to set process forming parameters; the surface roughness of the to-be-welded surface of the prepared split part reaches a preset range through machining; welding pretreatment is conducted, specifically, the to-be-welded surfaces of the machined split parts are subjected to welding pretreatment; the n split parts obtained after pretreatment are assembled, then the split parts are put into a furnace to be subjected to vacuum diffusion welding, and the phase change energy storage heat exchanger part is obtained; n is an integer greater than 1. The cleaning difficulty of metal powder in the runner can be effectively reduced, and the fusion welding defect is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal additive manufacturing, and in particular, to a manufacturing process method and system for a flow channel part, and in particular, to a manufacturing process method and system for a complex inner flow channel part. Background Art

[0002] With the increasing demand for lightweighting in the aerospace field, the trend of structural complexity is obvious, and the limitations of traditional manufacturing processes in complex structural processes are becoming more and more prominent. Complex internal flow channel parts are usually manufactured in steps using a combination of traditional processes such as machining and welding. The manufacturing process is cumbersome and the cycle is long. In addition, the internal flow channel structure design based on traditional manufacturing process methods has a low degree of freedom, and the design usually has to sacrifice some product performance to meet process constraints or reduce manufacturing cost pressure. Laser selective melting technology can shorten the product development cycle, form parts with complex structures, and reduce the cost of personalized customization. Therefore, laser selective melting forming technology has obvious advantages in the manufacturing of complex and fine structures.

[0003] However, based on the principle of layer-by-layer powder spreading and layer-by-layer sintering of laser selective melting, after the laser selective melting of complex inner flow channel structure products is completed, the powder in the internal unmelted area needs to be cleaned and recovered. However, it is difficult and inefficient to remove the powder inside the complex inner flow channel structure, and there is a risk of excess material, which restricts the application of laser selective melting forming technology in complex inner flow channel structure products. Therefore, solving the forming problem of complex inner flow channel structure parts is a difficult problem that people in this field need to solve urgently.

[0004] The patent document with publication number CN105333649A discloses a heat exchanger, including a collecting unit, the collecting unit including a first component and a second component fixed to the first component, the first component including a first connecting portion and a first cavity; the second component including a second connecting portion and a third cavity, the second component also including a first slit hole penetrating the third cavity; the first connecting portion and the second connecting portion are fitted and fixed to form a first flow cavity; the collecting unit also includes a first spoiler unit, the first spoiler unit is integrally formed with the first combination and / or the second combination, the first spoiler unit protrudes from the outside of the flow cavity to the inside of the flow cavity, and the first spoiler unit forms a shrinkage structure in the internal space of the first flow cavity; in this way, the collecting unit formed by stamping the plate can reduce the height of the collecting unit; the spoiler element integrally formed in the collecting unit has a simple structure, and can suppress the gas-liquid separation phenomenon of the fluid in the collecting unit, and can improve the heat exchange efficiency. The connection method between the parts of the invention is fitting, which is not firm and has low assembly accuracy.

[0005] Traditional processing methods have a long manufacturing cycle and high difficulty. If laser selective melting forming technology is used for one-piece forming, the incomplete cleaning of the powder inside the part will cause the risk of excess material. Therefore, a manufacturing process method and system for internal flow channel parts are needed. Summary of the invention

[0006] In view of the defects in the prior art, an object of the present invention is to provide a manufacturing process method and system for an inner flow channel part.

[0007] A manufacturing process method of an inner flow channel part provided by the present invention comprises:

[0008] Decomposition step: decompose the three-dimensional model of the phase change energy storage heat exchanger into n parts as needed, and set process parameters to ensure that the parts meet the preset laser selective melting processability standards;

[0009] Preparation step: preparing n separate parts according to the set process forming parameters;

[0010] Processing step: through processing, the surface roughness of the prepared split parts to be welded reaches a preset range;

[0011] Welding pretreatment step: welding pretreatment is performed on the surface to be welded of the processed split parts;

[0012] Welding steps: assemble the n pre-treated parts, and then put the parts into a furnace for vacuum diffusion welding to obtain phase change energy storage heat exchanger parts;

[0013] n is an integer greater than 1.

[0014] Preferably, the decomposition step comprises:

[0015] In the 3D model, a preset range of machining allowance is added to the surface of the split part to be welded.

[0016] Preferably, the preparation step comprises:

[0017] Powder pretreatment step: drying and baking the powder required for forming;

[0018] Layering step: n split parts are sliced ​​and processed separately, and the laser selected area is evacuated and filled with argon gas for protection;

[0019] Forming step: forming the slices layer by layer;

[0020] Reprocessing step: Stress relief annealing treatment is performed on the formed split parts.

[0021] Preferably, the processing steps include:

[0022] The surfaces to be welded of the split parts are machined, including milling and grinding, so that the roughness of the surfaces to be welded is Ra≤1.0μm.

[0023] Preferably, the welding pretreatment step comprises:

[0024] Oxide film removal step: Use sandpaper to grind the surface to be welded to remove the oxide film on the surface to be welded of the split parts;

[0025] Sandblasting step: sandblasting the surface of the split parts to be welded;

[0026] Degreasing steps: Place the split parts in acetone for ultrasonic cleaning to remove oil and dust on the surface of the split parts.

[0027] A manufacturing process system for an inner flow channel part provided by the present invention comprises:

[0028] Decomposition module: decompose the three-dimensional model of the phase change energy storage heat exchanger into n parts as needed, and set the process parameters to ensure that the parts meet the preset laser selective melting processability standards;

[0029] Preparation module: prepare n separate parts according to the set forming parameters;

[0030] Processing module: through processing, the surface roughness of the prepared split parts to be welded is made to reach the preset range;

[0031] Welding pretreatment module: perform welding pretreatment on the surface to be welded of the processed split parts;

[0032] Welding module: Assemble the n pre-treated parts, and then put the parts into the furnace for vacuum diffusion welding to obtain phase change energy storage heat exchanger parts;

[0033] n is an integer greater than 1.

[0034] Preferably, the decomposition module comprises:

[0035] In the 3D model, a preset range of machining allowance is added to the surface of the split part to be welded.

[0036] Preferably, the preparation module comprises:

[0037] Powder pretreatment module: Dry and bake the powder required for forming;

[0038] Layering module: slice n parts into layers respectively, and evacuate the laser selected area and fill it with argon for protection;

[0039] Forming module: to process the slices layer by layer;

[0040] Reprocessing module: Stress relief annealing is performed on the formed split parts.

[0041] Preferably, the processing module comprises:

[0042] The surfaces to be welded of the split parts are machined, including milling and grinding, so that the roughness of the surfaces to be welded is Ra≤1.0μm.

[0043] Preferably, the welding pretreatment module comprises:

[0044] Oxide film removal module: use sandpaper to polish the surface to be welded to remove the oxide film on the surface to be welded of the split parts;

[0045] Sandblasting module: sandblasting the surface of the split parts to be welded;

[0046] Degreasing module: Place the split parts in acetone for ultrasonic cleaning to remove oil and dust on the surface of the split parts.

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] 1. The present invention can effectively reduce the difficulty of cleaning the metal powder in the flow channel by performing split additive manufacturing on the complex inner flow channel structure parts, thereby solving the problem of excess materials existing in the integral forming of the inner flow channel parts by additive manufacturing;

[0049] 2. The present invention connects additively manufactured split parts by diffusion welding, which can avoid fusion welding defects, and there is no heat-affected zone, and can connect internal and multi-point, large-area parts;

[0050] 3. The present invention can decompose the model into appropriate quantities by freely decomposing the model, thereby further simplifying the processing process and improving efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0052] Figure 1 It is a flow chart of the manufacturing process method of the inner flow channel part of the present invention;

[0053] Figure 2 It is a schematic diagram of the internal cross section of the inner flow channel part of the present invention;

[0054] Figure 3 It is a schematic diagram of the complex inner flow channel parts in the embodiment of the present invention;

[0055] Figure 4 This is the diffusion welding cross-section microstructure of the complex inner flow channel part in the embodiment of the present invention. DETAILED DESCRIPTION

[0056] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0057] Example 1

[0058] The part in this example is a phase-change energy storage heat exchanger, made of AlSi10Mg aluminum alloy. The internal cross-section of the part is as follows: Figure 2 As shown in the figure, there are 108 rectangular channels inside the part, the channel length is 192mm, and the channel wall thickness is 0.5mm. The traditional processing method has a long manufacturing cycle and high difficulty. If the laser selective melting forming technology is used for one-piece forming, the incomplete cleaning of the powder inside the part will cause the risk of excess material. Therefore, the laser selective melting forming-diffusion welding composite manufacturing method can be used to prepare the part, which specifically includes the following steps:

[0059] (1) Figure 3 As shown, in this example, the three-dimensional model of the phase change energy storage heat exchanger is divided into three separate parts. The powder inside the flow channel can be easily and directly poured out from both ends of the separate part 2, effectively avoiding the dead corners of powder cleaning. Figure 3 The schematic diagram of the splitting is shown below; then a 2mm machining allowance is added to the surface of the split part to be welded. Specifically, the three-dimensional model of the phase change energy storage heat exchanger is decomposed into n split parts. The split parts should have good laser selective melting processability, and the metal powder inside the split part flow channel is easier to clean. The number of split parts is set according to the structural characteristics of the phase change energy storage heat exchanger.

[0060] (2) The material used in this example is AlSi10Mg aluminum alloy powder. Before forming, the powder needs to be vacuum dried at a powder baking temperature of 120°C for 3 hours. The treated metal powder is laid on the powder feeding platform. The split parts 1, 2 and 3 are layered and sliced ​​using the layering software, and the laser selective melting forming process parameters are set. The process parameters of each split part are consistent. The specific process parameters are: laser power of 390W, scanning speed of 1300mm / s, scanning interval of 0.19mm, and powder laying thickness of 0.03mm. Before laser selective melting forming, vacuum is evacuated and argon gas is filled for protection. After the oxygen content is lower than 300ppmm, layer-by-layer forming is started until the split parts are completed. After the split parts are prepared by laser selective melting, the powder inside the split parts is cleaned and the split parts are subjected to stress relief annealing. The stress relief annealing mechanism is at 200°C / 2h and cooled with the furnace. After the stress relief annealing is completed, the split parts are cut from the substrate using wire cutting. Avoid deformation of split parts caused by stress release after wire cutting.

[0061] (3) The surfaces to be welded of the split parts 1, 2 and 3 cut from the substrate are machined, including milling and grinding, to ensure that the surface roughness Ra of the split parts to be welded is ≤ 1.0 μm.

[0062] (4) The oxide film on the surface of the split part to be welded is removed by sandpaper polishing; the surface of the split part to be welded is sandblasted; then, the split part is ultrasonically cleaned in acetone for 15 to 20 minutes to remove oil and dust on the surface of the split part.

[0063] (5) After the split parts 1, 2 and 3 are assembled, they are put into the furnace. The upper and lower pressure heads are used to apply pressure to the welded parts to maintain good axial alignment between the split parts and the pressure head. The pressure is 5 MPa. Then, the vacuum hot pressing furnace is evacuated. When the vacuum degree reaches 5×10 -1 When the pressure is below Pa, the temperature is increased to 540°C at a heating rate of 10°C / min and kept warm for 90min under a pressure of 5MPa. After the diffusion welding is completed, the pressure is released and the temperature is reduced to 400°C at a cooling rate of 5°C / min. Then, the furnace is cooled to room temperature to obtain the phase change energy storage heat exchanger parts manufactured by laser selective melting-diffusion welding composite.

[0064] Complex internal flow channel parts are prepared by laser selective melting-diffusion welding composite manufacturing method. The powder cleaning inside the parts is easy and efficient. The microstructure of the diffusion welding cross section of the parts obtained by this method is as follows Figure 4 shown.

[0065] Obviously, those skilled in the art can make various changes and modifications to the invention without departing from the spirit and scope of the invention. Thus, if these modifications and variations of the invention fall within the scope of the claims of the invention and their equivalents, the invention is also intended to include these modifications and variations.

[0066] The present invention also provides a manufacturing process system for an inner runner part. The manufacturing process system for the inner runner part can be realized by executing the process steps of the manufacturing process method for the inner runner part. That is, those skilled in the art can understand the manufacturing process method for the inner runner part as a preferred implementation mode of the manufacturing process system for the inner runner part.

[0067] A manufacturing process system for an inner flow channel part comprises: a decomposition module: decomposing a three-dimensional model of a phase change energy storage heat exchanger into n separate parts as required, and setting process parameters to ensure that the separate parts meet preset laser selective melting processability standards; a preparation module: preparing n separate parts according to set forming parameters; a processing module: making the surface roughness of the prepared separate parts to be welded reach a preset range through processing; a welding pretreatment module: performing welding pretreatment on the surface to be welded of the processed separate parts; a welding module: assembling the n separate parts after pretreatment, and then placing the separate parts into a furnace for vacuum diffusion welding to obtain phase change energy storage heat exchanger parts; n is an integer greater than 1.

[0068] Specifically, the decomposition module includes: in the three-dimensional model, adding a preset range of machining allowance to the surface to be welded of the split component.

[0069] Specifically, the preparation module includes: a powder pretreatment module: drying and baking the powder required for forming; a layering module: slicing n separate parts separately, and vacuuming the laser selected area and filling it with argon for protection; a forming module: forming the slicing layer by layer; a reprocessing module: performing stress relief annealing on the formed separate parts.

[0070] Specifically, the processing module includes: machining the surface to be welded of the split component, including milling and grinding, so that the roughness Ra of the surface to be welded is ≤1.0 μm.

[0071] Specifically, the welding pretreatment module includes: an oxide film removal module: using sandpaper to grind the surface to be welded to remove the oxide film on the surface of the split part to be welded; a sandblasting module: performing sandblasting on the surface to be welded of the split part; and an oil removal module: placing the split part in acetone for ultrasonic cleaning to remove oil and dust on the surface of the split part.

[0072] Those skilled in the art know that, in addition to realizing the system and its various devices, modules, and units provided by the present invention in a purely computer-readable program code, it is entirely possible to realize the same functions in the form of logic gates, switches, application-specific integrated circuits, programmable logic controllers, and embedded microcontrollers by logically programming the method steps. Therefore, the system and its various devices, modules, and units provided by the present invention can be considered as a hardware component, and the devices, modules, and units included therein for realizing various functions can also be regarded as structures within the hardware component; the devices, modules, and units for realizing various functions can also be regarded as both software modules for realizing the method and structures within the hardware component.

[0073] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.

Claims

1. A manufacturing process for an inner flow channel part, characterized in that: include: Decomposition step: decompose the three-dimensional model of the phase change energy storage heat exchanger into n parts as needed, and set process parameters to ensure that the parts meet the preset laser selective melting processability standards; Preparation step: preparing n separate parts according to the set process forming parameters; Processing step: through processing, the surface roughness of the prepared split parts to be welded reaches a preset range; Welding pretreatment step: welding pretreatment is performed on the surface to be welded of the processed split parts; Welding steps: assemble the n pre-treated parts, and then put the parts into a furnace for vacuum diffusion welding to obtain phase change energy storage heat exchanger parts; n is an integer greater than 1.

2. The manufacturing process of the inner flow channel part according to claim 1, characterized in that: The decomposition step comprises: In the 3D model, a preset range of machining allowance is added to the surface of the split part to be welded.

3. The manufacturing process of the inner flow channel component according to claim 1, characterized in that: The preparation steps include: Powder pretreatment step: drying and baking the powder required for forming; Layering step: n split parts are sliced ​​and processed separately, and the laser selected area is evacuated and filled with argon gas for protection; Forming step: forming the slices layer by layer; Reprocessing step: Stress relief annealing treatment is performed on the formed split parts.

4. The manufacturing process of the inner flow channel component according to claim 1, characterized in that: The processing steps include: The surfaces to be welded of the split parts are machined, including milling and grinding, so that the roughness of the surfaces to be welded is Ra≤1.0μm.

5. The manufacturing process of the inner flow channel component according to claim 1, characterized in that: The welding pretreatment step comprises: Oxide film removal step: Use sandpaper to grind the surface to be welded to remove the oxide film on the surface to be welded of the split parts; Sandblasting step: sandblasting the surface of the split parts to be welded; Degreasing steps: Place the split parts in acetone for ultrasonic cleaning to remove oil and dust on the surface of the split parts.

6. A manufacturing process system for an inner flow channel part, characterized in that: include: Decomposition module: decompose the three-dimensional model of the phase change energy storage heat exchanger into n parts as needed, and set the process parameters to ensure that the parts meet the preset laser selective melting processability standards; Preparation module: prepare n separate parts according to the set forming parameters; Processing module: through processing, the surface roughness of the prepared split parts to be welded is made to reach the preset range; Welding pretreatment module: perform welding pretreatment on the surface to be welded of the processed split parts; Welding module: Assemble the n pre-treated parts, and then put the parts into the furnace for vacuum diffusion welding to obtain phase change energy storage heat exchanger parts; n is an integer greater than 1.

7. The manufacturing process system of the inner flow channel part according to claim 6, characterized in that: The decomposition module comprises: In the 3D model, a preset range of machining allowance is added to the surface of the split part to be welded.

8. The manufacturing process system of the inner flow channel part according to claim 6, characterized in that: The preparation module comprises: Powder pretreatment module: Dry and bake the powder required for forming; Layering module: slice n parts into layers respectively, and evacuate the laser selected area and fill it with argon for protection; Forming module: to process the slices layer by layer; Reprocessing module: Stress relief annealing is performed on the formed split parts.

9. The manufacturing process system of the inner flow channel component according to claim 6, characterized in that: The processing module comprises: The surfaces to be welded of the split parts are machined, including milling and grinding, so that the roughness of the surfaces to be welded is Ra≤1.0μm.

10. The manufacturing process system of the inner flow channel component according to claim 6, characterized in that: The welding pretreatment module comprises: Oxide film removal module: use sandpaper to polish the surface to be welded to remove the oxide film on the surface to be welded of the split parts; Sandblasting module: sandblasting the surface of the split parts to be welded; Degreasing module: Place the split parts in acetone for ultrasonic cleaning to remove oil and dust on the surface of the split parts.