Plate girder manufacturing process

By introducing steps such as wing web docking bevel splicing, heat treatment and vibration aging in the plate beam manufacturing process, the problems of high precision and internal stress of plate beams in traditional processes are solved, and high-precision installation and low stress of plate beams are achieved Production.

CN118989882APending Publication Date: 2024-11-22CHINA MCC5 GROUP CORP LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411402181.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The traditional steel structure production process cannot guarantee the production and installation accuracy of the plate beam, and it also leads to high stress in the plate beam and cannot meet the installation requirements.

Method used

A plate beam manufacturing process is adopted, including plate beam cutting, wing web docking bevel splicing, heat treatment and vibration aging treatment, H-shaped steel assembly and welding, and correction steps. By precisely controlling weld and heat treatment parameters, the plate beam is reduced internal stress.

Benefits of technology

Effectively ensure the production and installation accuracy of the plate beam, meet the installation requirements of the plate beam, and at the same time reduce the internal stress of the plate beam, and improve the overall performance of the plate beam.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989882A_ABST
    Figure CN118989882A_ABST
Patent Text Reader

Abstract

The invention discloses a plate girder manufacturing process. The technical problems that in the prior art, the manufacturing and mounting precision of a plate girder cannot be guaranteed, and the internal stress of the plate girder is large are solved. The method comprises the following steps: step 1, blanking a plate girder; secondly, butt-joint beveling and splicing are conducted on wing webs of the plate girder; 3, heat treatment and vibration aging treatment; fourthly, overall blanking is conducted after web plates of the plate girder are spliced; fifthly, plate girder H-shaped steel is assembled and welded; and sixthly, plate girder H-shaped steel is corrected. The method is scientific and reasonable in design, the manufacturing and mounting precision of the plate girder can be effectively guaranteed to meet the plate girder mounting requirement, and meanwhile the internal stress of the plate girder can be effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel structure processing, and in particular relates to a plate beam manufacturing process. Background Art

[0002] The plate beam is an important component of the boiler steel frame, which is also called the stacked beam. When making the plate beam of the boiler steel frame, if the traditional steel structure manufacturing process or process is used, the manufacturing and installation accuracy of the plate beam cannot be guaranteed, and the plate beam made in this way will have a large internal stress.

[0003] Therefore, designing a plate beam manufacturing process so that the manufactured plate beam can meet the installation requirements and reduce the internal stress of the plate beam has become a technical problem that needs to be urgently solved by technicians in the relevant technical field. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a plate beam manufacturing process to at least solve part of the above technical problems.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A plate beam manufacturing process comprises the following steps:

[0007] Step 1: Cutting of slab beams;

[0008] Step 2: Butt bevel and splice the wing web of the plate beam;

[0009] Step 3: heat treatment and vibration aging treatment;

[0010] Step 4: After the webs of the plate beam are spliced, they are cut as a whole;

[0011] Step 5: Assemble and weld the plate beam H-beam;

[0012] Step 6: Correction of H-shaped steel of plate beam.

[0013] Further, in the step 2, when the wing webs are butt-jointed and spliced, a single-sided V-shaped groove is formed on the wing webs, the groove is 60±5°, and the blunt edge is 2mm; the wing webs of the wing plates adopt unequal-sided X-shaped grooves; the blunt edge is 30mm when the thickness of the top plate main beam support stiffening rib is 50mm, and the blunt edge is 60mm when the thickness is 100mm, the groove is K-shaped, and the groove degree is 50°;

[0014] When butt-jointing the wing web of the plate beam, first grind off the impurities including oxide layer, rust and oil within 50mm of the weld area, and repair the groove defects; set arc starting and lead-out plates at both ends of the weld, the width of the arc starting and lead-out plates shall be greater than 80mm, the length shall be twice the plate thickness and not less than 100mm, the thickness shall be the same as the welded wing web and the groove shall be the same; the lead-out length of the automatic welding weld shall be greater than 80mm, and the arc starting plate shall be flame cut after welding is completed; the butt spot welding length shall be 40-60mm, the spacing shall be 250-300mm, and the butt misalignment shall be ≤2mm.

[0015] Further, in the step 2, when the wing web is butted against the groove and spliced, the wing web is butted against the weld, and preheating treatment is performed before welding. The working place is selected to have an ambient temperature not lower than 0°C, and the wing web is heated to 50-80°C. The preheating method of the wing web is flame heating. When the preheating temperature is measured, it is measured at 50mm from the center of the weld on the reverse side of the heated steel. If the plate thickness is less than δ32mm, the web butt is not preheated before welding.

[0016] When the wing and belly plates are butt-jointed, the total thickness of the welding filling layer shall be 1 to 2 mm lower than the surface of the parent material, and the groove edge shall not be melted. The covering layer shall make the weld width on the groove 3 mm ± 1 mm on each side. The welding speed shall be adjusted so that the excess height is 0 to 3 mm, and no sparks or arcs shall be ignited on the parent material other than the weld.

[0017] Furthermore, in the step 1, when the plate beam is cut, the large plate beam is pre-arched, and when the flange web of the plate beam is cut, a fillet weld shrinkage of 0.3 / 1000 to 0.6 / 1000 is added, and a secondary cutting amount of 50 mm is added in the length direction when the plate beam and the flange web of the plate beam are cut;

[0018] In step three, during the heat treatment and vibration aging treatment, the splicing seams of the plate beam and the plate beam flange with a thickness of more than δ32mm are subjected to stress relief heat treatment after welding is completed and passed the flaw detection, and the web of the plate beam is subjected to stress relief vibration aging treatment after welding is completed and passed the flaw detection inspection.

[0019] Furthermore, in the step three, when the wing plate is heat treated, the heating temperature is 570-630°C, and an electric heating method is adopted. The temperature is measured and recorded by a thermocouple temperature recorder. The thickness of the plate beam wing plate is δ90mm, the insulation time of the wing plate is 2.5 hours, and the width of the heating area on both sides of the weld is 3 times the plate thickness and not less than 200mm, and electric heating is used; when the plate temperature reaches 400°C, the heating rate is controlled. When the insulation time is reached, the cooling rate is controlled within the temperature range above 400°C. During the insulation process, within the specified effective heating range, the maximum temperature difference of the heated part does not exceed 85°C.

[0020] Furthermore, in the step three, the stress relief heat treatment weld needs to be stress relieved heat treated 24 hours after welding, the weld needs to be qualified by nondestructive testing before heat treatment, and 100% of each butt joint is inspected after heat treatment; during the vibration aging treatment of the web of the plate beam, in order to reduce and homogenize the residual stress in the weld, the web splicing weld is subjected to vibration aging treatment. Since the weld of the long web in the plate beam is longer, the length direction is divided into three equal parts, and the vibration aging is completed in two times, and the short web is completed in one time.

[0021] Furthermore, in the step 4, when the web is spliced ​​and the whole is cut, after the web welding and heat treatment of the plate beam are completed, the weld angle deformation is corrected and the web is cut as a whole. The overall cutting needs to add a secondary cutting amount of 50mm in the length direction. The overall splicing of the web of the plate beam is completed in the workshop and the arching degree is controlled within 6mm; the T-type weld between the web and the wing of the plate beam, the web has a K-type 45° groove, a blunt edge of 7mm, and a weld angle of ≥8mm; the T-type weld between the web and the wing of the plate beam δ36mm, the web has a K-type 45° groove, a blunt edge of 12mm, and a weld angle of ≥12mm; the T-type weld between the web and the wing of the plate beam δ40mm, the web has a K-type 45° groove, a blunt edge of 13mm, and a weld angle of ≥14mm.

[0022] Further, in the step 5, when the plate beam H-shaped steel is assembled and welded, the H-shaped steel of the plate beam is assembled in a workshop, and the edge of the web is polished to remove cutting slag, burrs, and oil stains; the welding rod used for spot welding is E5016 or gas shielded welding ER50-6, the spot welding length is 40-60mm, the spacing is 300-350mm, the two sides of the web are staggered for spot welding, the arc starting plate is 200mm long, 100mm wide, the thickness is the same as the beam wing web, and the groove is consistent with the beam wing web;

[0023] The H-beam of the plate beam is welded by cantilever automatic welding. The T-shaped weld between the plate beam wing and the web is welded three times. The welding sequence is to weld the lower chord of the upper beam first and then the upper chord. When welding the lower beam, weld the lower chord of the lower beam first and then the upper chord.

[0024] The fillet welds of the flange and web of the plate beam need to be post-heat treated after welding. The temperature is 200-250℃, the insulation time is 1 hour, the heating area is in the center of the weld, the width is 1.5 times the plate thickness and not less than 100mm; gas heating is used, insulation is carried out with thermal insulation cotton, and the temperature is measured and recorded with a thermocouple temperature recorder. Post-heat treatment must be carried out immediately after welding.

[0025] Furthermore, in the step 6, when the plate beam H-shaped steel is corrected, the angular deformation of the flange after welding of the plate beam H-shaped steel is corrected by mechanical methods, and the ambient temperature is not lower than 0°C. During the correction, it is necessary to prevent the surface of the component from being seriously scratched. If there are still local unqualified parts after mechanical correction, flame correction is required to make it meet the specification requirements;

[0026] The angular deformation of the flange plate after welding and the lateral bending of the plate beam are corrected by heating. During the thermal correction construction, the heating temperature does not exceed 900℃. When the temperature naturally cools to 600℃, it can be hammered. It is necessary to prevent overheating from causing overburning of the material and local sinking;

[0027] When asymmetric angle deformation occurs on the H-shaped steel flange, the weld should be directly heated by flame heating on one side with an angle greater than 90°, and then mechanically corrected after cooling to meet the specification requirements;

[0028] The flanges where the plates and beams overlap must strictly control the inclination of the web and flanges and the non-straightness in the length direction, and the deviation cannot be greater than ±1mm.

[0029] Furthermore, in the step 2, node plate cutting, node plate correction, groove cutting and hole making are carried out simultaneously; after the plate beam H-shaped steel is corrected, the node plate and plate beam H-shaped steel are used to assemble, weld and inspect the beams and columns, and then the beams and columns are repaired, polished, corrected and inspected, and finally the beams and columns are painted and the painting is inspected.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The invention is scientifically and reasonably designed, can effectively ensure the manufacturing and installation accuracy of the plate beam to meet the plate beam installation requirements, and can also effectively reduce the internal stress of the plate beam. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic diagram of the process flow of manufacturing the plate beam of the present invention.

[0033] Figure 2 It is a schematic diagram of the web groove of the plate beam wing of the present invention.

[0034] Figure 3 This is a schematic diagram of the web groove of the plate beam wing when the stiffening rib plate thickness is 50 mm.

[0035] Figure 4 This is the stress relief heat treatment process curve of the present invention.

[0036] Figure 5 It is a schematic diagram of the positions of the support points, the exciter and the vibration pickup of the long web 3280-3480×29435 of the primary vibration aging treatment system of the present invention.

[0037] Figure 6 This is the three vibration aging position diagram of the present invention.

[0038] Figure 7 It is a schematic diagram of the assembly sequence of the H-shaped steel plate beam of the present invention. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0040] Example 1.

[0041] like Figure 1-Figure 7 As shown, a plate beam manufacturing process provided by the present invention comprises the following steps:

[0042] Step 1: Cutting of slab beams.

[0043] When cutting the plate beam, the large plate beam is pre-arched, and when cutting the flange and web of the plate beam, an additional 0.3 / 1000 to 0.6 / 1000 shrinkage allowance of the fillet weld is added. When cutting the plate beam and the flange and web of the plate beam, a secondary cutting allowance of 50mm is added in the length direction.

[0044] Step 2: Butt-joint bevel and splice the web plates of the plate beam.

[0045] When the wing web is butted and spliced, the wing web is opened with a single-sided V-shaped groove, the groove is 60±5°, and the blunt edge is 2mm; the wing web adopts an unequal-sided X-shaped groove; the top plate main beam support stiffening rib has a blunt edge of 30mm when the plate thickness is 50mm and a blunt edge of 60mm when the plate thickness is 100mm, the groove is K-shaped, and the groove degree is 50°;

[0046] When butt-jointing the wing web of the plate beam, first grind off the impurities including oxide layer, rust and oil within 50mm of the weld area, and repair the groove defects; set arc starting and lead-out plates at both ends of the weld, the width of the arc starting and lead-out plates shall be greater than 80mm, the length shall be twice the plate thickness and not less than 100mm, the thickness shall be the same as the welded wing web and the groove shall be the same; the lead-out length of the automatic welding weld shall be greater than 80mm, and the arc starting plate shall be flame cut after welding is completed; the butt spot welding length shall be 40-60mm, the spacing shall be 250-300mm, and the butt misalignment shall be ≤2mm.

[0047] When the wing web is butted and welded, the wing web weld should be preheated before welding. The working place should be a place with an ambient temperature not lower than 0℃. The wing web should be heated to 50-80℃. The preheating method of the wing web is flame heating. The preheating temperature should be measured at 50mm from the center of the weld on the reverse side of the heated steel. The web butt weld with a plate thickness below δ32mm does not require preheating before welding.

[0048] When the wing and belly plates are butt-jointed, the total thickness of the welding filling layer shall be 1 to 2 mm lower than the surface of the parent material, and the groove edge shall not be melted. The covering layer shall make the weld width on the groove 3 mm ± 1 mm on each side. The welding speed shall be adjusted so that the excess height is 0 to 3 mm, and no sparks or arcs shall be ignited on the parent material other than the weld.

[0049] The node plates are cut, corrected, beveled and holed simultaneously. After the plate-beam H-shaped steel is corrected, the node plates and plate-beam H-shaped steel are used to assemble, weld and inspect the beams and columns. The beams and columns are then repaired, polished, corrected and inspected. Finally, the beams and columns are painted and the painting is inspected.

[0050] Step 3: Heat treatment and vibration aging treatment.

[0051] During heat treatment and vibration aging treatment, the joints of plate beams and plate beam flanges with a thickness of more than δ32mm shall be subjected to stress relief heat treatment after welding is completed and passed the flaw detection. After the web welding of the plate beam is completed and passed the flaw detection inspection, stress relief vibration aging treatment shall be performed.

[0052] During the heat treatment of the wing plate, the heating temperature is 570-630℃, and the electric heating method is adopted. The temperature is measured and recorded by a thermocouple temperature recorder. The thickness of the plate beam wing plate is δ90mm, the insulation time of the wing plate is 2.5 hours, and the width of the heating area on both sides of the weld is 3 times the plate thickness and not less than 200mm, and it is heated by electricity; when the plate temperature reaches 400℃, the heating rate is controlled. When the insulation time is reached, the cooling rate is controlled within the temperature range above 400℃. During the insulation process, within the specified effective heating range, the maximum temperature difference of the heated part does not exceed 85℃.

[0053] Stress relief heat treatment welds need to be stress relieved heat treatment 24 hours after welding. The welds must be inspected and qualified before heat treatment. After heat treatment, 100% of each butt joint is inspected. During vibration aging treatment of the web of the plate beam, in order to reduce and homogenize the residual stress in the weld, the web splicing welds are subjected to vibration aging treatment. Since the welds of the long web in the plate beam are longer, the length direction is divided into three equal parts and the vibration aging is completed in two times, and the short web is completed in one time.

[0054] Step 4: After the webs of the plate beam are spliced, cut as a whole.

[0055] When the web is spliced ​​and the whole is cut, after the web welding and heat treatment of the plate beam are completed, the deformation of the weld angle is corrected and the web is cut as a whole. The overall cutting requires an additional secondary cutting amount of 50mm in the length direction. The overall splicing of the web of the plate beam is completed in the workshop and the arching degree is controlled within 6mm; the T-type weld between the web and the wing of the plate beam has a K-type 45° groove on the web, a blunt edge of 7mm, and a weld angle of ≥8mm; the T-type weld between the web and the wing of the plate beam δ36mm has a K-type 45° groove on the web, a blunt edge of 12mm, and a weld angle of ≥12mm; the T-type weld between the web and the wing of the plate beam δ40mm has a K-type 45° groove on the web, a blunt edge of 13mm, and a weld angle of ≥14mm.

[0056] Step 5: Assemble and weld the H-shaped steel plate beam.

[0057] When assembling and welding the H-shaped steel of the plate beam, the H-shaped steel of the plate beam is assembled in the workshop, and the edge of the web is polished to remove cutting slag, burrs and oil stains; the welding rod used for spot welding is E5016 or gas shielded welding ER50-6, the spot welding length is 40~60mm, the spacing is 300~350mm, the two sides of the web are staggered spot welded, the arc starting plate is 200mm long and 100mm wide, the thickness is the same as the beam wing web, and the groove is consistent with the beam wing web.

[0058] The H-shaped steel of the plate beam is welded by cantilever automatic welding. The T-shaped weld between the plate beam wing and the web is welded three times. The welding sequence is to first weld the lower chord of the upper beam and then the upper chord. When welding the lower beam, first weld the lower chord of the lower beam and then the upper chord.

[0059] The fillet welds of the flange and web of the plate beam need to be post-heat treated after welding. The temperature is 200-250℃, the insulation time is 1 hour, the heating area is in the center of the weld, the width is 1.5 times the plate thickness and not less than 100mm; gas heating is used, insulation is carried out with thermal insulation cotton, and the temperature is measured and recorded with a thermocouple temperature recorder. Post-heat treatment must be carried out immediately after welding.

[0060] Step 6: Correction of H-shaped steel of plate beam.

[0061] When correcting the H-beam of the plate beam, the angular deformation of the flange after welding of the H-beam of the plate beam is corrected by mechanical methods. The ambient temperature is not lower than 0℃. During the correction, it is necessary to prevent serious scratches on the surface of the component. If there are still local unqualified parts after mechanical correction, flame correction is required to make it meet the requirements of the specification.

[0062] The angular deformation of the flange plate of the plate beam after welding and the lateral bending of the plate beam are corrected by heating. During the thermal correction construction, the heating temperature does not exceed 900℃. When the temperature naturally cools to 600℃, it can be hammered. Excessive heating must be prevented from causing overburning of the material and local subsidence.

[0063] When asymmetric angular deformation occurs in the H-shaped steel flange, the weld is directly heated by flame heating on one side that is greater than 90°, and then mechanically corrected after cooling to meet the specification requirements.

[0064] The flanges where the plates and beams overlap must strictly control the inclination of the web and flanges and the non-straightness in the length direction, and the deviation cannot be greater than ±1mm.

[0065] The invention is scientifically and reasonably designed, can effectively ensure the manufacturing and installation accuracy of the plate beam to meet the plate beam installation requirements, and can also effectively reduce the internal stress of the plate beam.

[0066] The present invention provides a plate beam manufacturing process, which is mainly to solve the technical problem that the plate beams manufactured by the prior art are not accurate enough and cannot meet the installation requirements, and at the same time can well reduce the internal stress of the plate beams. The present invention mainly includes the following steps:

[0067] Step 1: Cutting of slab beams.

[0068] Large plate beams should be pre-arched, and the shrinkage of fillet welds should be appropriately increased by 0.3 / 1000 to 0.6 / 1000 when cutting the flange webs of plate beams. The cutting of plate beams and flange webs of plate beams should be increased by 50mm in the length direction.

[0069] Step 2: Butt-joint bevel and splice the wing web.

[0070] 1. If Figure 2 As shown in the figure, the web of the plate beam has a single-sided V-shaped groove with a groove of 60±5° and a blunt edge of 2mm. The web of the wing plate adopts an unequal-sided X-shaped groove. Figure 3 As shown in the figure, when the thickness of the top plate main beam support stiffener is 50mm, the blunt edge is 30; when the thickness is 100mm, the blunt edge is 60mm. The groove is K-type, and the groove angle is 50°.

[0071] 2. When the wing web of the plate beam is butt-jointed, first grind the oxide layer, rust, oil and other impurities within 50mm of the weld area and repair the groove defects. Set the arc starter and lead-out plates at both ends of the weld. The width of the arc starter and lead-out plates is greater than 80mm, the length is twice the thickness of the plate and not less than 100mm, the thickness is the same as the welded wing web and the groove is the same. The lead-out length of the automatic welding weld must be greater than 80mm. After welding, it is strictly forbidden to hammer off the arc starter plate and use flame cutting. The length of the butt spot welding is 40-60mm, the spacing is 250-300mm, and the butt misalignment is ≤2mm.

[0072] 3. The butt weld of the flange of the plate beam should be preheated before welding. When the working place temperature is not lower than 0℃, it needs to be heated to 50-80℃. The preheating method of the flange web is flame heating. The preheating temperature is generally measured at 50mm from the center of the weld on the reverse side of the heated steel. The web butt weld with a plate thickness of less than δ32mm does not require preheating before welding.

[0073] 4. When the wing web is butt-jointed, the total thickness of the welding filling layer is 1-2mm lower than the surface of the parent material, slightly concave, and the groove edge must not be melted. The cover layer makes the weld width on the groove 3mm±1mm on each side, and adjust the welding speed to make the excess height 0-3mm. Do not ignite and start the arc on the parent material other than the weld. The welding parameters for the butt joint of the wing web of the plate beam are shown in Table 1.

[0074] Table 1 Welding parameters used when butt jointing the web of the plate beam wing

[0075]

[0076] Step 3: Heat treatment and vibration aging treatment.

[0077] 1. After the welding of the plate beam and the plate beam flange with a thickness of more than δ32mm is completed and the flaw detection is passed, the stress relief heat treatment is carried out. After the web welding of the plate beam is completed and the flaw detection is passed, the stress relief vibration aging treatment is carried out.

[0078] 2. Heat treatment of wing plate. The heating temperature is 570-630℃, and the electric heating method is adopted. The temperature is measured and recorded by a thermocouple temperature recorder. The insulation time of the δ90mm wing plate is 2.5 hours. The width of the heating area on both sides of the weld should be 3 times the thickness of the plate and not less than 200mm, and it should be heated by electricity. When the plate temperature reaches 400℃, the heating rate needs to be controlled. The heating rate control is shown in Table 2; when the insulation time is reached, the cooling rate needs to be controlled within the range above 400℃. The cooling rate control is shown in Table 2.

[0079] Table 2 Wing plate heat treatment heating and cooling speed control table (h-hours)

[0080] Plate thickness Heating rate Cooling speed Plate thickness Heating rate Cooling speed δ36 ≤153℃ / h ≤191℃ / h δ70 ≤79℃ / h ≤98℃ / h δ40 ≤138℃ / h ≤172℃ / h δ80 ≤69℃ / h ≤86℃ / h δ50 ≤110℃ / h ≤138℃ / h δ90 ≤61℃ / h ≤76℃ / h δ60 ≤91℃ / h ≤115℃ / h δ100 ≤55℃ / h ≤68℃ / h

[0081] During the insulation process, within the specified effective heating range, the maximum temperature difference at various locations of the heated part shall not exceed 85°C.

[0082] 3. If Figure 4 As shown in the figure, stress relief heat treatment welds need to be stress relieved 24 hours after welding. The welds must be inspected and qualified before heat treatment. After heat treatment, 100% of each butt joint is inspected.

[0083] 4. Vibration aging treatment of web of plate beam: Figure 5 and Figure 6 As shown in the figure, in order to reduce and homogenize the residual stress in the weld, the splicing welds of the web are subjected to vibration treatment. Since the welds of the long webs in the plate beams are longer, the length direction is divided into three equal parts and the vibration treatment is completed in two times, while the short webs are completed in one time.

[0084] Step 4: Cut the web as a whole after splicing.

[0085] 1. After the web welding and heat treatment of the plate beam are completed, the weld angle deformation is leveled. The web is cut as a whole, and a secondary cutting amount of 50mm is added in the length direction. The web of the plate beam is spliced ​​as a whole in the workshop and the camber is controlled within 6mm.

[0086] 2. T-type weld between web and flange of plate beam, web has K-type 45° groove, blunt edge 7mm, welding angle ≥8mm.

[0087] The web and flange of the plate beam are T-welded with a δ36mm diameter. The web has a K-shaped 45° groove, a blunt edge of 12mm, and a weld angle of ≥12mm.

[0088] The web and flange of the plate beam are T-welded with a δ40mm diameter. The web has a K-shaped 45° groove, a blunt edge of 13mm, and a weld angle of ≥14mm.

[0089] Step 5: Assemble and weld the H-shaped steel plate beam.

[0090] 1. The H-shaped steel of the plate beam is assembled on a special tooling in the workshop. The edge of the web needs to be polished to remove impurities such as cutting slag, burrs, and oil stains. The welding rod used for spot welding is E5016 or gas shielded welding ER50-6. The spot welding length is 40-60mm, the spacing is 300-350mm, and the two sides of the web need to be staggered. The arc starter plate is 200mm long and 100mm wide. The thickness is the same as the web of the beam wing, and the groove is consistent with the web.

[0091] 2. The H-beam welding of the plate beam is carried out using cantilever automatic welding.

[0092] The T-shaped welds between the flange and web of the plate beam are welded twice, and the welding parameters used are shown in Table 3. Figure 7 shown.

[0093] Table 3 Welding parameters of T-type welds between flange and web of plate beam

[0094]

[0095] 3. The T-shaped weld between the plate beam wing and the web is welded three times. The welding order is to first weld the lower chord of the upper beam and then the upper chord. When welding the lower beam, first weld the lower chord of the lower beam and then the upper chord.

[0096] 4. The fillet welds of the flange and web of the plate beam should be post-heat treated at a temperature of 200-250°C. The holding time is 1 hour, and the heating area should be at the center of the weld with a width of 1.5 times the thickness of the plate and not less than 100 mm. Use gas heating and insulation cotton for insulation, and use a thermocouple temperature recorder to measure and record the temperature. Post-heat treatment should be carried out immediately after welding.

[0097] Step 6: Correction of H-shaped steel of plate beam.

[0098] 1. The angular deformation of the flange plate after welding of the H-beam of the plate beam is corrected by mechanical methods. The ambient temperature must be no less than 0℃. During the correction, it is necessary to prevent serious scratches on the surface of the component. If there are still local unqualified parts after mechanical correction, flame correction is required to make them meet the requirements of the specification.

[0099] 2. The angular deformation of the flange plate after welding and the lateral bending of the plate beam are corrected by heating. During the thermal correction construction, the heating temperature is strictly prohibited to exceed 900℃, at which the color of the steel plate is bright cherry red. When the temperature naturally cools to 600℃, hammering is allowed. Strictly prevent overheating from causing overburning of the material and local sinking.

[0100] 3. When asymmetric angular deformation occurs on the H-shaped steel flange, the weld should be directly heated by flame heating on the side that is greater than 90°, and then mechanically corrected after cooling to meet the specification requirements.

[0101] 4. The flanges where the plates and beams overlap must strictly control the inclination of the web and flanges and the non-straightness in the length direction, and the deviation cannot be greater than ±1mm.

[0102] The invention is scientifically and reasonably designed, can effectively ensure the manufacturing and installation accuracy of the plate beam to meet the plate beam installation requirements, and can also effectively reduce the internal stress of the plate beam.

[0103] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solution of the present invention, but not to limit it, and certainly not to limit the patent scope of the present invention. Any changes or modifications that are made to the main design concept and spirit of the present invention without any substantial meaning, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention; in addition, the direct or indirect application of the technical solution of the present invention in other related technical fields is also included in the patent protection scope of the present invention.

Claims

1. A plate beam manufacturing process, characterized in that: The following steps are involved: Step 1: Cutting of slab beams; Step 2: Butt bevel and splice the wing web of the plate beam; Step 3: heat treatment and vibration aging treatment; Step 4: After the webs of the plate beam are spliced, they are cut as a whole; Step 5: Assemble and weld the plate beam H-beam; Step 6: Correction of H-shaped steel of plate beam.

2. A plate beam manufacturing process according to claim 1, characterized in that: In the step 2, when the wing web is butted and spliced, a single-sided V-shaped groove is formed on the wing web, the groove is 60±5°, and the blunt edge is 2mm; the wing web adopts an unequal-sided X-shaped groove; the blunt edge is 30mm when the thickness of the top plate main beam support stiffening rib is 50mm, and the blunt edge is 60mm when the thickness is 100mm, the groove is K-shaped, and the groove degree is 50°; When butt-jointing the wing web of the plate beam, first grind off the impurities including oxide layer, rust and oil within 50mm of the weld area, and repair the groove defects; set arc starting and lead-out plates at both ends of the weld, the width of the arc starting and lead-out plates shall be greater than 80mm, the length shall be twice the plate thickness and not less than 100mm, the thickness shall be the same as the welded wing web and the groove shall be the same; the lead-out length of the automatic welding weld shall be greater than 80mm, and the arc starting plate shall be flame cut after welding is completed; the butt spot welding length shall be 40-60mm, the spacing shall be 250-300mm, and the butt misalignment shall be ≤2mm.

3. A plate beam manufacturing process according to claim 1, characterized in that: In the step 2, when the wing web is butted against the groove and spliced, the wing web is butted against the weld, and preheating treatment is performed before welding. The working place is selected to have an ambient temperature not lower than 0°C. At the same time, the wing web is heated to 50-80°C. The preheating method of the wing web is flame heating. When the preheating temperature is measured, it is measured at 50mm from the center of the weld on the reverse side of the heated steel. If the plate thickness is less than δ32mm, the web butt joint does not undergo preheating treatment before welding. When the wing and belly plates are butt-jointed, the total thickness of the welding filling layer shall be 1 to 2 mm lower than the surface of the parent material, and the groove edge shall not be melted. The covering layer shall make the weld width on the groove 3 mm ± 1 mm on each side. The welding speed shall be adjusted so that the excess height is 0 to 3 mm, and no sparks or arcs shall be ignited on the parent material other than the weld.

4. A plate beam manufacturing process according to claim 1, characterized in that: In the step 1, when the plate beam is cut, the large plate beam is pre-arched, and when the flange web of the plate beam is cut, a fillet weld shrinkage of 0.3 / 1000 to 0.6 / 1000 is added, and a secondary cutting amount of 50 mm is added in the length direction when the plate beam and the flange web of the plate beam are cut; In step three, during the heat treatment and vibration aging treatment, the splicing seams of the plate beam and the plate beam flange with a thickness of more than δ32mm are subjected to stress relief heat treatment after welding is completed and passed the flaw detection, and the web of the plate beam is subjected to stress relief vibration aging treatment after welding is completed and passed the flaw detection inspection.

5. A plate beam manufacturing process according to claim 1, characterized in that: In the step three, when the wing plate is heat treated, the heating temperature is 570-630°C, and the electric heating method is adopted. The temperature is measured and recorded by a thermocouple temperature recorder. The thickness of the plate beam wing plate is δ90mm, the wing plate insulation time is 2.5 hours, and the width of the heating area on both sides of the weld is 3 times the plate thickness and not less than 200mm, and it is electrically heated; when the plate temperature reaches 400°C, the heating rate is controlled. When the insulation time is reached, the cooling rate is controlled within the temperature range above 400°C. During the insulation process, within the specified effective heating range, the maximum temperature difference of each part of the heated part does not exceed 85°C.

6. A plate beam manufacturing process according to claim 1, characterized in that: In the step three, the stress relief heat treatment weld needs to be stress relieved heat treated 24 hours after welding, the weld needs to be qualified by flaw detection before the heat treatment, and 100% of each butt joint is inspected after the heat treatment; during the vibration aging treatment of the web of the plate beam, in order to reduce and homogenize the residual stress in the weld, the web splicing weld is subjected to vibration aging treatment. Since the weld of the long web in the plate beam is longer, the length direction is divided into three equal parts, and the vibration aging is completed in two times, and the short web is completed in one time.

7. A plate beam manufacturing process according to claim 1, characterized in that: In the step 4, when the web is spliced ​​and the whole is cut, after the web welding and heat treatment of the plate beam are completed, the deformation of the weld angle is corrected and the web is cut as a whole. The overall cutting needs to add a secondary cutting amount of 50mm in the length direction. The overall splicing of the web of the plate beam is completed in the workshop and the camber is controlled within 6mm; the web and the wing plate of the plate beam are T-welded, the web has a K-shaped 45° groove, the blunt edge is 7mm, and the weld angle is ≥8mm; the web and the wing plate of the plate beam δ36mm T-welded, the web has a K-shaped 45° groove, the blunt edge is 12mm, and the weld angle is ≥12mm; the web and the wing plate of the plate beam δ40mm T-welded, the web has a K-shaped 45° groove, the blunt edge is 13mm, and the weld angle is ≥14mm.

8. A plate beam manufacturing process according to claim 1, characterized in that: In the step 5, when the plate beam H-shaped steel is assembled and welded, the H-shaped steel of the plate beam is assembled in a workshop, and the edge of the web is polished to remove cutting slag, burrs, and oil stains; the welding rod used for spot welding is E5016 or gas shielded welding ER50-6, the spot welding length is 40-60mm, the spacing is 300-350mm, the two sides of the web are staggered for spot welding, the arc starting plate is 200mm long, 100mm wide, the thickness is the same as the beam wing web, and the groove is consistent with the beam wing web; The H-beam of the plate beam is welded by cantilever automatic welding. The T-shaped weld between the plate beam wing and the web is welded three times. The welding sequence is to weld the lower chord of the upper beam first and then the upper chord. When welding the lower beam, weld the lower chord of the lower beam first and then the upper chord. The fillet welds of the flange and web of the plate beam need to be post-heat treated after welding. The temperature is 200-250℃, the insulation time is 1 hour, the heating area is in the center of the weld, the width is 1.5 times the plate thickness and not less than 100mm; gas heating is used, insulation is carried out with thermal insulation cotton, and the temperature is measured and recorded with a thermocouple temperature recorder. Post-heat treatment must be carried out immediately after welding.

9. A plate beam manufacturing process according to claim 1, characterized in that: In the step 6, when the plate beam H-shaped steel is corrected, the angular deformation of the flange after welding of the plate beam H-shaped steel is corrected by mechanical methods, and the ambient temperature is not lower than 0°C. During the correction, it is necessary to prevent the surface of the component from being seriously scratched. If there are still local unqualified parts after mechanical correction, flame correction is required to make it meet the specification requirements; The angular deformation of the flange plate after welding and the lateral bending of the plate beam are corrected by heating. During the thermal correction construction, the heating temperature does not exceed 900℃. When the temperature naturally cools to 600℃, it can be hammered. It is necessary to prevent overheating from causing overburning of the material and local sinking; When asymmetric angle deformation occurs on the H-shaped steel flange, the weld should be directly heated by flame heating on one side with an angle greater than 90°, and then mechanically corrected after cooling to meet the specification requirements; The flanges where the plates and beams overlap must strictly control the inclination of the web and flanges and the non-straightness in the length direction, and the deviation cannot be greater than ±1mm.

10. A plate girder manufacturing process according to claim 1, characterized in that: In the step 2, node plate cutting, node plate correction, groove cutting and hole making are carried out simultaneously; after the plate beam H-shaped steel is corrected, the node plate and plate beam H-shaped steel are used to assemble, weld and inspect the beams and columns, and then the beams and columns are repaired, polished, corrected and inspected, and finally the beams and columns are painted and the painting is inspected.

Citation Information

Patent Citations

  • Boiler steel structure superposed beam manufacturing process

    CN104475928A

  • Method for processing pi-type plate girder of tower type boiler

    CN109483160A

  • Fabrication method for tower type boiler steel frame superposition type large plate beam

    CN109590675A

  • H-shaped steel welding process

    CN110695618A

  • H-shaped steel assembly process

    CN112059455A