A grinding magnetic needle, its preparation method and application

By spraying high-temperature epoxy resin and ceramic particles onto the outside of the magnetic needle body to form an abrasive magnetic needle, the problems of poor polishing effect and corrosion in the existing magnetic polishing technology are solved, and efficient surface polishing of additive manufacturing structural parts is achieved, especially the treatment of irregular curved surfaces and micro grooves.

CN118990138BActive Publication Date: 2026-11-17SICHUAN WEIJIA ADDITIVE MFG TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411264272.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2026-11-17
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The polishing medium material used in existing magnetic polishing technology is stainless steel, which has poor polishing effect and may cause corrosion of parts during service. It is also difficult to effectively handle irregular curved surfaces and micro-grooves of additive manufacturing structural parts.

Method used

A grinding magnetic needle with magnetic conductivity and structural strength is prepared by spraying a high-temperature epoxy resin to form an adhesive layer on the outside of the needle body and then spraying ceramic particles to form a ceramic layer. This is used in a magnetic polishing system to polish the surface of hard metal additive manufacturing structural parts.

Benefits of technology

It achieves efficient surface polishing of additively manufactured structural parts, especially the treatment of irregular curved surfaces and micro-grooves, avoiding polishing dead corners and corrosion problems, and improving polishing effect and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118990138B_ABST
    Figure CN118990138B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a grinding magnetic needle, comprising the following steps: selecting a needle-shaped magnetic needle body with magnetic conductivity; uniformly scattering the magnetic needle body into the container of a magnetic polishing machine, adjusting the direction and intensity of the magnetic field in the container to keep the magnetic needle bodies vertical and adjacent magnetic needle bodies within a preset distance range; then performing at least one spraying operation on the surface of the magnetic needle body, each spraying operation comprising: first uniformly spraying high-temperature epoxy resin heated to 300-350℃ onto the surface of the magnetic needle body to form an adhesive layer; then heating the container to at least 200℃, and then uniformly spraying ceramic particles onto the adhesive layer to form a ceramic layer; compared with the prior art, it has the following advantages: the prepared grinding magnetic needle can be used in a magnetic polishing system to efficiently perform surface polishing on additive manufacturing structural parts formed from difficult-to-machine hard metals, and can efficiently perform surface polishing on various irregular curved surfaces and micro-grooves without leaving dead corners.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of precision machining technology for parts, specifically to a grinding magnetic needle, its preparation method, and its application. Background Technology

[0002] Additive manufacturing is a technology that discretizes complex three-dimensional structural parts into two-dimensional structures and then stacks them layer by layer to form the final product. As a result, its applications in aerospace, automotive, and mold industries are increasing, facilitating rapid manufacturing to achieve lightweighting, miniaturization, and integration in high-end equipment manufacturing. However, due to the inherent characteristics of additive manufacturing processes such as temperature gradients and layer-by-layer forming, the outer surface of parts may exhibit partially burned or adhered powder particles, residual supports, and a surface "step" effect.

[0003] Currently, additive manufacturing structural components generally employ surface polishing technology to eliminate powder adhesion and residual support, and only after polishing rough surfaces can they meet the requirements for product assembly, service life, and safety. Existing surface treatment processes for additively manufactured structural components have several limitations. For example, chemical reagent treatments have low polishing efficiency on the outer surfaces of additively manufactured structural components; electrochemical treatments are difficult to apply to micro-pores and irregularly shaped surfaces, making it impossible to polish them; contact polishing is limited by tool freedom; abrasive flow polishing technology for internal channels is unsuitable for polishing the outer surfaces of additively manufactured structural components; water jet polishing, due to its erosion effect on the material surface by the polishing medium ejected from micro-nozzles, has a very small removal volume and range, and is generally used for polishing hard and brittle materials such as glass, with low polishing efficiency for large-scale structural components and excessively rough additively manufactured surfaces; magnetorheological polishing is limited by the magnetic field distribution and is only suitable for common polishing methods such as regularly oriented tubular shapes and outer surface structures; in addition, chemical methods such as chemical, electrochemical, and plasma polishing, besides having small removal volumes and being difficult to improve the rough surfaces of additively manufactured structural components on a large scale, can also cause various corrosion and elemental contamination defects. Corrosive liquids and reactive gases can also have adverse effects on the environment, personnel, and equipment, and have been classified as restricted processes in the engine field.

[0004] To address the aforementioned issues, magnetic polishing technology is generally used to polish the surfaces of additively manufactured structural parts. However, some additively manufactured structural parts are made of hard metals that are difficult to machine, such as titanium alloys, high-temperature alloys, cobalt-chromium alloys, mold steel, and high-strength steel. The polishing medium used in magnetic polishing technology is generally stainless steel, which results in very poor polishing effect. Furthermore, polishing harder materials (such as high-temperature alloys) can induce corrosion during the service life of the parts. Summary of the Invention

[0005] In view of the shortcomings of the existing technology, the purpose of this invention is to provide a grinding magnetic needle, its preparation method and application, so as to solve the problem that the polishing medium used in the magnetic polishing technology is generally stainless steel, which has a very poor polishing effect and the polished material can induce corrosion of the parts during service.

[0006] To achieve the above objectives, the first aspect of the present invention adopts the following technical solution: a method for preparing a grinding magnetic needle, comprising the following steps:

[0007] Select a needle-shaped magnetic needle body with magnetic conductivity;

[0008] Evenly sprinkle the magnetic needles into the container of the magnetic grinder, and adjust the direction and intensity of the magnetic field in the container to keep the magnetic needles vertical and ensure that adjacent magnetic needles are within a preset distance.

[0009] Then, at least one spraying operation is performed on the surface of the magnetic needle body, and each spraying operation includes:

[0010] To form an adhesive layer, high-temperature epoxy resin heated to 300-350℃ is first evenly sprayed onto the surface of the magnetic needle body to form an adhesive layer.

[0011] A ceramic layer is formed, and then the container is heated to at least 200°C. Ceramic particles are then evenly sprayed onto the adhesive layer to form the ceramic layer.

[0012] The second aspect of the present invention adopts the following technical solution: a grinding magnetic needle, which is prepared by the grinding magnetic needle preparation method described in the first aspect of the present invention.

[0013] The third aspect of the present invention adopts the following technical solution: an application of a grinding magnetic needle, as described in the second aspect of the present invention, in a magnetic polishing system for polishing hard additive manufacturing structural parts.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] The method for preparing this grinding magnetic needle allows for the stable and uniform distribution of an adhesive layer and a ceramic layer on the outer side of the magnetic needle body. The resulting grinding magnetic needle uses the needle-shaped and magnetically conductive magnetic needle body as the basic framework, combined with the ceramic layer, to give the prepared grinding magnetic needle sufficient structural strength. This allows it to be used in magnetic polishing systems to efficiently perform surface polishing on additive manufacturing structural parts made of difficult-to-machine hard metals such as titanium alloys, high-temperature alloys, cobalt-chromium alloys, mold steel, and high-strength steel. It can also efficiently polish various irregular curved surfaces and micro-grooves on additive manufacturing structural parts, ensuring that there are no polishing dead corners.

[0016] The grinding magnetic needle prepared by this method has a ceramic layer as its outermost layer, which will not corrode during the service life of the additive manufacturing structure when it is used for surface polishing. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of the movement of the spray head during the spraying process in this invention;

[0018] Figure 2 This is a diagram showing the arrangement of the magnetic needle body within the container in this invention;

[0019] Figure 3 An optical photograph of a cross-sectional view of the grinding magnetic needle prepared according to the present invention;

[0020] Figure 4 An optical photograph of the side surface of the polished magnetic needle prepared according to the present invention;

[0021] Figure 5 This is a schematic diagram of the grinding magnetic needle size detection scheme prepared according to the present invention;

[0022] Figure 6 A comparison of the polishing effects of the grinding magnetic needle prepared according to the present invention and a conventional magnetic needle after grinding and polishing a titanium alloy additive manufacturing process. Detailed Implementation

[0023] The present invention will be further described in detail below through specific embodiments:

[0024] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a grinding magnetic needle, comprising the following steps:

[0025] Step s1: Select a needle-shaped magnetic needle body that is magnetically conductive;

[0026] Step s2: Evenly sprinkle the magnetic needle body into the container of the magnetic grinder, and adjust the direction and intensity of the magnetic field in the container to keep the magnetic needle body vertical and the adjacent magnetic needle bodies within a preset distance range.

[0027] Step s3, then perform at least one spraying operation on the surface of the magnetic needle body, each spraying operation including:

[0028] Step s31, forming an adhesive layer: First, high-temperature epoxy resin heated to 300-350℃ is uniformly sprayed onto the surface of the magnetic needle body to form an adhesive layer.

[0029] Step s32: A ceramic layer is formed. The container is then heated to at least 200°C. Ceramic particles are then uniformly sprayed onto the adhesive layer to form the ceramic layer.

[0030] This method for preparing a polishing magnetic needle allows for the sequential and stable uniform distribution of an adhesive layer and a ceramic layer on the outer side of the magnetic needle body, forming a polishing magnetic needle (such as...). Figure 3 and Figure 4 Using a needle-shaped, magnetically conductive needle body as the basic framework, combined with a ceramic layer, the prepared grinding magnetic needle possesses sufficient structural strength to move under the influence of a magnetic field in a magnetic polishing system. This enables efficient surface polishing of additive manufacturing components made of difficult-to-machine hard metals such as titanium alloys, high-temperature alloys, cobalt-chromium alloys, mold steel, and high-strength steel. Furthermore, it can efficiently polish various irregular curved surfaces and micro-grooves on additive manufacturing components, ensuring no polishing dead angles exist. The outermost layer of the grinding magnetic needle prepared by this method is a ceramic layer, which will not corrode during the service life of the additive manufacturing components during surface polishing.

[0031] In this embodiment:

[0032] In step s1:

[0033] The magnetic needle body is made of wire by punching or wire cutting. The wire material can be stainless steel such as 304, 316 or 230, so that the magnetic needle body has good magnetic conductivity. Here, the material of the magnetic needle body is not limited to any kind of magnetic material.

[0034] Specifically, a magnetic needle body with a diameter d = 0.1mm to 5mm and a length of 1mm to 10mm is selected, which can achieve effective contact and processing of the outer surface of irregular and complex structures and micro-holes and grooves. At the same time, it can be moved by the magnetic field of the magnetic polishing system, thereby improving the polishing effect.

[0035] In step s2:

[0036] After evenly scattering the magnetic needles into the container of the magnetic polishing machine, the magnitude and direction of the electromagnetic coil current within the container are set to determine the strength and direction of the magnetic field generated within the container. The electromagnetic coil current is typically set within the range of 1–10 A to achieve a magnetic field strength within the range of 0.30–1.0 T. The magnetic needles are then arranged vertically within the container, with a spacing of 1–5 mm between adjacent needles. Figure 2 This facilitates the uniform distribution of high-temperature epoxy resin and ceramic particles during subsequent spraying.

[0037] In step s31:

[0038] First, the high-temperature epoxy resin (epoxy value 0.25-0.45) is heated to 300-350℃. The flow state of the heated epoxy resin is observed; it exhibits a certain degree of fluidity, allowing it to be sprayed out by the spraying equipment and adhere to the outer surface of the magnetic needle. The heating temperature of the high-temperature epoxy resin can be 300℃, 310℃, 320℃, 330℃, 340℃, or 350℃. During the heating process, the high-temperature epoxy resin is first heated to 300℃, and its state is observed to determine whether the heating temperature needs to be increased. In actual experiments, it was found that a heating temperature not exceeding 350℃ is sufficient to meet the usage requirements.

[0039] Next, a 20 cm long and 1 cm wide adhesive nozzle is installed on the spraying equipment, and the spraying angle of the adhesive nozzle is designed to be 45° to 75°, specifically 45°, 50°, 55°, 60°, 65°, 70° or 75°, etc.; and the spraying pressure of the spraying equipment is set to 0.03 to 0.1 MPa, specifically 0.03 MPa, 0.05 MPa, 0.08 MPa or 0.1 MPa, etc. This spraying angle is designed to ensure that the small gap of 1 to 5 mm between adjacent magnetic needles can be completely covered by the uniform spraying of high-temperature epoxy resin; and to ensure that the distance between the adhesive nozzle of the spraying equipment and the top of the magnetic needle is 2 cm, to prevent the heated high-temperature epoxy resin from solidifying due to excessive spraying distance, which would make the spraying work impossible. Then, the spraying equipment is run again to move the adhesive nozzle along the x-axis at a speed of 38-52 cm / min from point 0 to point P, then in the opposite direction to point P', and then in the opposite direction back to point 0 to complete one spraying cycle (e.g., ...). Figure 1 );

[0040] In this embodiment, points P and P′ are symmetrically arranged on the x-axis with point O as the center. The distance between points P and P′ is 200 cm. The moving speed of the adhesive spray nozzle can be 38 cm / min, 40 cm / min, 42 cm / min, 44 cm / min, 46 cm / min, 48 cm / min, 50 cm / min, or 52 cm / min, etc. This moving speed facilitates dense coverage of the magnetic needle with high-temperature epoxy resin, ensuring the uniformity of the adhesive layer formation.

[0041] During the spraying process, the current of the electromagnetic coil can be periodically and dynamically changed between 1 and 10A at a rate of 4A per minute, so that the magnetic needle body can be continuously shaken in the container. This, combined with the above-mentioned spraying path and parameter settings, ensures that the surface of the magnetic needle body can be evenly coated with high-temperature epoxy resin to form a uniformly distributed adhesive layer.

[0042] In step s32:

[0043] Heat the container to 200℃, clean the spraying equipment, and then fill it with ceramic particles. Replace the spraying equipment with a 20cm long and 1cm wide sandblasting nozzle, and design the spraying angle of the sandblasting nozzle to be 45°~75°, specifically 45°, 50°, 55°, 60°, 65°, 70°, or 75°, etc. Set the spraying pressure of the spraying equipment to 0.05~0.3MPa, specifically 0.05MPa, 0.08MPa, 0.12MPa, 0.15MPa, 0.2MPa, 0.25MPa, or 0.3MPa, etc. Ensure that the distance between the sandblasting nozzle of the spraying equipment and the top of the magnetic needle body is 2cm.

[0044] Then run the spraying equipment to move the sandblasting nozzle along the x-axis at a speed of 38-52 cm / min from point 0 to point P, then reverse to point P', and then reverse back to point 0 to complete one spraying cycle (e.g., Figure 1 );

[0045] In this embodiment, points P and P′ are symmetrically arranged on the x-axis with point O as the center. The distance between points P and P′ is 200cm. The moving speed of the sandblasting nozzle can be 38cm / min, 40cm / min, 42cm / min, 44cm / min, 46cm / min, 48cm / min, 50cm / min or 52cm / min, etc.

[0046] During the spraying process, the current of the electromagnetic coil can be periodically and dynamically changed between 1 and 10A at a rate of 4A per minute, so that the magnetic needle body can be continuously shaken in the container. This, combined with the above-mentioned spraying path and parameter settings, ensures that the semi-solid adhesive layer can be evenly coated with ceramic particles to form a uniformly distributed ceramic layer.

[0047] In the above description, the ceramic layer is made of one or more combinations of chromium corundum, diamond, boron nitride, alumina, zirconium oxide, carbides, and titanium nitride. This ensures that the formed grinding magnetic needle has sufficient structural strength to perform surface polishing on workpieces primarily made of difficult-to-machine hard metals such as titanium alloys, high-temperature alloys, cobalt-chromium alloys, mold steel, and high-strength steel.

[0048] Preferably, the ceramic layer is made of chromium corundum, with a particle size of 90-110 μm and its main components being Al2O3 and Cr2O3, wherein Al2O3 accounts for 97.5% by mass and Cr2O3 accounts for 1.3% by mass. Because this chromium corundum has a hardness higher than most materials, it is highly suitable for polishing materials, resulting in high-quality polishing. Furthermore, its high hardness will not scratch the surfaces of metals with moderate hardness, such as titanium alloys and stainless steel.

[0049] It should be noted that multiple coating processes can be performed on the surface of the magnetic needle body as needed. This involves alternating layers of adhesive and ceramic layers on the outer surface of the needle body, with the outermost layer always being ceramic. To further improve the uniform distribution of the adhesive and ceramic layers on the needle body, when the nozzle moves to points P and P′ on the x-axis, the direction of the electromagnetic coil current within the container of the magnetic polishing machine needs to be changed. This alters the magnetic field direction, causing the original N pole to become the S pole and vice versa, thus changing the orientation of the magnetic needle body within the container and reducing coating dead zones caused by contact between the needle body and the container's inner wall.

[0050] The grinding magnetic needles prepared by this method have high grinding force and grinding efficiency. For the fine requirements of size, roughness and removal amount after polishing of the outer surface of complex irregular structures in additive manufacturing, based on the theory of outer cylindrical infeed grinding surface and engineering data accumulated in actual processing, empirical formulas are established between the removal amount, roughness and processing time process parameters of different materials, so as to meet the process parameter control requirements of fine size, roughness and removal amount under different materials.

[0051] For example, using a microscope to measure the dimensions of the crescent-shaped groove can help determine the amount of material removed from the groove wall during magnetic abrasion. Dimensional measurement methods include... Figure 5 As shown, Φ is measured respectively. max , l min ,l′ min Three sizes. Φ max The maximum diameter at the center of the crescent-shaped sulcus is measured by drawing circles at two tangent points under a microscope. The arc length AB on the left side is denoted as l. min The arc length of the right side A′B′ is denoted as l′. min The arc length was measured using a microscope's arc length tool. Specifically, a circle with a radius of 1 mm was drawn, centered at the cusp of the crescent moon, intersecting the crescent groove at points AB and A′B′. Φ was measured and recorded. max , l min ,l′ min The values ​​of these three parameters, along with processing time, provide data on the bilateral removal amount at the widest and narrowest points of the crescent groove. The removal amount at the widest and narrowest points of the crescent groove was chosen as the feature data because these two points represent the areas with the greatest difference in abrasive throughput and grinding effect.

[0052] Table 1 shows the dimensional inspection results of the composite magnetic needles after grinding. Φ was measured every hour starting from the 2nd hour. max , l min ,l′ min Three dimensions. As can be seen from the table, after a processing time of 6 hours, Φ max , l min ,l′ minThe three dimensions tend to stabilize. The bilateral removal amount at the widest point in the middle of the crescent groove is 0.226 mm, while the bilateral removal amounts at the two apex points of the crescent groove are 0.2 mm and 0.207 mm, respectively. This indicates that bonded abrasive grains can effectively remove material from high-temperature alloys through grinding. The removal amount after 8 hours can reach the thickness of a remelted layer of 0.05 mm to 0.2 mm after typical electrical discharge machining. However, the grinding efficiency still decreases after 6 hours, and the removal amount tends to reach its limit. Furthermore, the bilateral removal amount at the widest point in the middle of the crescent groove differs from that at the two apex points by approximately two times. This is because a higher abrasive throughput results in a better grinding effect.

[0053] Table 1. Dimensional inspection results of composite magnetic needles after grinding.

[0054]

[0055] The grinding magnetic needle prepared by this method and a traditional magnetic needle (i.e., the magnetic needle body in this method) were respectively applied to a magnetic polishing system to grind and polish the outer surface of a titanium alloy additive manufacturing process. The effect image after grinding and polishing is shown below. Figure 6 , Figure 6 The image on the left shows the effect of using a traditional magnetic needle in a magnetic polishing system to polish the outer surface of titanium alloy additive manufacturing. Figure 6 The image on the right shows the effect of using a traditional magnetic needle in a magnetic polishing system to polish the outer surface of titanium alloy additive manufacturing.

[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A method for preparing a grinding magnetic needle, characterized in that, Includes the following steps: Select a needle-shaped magnetic needle body with magnetic conductivity; Evenly sprinkle the magnetic needles into the container of the magnetic grinder, and adjust the direction and intensity of the magnetic field in the container to keep the magnetic needles vertical and ensure that adjacent magnetic needles are within a preset distance. Then, at least one spraying operation is performed on the surface of the magnetic needle body. During the spraying process, the current of the electromagnetic coil changes periodically between 1 and 10 A at a rate of 4 A per minute, causing the magnetic needle body to continuously shake inside the container. Each spraying operation includes: To form an adhesive layer, high-temperature epoxy resin heated to 300-350℃ is first evenly sprayed onto the surface of the magnetic needle body to form an adhesive layer. A ceramic layer is formed, and then the container is heated to at least 200°C. Ceramic particles are then evenly sprayed onto the adhesive layer to form the ceramic layer.

2. The method for preparing a grinding magnetic needle according to claim 1, characterized in that: The process of forming the adhesive layer or the ceramic layer is carried out by spraying equipment, and the nozzles of the spraying equipment spray in the following manner: The nozzle of the spraying equipment moves from point 0 to point P at a speed of 38~52cm / min on the x-axis, then moves in the opposite direction to point P′, and then moves in the opposite direction back to point 0 to complete one spraying cycle. Points P and P′ are arranged symmetrically on the x-axis with point O as the center.

3. The method for preparing a grinding magnetic needle according to claim 2, characterized in that: During the formation of the adhesive layer, the spraying pressure of the spraying equipment is 0.03~0.1MPa, the distance between the nozzle of the spraying equipment and the top of the magnetic needle body is 2cm, and the spraying angle of the nozzle of the spraying equipment is 45°~75°.

4. The method for preparing a grinding magnetic needle according to claim 2, characterized in that: During the formation of the ceramic layer, the spraying pressure of the spraying equipment is 0.05~0.3MPa, the distance between the nozzle of the spraying equipment and the top of the magnetic needle body is 2cm, and the spraying angle of the nozzle of the spraying equipment is 45°~75°.

5. The method for preparing a grinding magnetic needle according to claim 1, wherein the diameter d of the magnetic needle body is 0.1mm~5mm and its length is 1mm~10mm.

6. The method for preparing a grinding magnetic needle according to claim 1, wherein the magnetic needle body is formed by punching or wire cutting of wire material.

7. The method for preparing a grinding magnetic needle according to claim 1, wherein the material of the ceramic layer is one or more combinations of chromium corundum, boron nitride, alumina, zirconium oxide and titanium nitride.

8. The method for preparing a grinding magnetic needle according to claim 1, wherein the ceramic layer is made of chromium corundum, the particle size of which is 90-110 μm and its main components are Al2O3 and Cr2O3.

9. A grinding magnetic needle, characterized in that, The grinding magnetic needle is prepared by any one of claims 1-8.

10. An application of a grinding magnetic needle, characterized in that, The application of a grinding magnetic needle as described in claim 9 in a magnetic polishing system for polishing hard additive manufacturing structural parts.

Citation Information

Patent Citations

  • Magnetic needle grinding process optimization method based on surface roughness visual quantitative evaluation

    CN117300739A

  • Bar magnet is with automatic burring device in batches

    CN205271664U