Aluminum oxide green body surface roughness control method, semi-finished product and ceramic substrate

By regulating the surface roughness by vacuum packaging and isostatic pressure technology in the isostatic pressure treatment of alumina ceramic substrate, the problem of inaccurate control of surface roughness of alumina ceramic substrate in the prior art is solved, and the problem of inaccurate control of surface roughness of alumina ceramic substrate in the prior art is improved Porcelain performance and production efficiency are suitable for large-scale production.

CN118990743APending Publication Date: 2024-11-22XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411226920.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to accurately control the surface roughness of alumina ceramic substrates according to actual needs, resulting in prone to cracks, crushing and other problems during processing, affecting its application and development.

Method used

By vacuum packaging and isostatic pressure processing between the pressure plates with surface roughness Ra2, the surface roughness Ra1 is adjusted to ensure that Ra1 is close to Ra2. The specific steps include preset surface roughness, vacuum packaging, Isostatic pressure treatment, the temperature is 55-60℃, the pressure is 60-80Mpa, and the insulation is 45-60 minutes.

Benefits of technology

It realizes precise control of the surface roughness of alumina ceramic substrate, avoids cracks and collapses during processing, improves porcelain performance, is suitable for large-scale production, and has the advantages of low cost and high efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005025463170000061
    Figure BDA0005025463170000061
  • Figure BDA0005025463170000071
    Figure BDA0005025463170000071
Patent Text Reader

Abstract

The invention relates to the technical field of ceramic materials, and provides an aluminum oxide green body surface roughness control method which comprises the following steps: step 1, presetting the surface roughness Ra1 of a required aluminum oxide green body; step 2, clamping the aluminum oxide green body between pressing plates with the surface roughness of Ra2, and performing vacuum packaging; step 3, isostatic pressing treatment; according to the method, the surface roughness of the aluminum oxide green body can be accurately regulated and controlled according to actual production requirements, and the method is suitable for large-batch production activities; the invention also discloses the semi-finished product and the ceramic substrate which are prepared by the method, and the semi-finished product and the ceramic substrate have the characteristics of controllable roughness and convenience for carrying out subsequent processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of ceramic materials, and in particular to a method for controlling the surface roughness of an alumina green body, a semi-finished product, and a ceramic substrate. Background Art

[0002] Ceramic substrate materials are widely used in power electronics, electronic packaging, hybrid microelectronics and multi-chip modules due to their excellent thermal conductivity and air tightness.

[0003] The quality of ceramic substrates is mainly reflected in parameters such as density, bending strength, flatness, and surface roughness. Among them, surface roughness affects the adsorption and friction processes of ceramic substrates. For ceramic membranes, surface roughness affects the filtration of ceramic membranes and has an important impact on the continuity of the resistor film layer. In addition, the surface roughness of ceramic substrates is not the smaller the better. Different ceramic substrates have slightly different requirements for surface roughness, which is mainly reflected in the fact that appropriate surface roughness is more conducive to subsequent attachment processes.

[0004] At present, the traditional surface treatment methods of ceramic substrates are mainly grinding, polishing, ultrasonic processing, laser processing, physical vapor deposition, etc. However, due to the high hardness and brittleness of the ceramic substrate itself, cracks and breakages are prone to occur during the processing. Therefore, exploring suitable surface treatment methods for ceramic substrates is of great significance for the application and further development of ceramic substrate materials.

[0005] CN107658230A discloses a method for regulating the surface roughness of a raw ceramic sheet and a LTCC substrate, comprising the following steps: stacking a raw ceramic sheet with a polymer film on a flat steel plate; after fixing the raw ceramic sheet, the steel plate and the polymer film, performing vacuum packaging; and performing isostatic pressing. Combined with its specification, it can be seen that the above-mentioned method for regulating the surface roughness of the raw ceramic sheet is mainly to reduce the surface roughness of the raw ceramic sheet by continuously increasing the temperature, pressure and other parameters of the isostatic pressing, and still fails to achieve accurate increase or decrease of the surface roughness of the ceramic substrate according to actual needs.

[0006] Based on this, the technical problem solved in this case is: how to control the surface roughness of the alumina green body according to actual needs, and then obtain an alumina ceramic substrate with a suitable surface roughness.

[0007] Application Contents

[0008] In order to solve the above technical problems, the present application provides a method for controlling the surface roughness of an alumina green embryo. The method can accurately adjust the surface roughness of an alumina green embryo according to actual production needs and is suitable for large-scale production activities. The present application also discloses a semi-finished product and a ceramic substrate obtained by the above method, both of which have the characteristics of controllable roughness and are convenient for subsequent processes.

[0009] The technical solution of this application is:

[0010] A method for controlling the surface roughness of an alumina green embryo comprises the following steps in sequence:

[0011] Step 1: Preset the required surface roughness Ra1 of the alumina green body;

[0012] Step 2: sandwiching the alumina green body between pressing plates with a surface roughness of Ra2 and vacuum packaging;

[0013] Step 3: isostatic pressing;

[0014] Among them, Ra2=Ra1+0.22~0.23μm, including but not limited to 0.22μm, 0.225μm, and 0.23μm.

[0015] The present application performs isostatic pressing by placing an alumina green body with a surface roughness of Ra1 between pressing plates with a surface roughness of Ra2. During the isostatic pressing process, the surface roughness Ra1 of the alumina green body will continuously approach the surface roughness Ra2 of the pressing plate. However, due to the material properties of alumina, Ra1 and Ra2 cannot be completely consistent, and there will be a gap of 0.22 to 0.23 μm. Therefore, in actual production, the present application can achieve the purpose of accurately controlling the surface roughness Ra1 of the alumina green body by adjusting Ra2 of the pressing plate.

[0016] In the above-mentioned method for controlling the surface roughness of alumina green body, Ra1 is 1.3-2.5 μm. It should be noted that this surface roughness range is only a preferred range for the properties of alumina in practical applications.

[0017] In the above-mentioned alumina green embryo surface roughness control method, the temperature of isostatic pressing in step 3 is 55-60° C., including but not limited to 55° C., 56° C., 57° C., 58° C., 59° C., and 60° C., and the pressure is 60-80 MPa, including but not limited to 60 MPa, 63 MPa, 65 MPa, 68 MPa, 70 MPa, 72 MPa, 75 MPa, 78 MPa, and 80 MPa, and the temperature and pressure are maintained for 45-60 min, including but not limited to 45 min, 50 min, 55 min, and 60 min.

[0018] In the above-mentioned method for controlling the surface roughness of alumina green body, the material of the pressing plate is any one of glass, plastic and metal.

[0019] In the above-mentioned method for controlling the surface roughness of the alumina green body, the pressing plate is glass with a surface roughness of Ra2, and the thickness of the glass is 1 to 3 mm.

[0020] In the above-mentioned method for controlling the surface roughness of an alumina green body, in step 2, the alumina green body is sandwiched between pressing plates having different surface roughnesses.

[0021] The present application also discloses a semi-finished alumina ceramic substrate, which is prepared by the above-mentioned method for controlling the surface roughness of an alumina green body.

[0022] The present application also discloses an alumina ceramic substrate, which is obtained by sintering the alumina ceramic substrate semi-finished product as described above.

[0023] The present application is based on the sintering shrinkage of the alumina green body in actual production and combined with the surface roughness control method of the basic solution, so as to obtain an alumina ceramic substrate with suitable surface roughness.

[0024] One of the above technical solutions of the present application has at least one of the following advantages or beneficial effects:

[0025] The present application places an alumina green body with a surface roughness of Ra1 between pressing plates with a surface roughness of Ra2 for isostatic pressing. In actual production, the present application can achieve the purpose of accurately controlling the surface roughness Ra1 of the alumina green body by adjusting the Ra2 of the pressing plate. The entire surface roughness treatment method is that before sintering, it will not cause damage to the finished porcelain, but can improve the performance of the finished porcelain through isostatic pressing.

[0026] In addition, according to the sintering shrinkage of the alumina green body in actual production, combined with the surface roughness control method of the basic solution, an alumina ceramic substrate with suitable surface roughness can be obtained. This application is suitable for mass production and has the advantages of low cost, high efficiency and excellent effect. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0028] The alumina green body of the present application is prepared by tape casting. Preferably, the alumina green body used in the following examples of the present application has a preparation process comprising the following steps:

[0029] First ball milling: 2 kg of alumina powder and a solvent were mixed and put into a ball mill, and then 1.5 kg of alumina balls with a size of 5 mm and 2.5 kg of alumina balls with a size of 15 mm were put into the ball mill, and the mixture was ball milled at a speed of 300 rpm for 12 hours to obtain a first mixed solution, wherein the solvent was a mixed solution of 0.2 kg of butanone and 0.3 kg of ethanol;

[0030] Secondary ball milling: the first mixed solution was mixed with 0.088 kg of acrylic polymer (binder) and 0.044 kg of dibutyl phthalate (plasticizer), and ball milled at a speed of 400 rpm for 16 h to obtain a second mixed solution;

[0031] Degassing and aging: The second mixed solution was transferred to a 15L degassing reactor through a 200-mesh filter, and then the degassing reactor was set, the constant temperature water was cooled to 22°C, stirring was started at a speed of 20r / min, vacuumed to -0.09Mpa, degassed for 1h, and then pressure-maintained and aged for 3h to obtain a slurry;

[0032] Tape casting: After the aging treatment is completed, open the valve to release the negative pressure, fill in nitrogen until the positive pressure of the degassing reactor reaches 0.08Mpa, transfer the slurry to the tape casting machine, filter it, and use the five-stage drying mode of 30℃, 40℃, 50℃, 60℃ and 75℃ for the drying channel of the tape casting machine. Turn on the tape casting film belt and adjust the speed to 0.3M / Min for tape casting. Adjust the scraper height to 650μm to flow out the alumina green embryo with uniform thickness of 200μm.

[0033] The alumina green embryos were cut to a width of 160 mm, placed in an oven at 120°C for drying for 5 hours, and punched into 150*150 mm alumina green embryos after cooling. The surface roughness was tested, and the surface roughness of the surface in contact with the cast paper was 0.77 μm, and the surface roughness of the surface in contact with the air was 1.42 μm.

[0034] Example 1

[0035] A method for controlling the surface roughness of an alumina green embryo comprises the following steps in sequence:

[0036] Step 1: Preset the required surface roughness Ra1 of the alumina green body. In this embodiment, Ra1 is 1.1 μm.

[0037] Step 2: Processing the glass to make its surface roughness satisfy Ra2=Ra1+0.22-0.23 μm. In this embodiment, the surface roughness Ra2 of the glass finally processed is 1.328 μm and the thickness is 2 mm. Then, the alumina green body prepared in Example 1 is sandwiched between two pieces of glass in this embodiment and vacuum-sealed.

[0038] Step 3: isostatically press the package obtained in step 2, wherein the isostatic pressing temperature is 60° C., the pressure is 80 MPa, and the temperature and pressure are maintained for 60 minutes.

[0039] Example 2

[0040] It is basically the same as Example 2, except that: in step 3, the temperature of the isostatic pressure is 40° C., the pressure is 80 MPa, and the temperature and pressure are maintained for 60 minutes.

[0041] Example 3

[0042] It is basically the same as Example 2, except that: in step 3, the temperature of the isostatic pressure is 100° C., the pressure is 80 MPa, and the temperature and pressure are maintained for 60 minutes.

[0043] Example 4

[0044] It is basically the same as Example 2, except that: in step 3, the temperature of the isostatic pressure is 60° C., the pressure is 40 MPa, and the temperature and pressure are maintained for 60 minutes.

[0045] Example 5

[0046] It is basically the same as Example 2, except that: in step 3, the temperature of the isostatic pressure is 60° C., the pressure is 60 MPa, and the temperature and pressure are maintained for 60 minutes.

[0047] Example 6

[0048] A method for controlling the surface roughness of an alumina green embryo comprises the following steps in sequence:

[0049] Step 1: Preset the required surface roughness Ra1 of the alumina green body. In this embodiment, the surface roughness Ra1 of the two sides of the alumina green body is required to be 2.5 μm and 1.3 μm respectively.

[0050] Step 2: Processing the glass to make its surface roughness satisfy Ra2=Ra1+0.22-0.23 μm. In this embodiment, the first pressing plate with a surface roughness Ra2 of 2.755 μm and the second pressing plate with a surface roughness Ra2 of 1.53 μm are finally processed, and the thickness is 2 mm. Then, the alumina green body prepared in Example 1 is sandwiched between the first pressing plate and the second pressing plate, and vacuum-packaged;

[0051] Step 3: isostatically press the package obtained in step 2, wherein the isostatic pressing temperature is 60° C., the pressure is 80 MPa, and the temperature and pressure are maintained for 60 minutes.

[0052] Test: The surface roughness of the semi-finished alumina ceramic substrates obtained in Examples 1 to 6 was tested. The results are as follows:

[0053] Table 1: Surface roughness and error of the semi-finished alumina ceramic substrates of Examples 1 to 6

[0054]

[0055] Example 7

[0056] It is basically the same as Example 1, except that: in this example, 4 alumina green billets are isostatically pressed at the same time, specifically, 4 alumina green billets are stacked in the order of pressing plate, alumina green billets, and pressing plate, and then vacuum packaged.

[0057] In this embodiment, it should be noted that the number of alumina green sheets processed at a single time in this application is only related to mechanical factors such as the isostatic pressing device and glass thickness. In other embodiments, it is also feasible to isostatically press 5 or 6 alumina green sheets at the same time.

[0058] Test: The surface roughness of the semi-finished alumina ceramic substrate obtained in Example 7, the results are as follows:

[0059] Table 2: Surface roughness and error of each layer of alumina green body in Example 7

[0060]

[0061] Example 8

[0062] The alumina green body obtained by sintering and casting and the alumina ceramic substrate semi-finished products obtained in Examples 1 to 7 were put into a furnace, heated to 800°C at a heating rate of 1.5°C / min, kept warm for 3 hours, then heated to 1400°C, kept warm for 5 hours, and naturally cooled to obtain alumina ceramic substrates. The surface roughness of each example was tested, and the results are shown in the following table.

[0063] Table 3: Surface roughness of ceramic substrates of Examples 1 to 7

[0064] Ceramic substrate surface roughness (Ra) Example 1 0.962 Example 2 0.955 Example 3 0.954 Example 4 0.961 Example 5 0.951 Example 6 2.17 / 1.12 Example 7 (average value) 0.962

[0065] Result analysis:

[0066] Comparing Examples 1 to 3, the surface roughness of the final alumina green bodies of the three are relatively small, and Example 1 is slightly closer to the preset surface roughness, indicating that within the appropriate isostatic pressing temperature range, the temperature has little effect on the results.

[0067] Comparing Example 1 with Examples 4 and 5, under the same temperature and heat preservation and pressing time, the effect of Example 4 is worse. It is speculated that the reason is that Example 4 cannot fully imprint the alumina green body and the glass under the condition of low pressure. After appropriately extending the heat preservation and pressing time, the error is significantly reduced.

[0068] Example 6 proves that the present application can simultaneously control the surface roughness of both sides of the alumina green body, and it still complies with the rule of Ra2=Ra1+0.22-0.23 μm.

[0069] In the case of lamination, the characteristics of isostatic pressing make the alumina green body still conform to the rule of Ra2=Ra1+0.22~0.23μm, and the difference between each layer is very small, so that the solution of the present application is suitable for large-scale production.

[0070] According to the reduction ratio of the surface roughness of the ceramic substrate in Example 8, surprisingly, the reduction ratio of the surface roughness of the alumina ceramic substrate has a significant relationship with the sintering shrinkage rate, specifically: the sintering shrinkage rate of the alumina green embryo obtained by test calculation is 14.08%, and the reduction ratio of the surface roughness of the ceramic substrate and the semi-finished product is very close to the sintering shrinkage rate, that is, the surface roughness of the ceramic substrate ≈ (1-14.08%) * the semi-finished alumina ceramic substrate. This makes the surface roughness of the alumina ceramic substrate controllable in actual production, which has great practical significance.

Claims

1. A method for controlling the surface roughness of an alumina green body, It is characterized in that The following steps are included in sequence: Step 1: Preset the required surface roughness Ra of the alumina green body 1 ; Step 2: Clamp the alumina green body with a surface roughness of Ra 2 Vacuum packaging between the pressure plates; Step 3: isostatic pressing; Among them, Ra 2 =Ra 1 +0.22~0.23μm.

2. The method for controlling the surface roughness of an alumina green body according to claim 1, It is characterized in that Ra 1 1.3~2.5μm.

3. The method for controlling the surface roughness of an alumina green body according to claim 1, It is characterized in that In step 3, the temperature of the medium static pressure is 55-60° C., the pressure is 60-80 MPa, and the temperature and pressure are maintained for 45-60 minutes.

4. The method for controlling the surface roughness of an alumina green body according to claim 1, It is characterized in that The material of the pressure plate can be any one of glass, plastic and metal.

5. The method for controlling the surface roughness of an alumina green body according to claim 4, It is characterized in that The surface roughness of the pressure plate is Ra 2 The glass has a thickness of 1 to 3 mm.

6. The method for controlling the surface roughness of an alumina green body according to claim 1, It is characterized in that In step 2, the alumina green body is sandwiched between press plates with different surface roughnesses.

7. A semi-finished alumina ceramic substrate, It is characterized in that The aluminum oxide green body is prepared by the surface roughness control method of any one of claims 1-6.

8. An alumina ceramic substrate, It is characterized in that It is obtained by sintering the semi-finished alumina ceramic substrate as claimed in claim 7.

Citation Information

Cited By

  • Forming method and forming die of large-size flaky ceramic and ceramic

    CN122323356A

  • Forming methods, molding dies, and ceramics for large-size thin-sheet ceramics