Design method of special-shaped rubber precise extrusion die head
By characterizing the rheological characteristics of rubber materials and designing two-stage dies, the problem of precise control of the form and size of special-shaped rubber products is solved, high-precision molding and efficient production are achieved, and yield and production efficiency are improved.
Patent Information
- Application Number
- CN202310562505.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, it is difficult to accurately control the form and size of the special-shaped rubber products, resulting in inaccurate shape of the semi-finished products of extruded molding, inconsistent internal structure and performance, low production efficiency and low yield.
By characterizing the rheological characteristics of rubber materials, a two-stage die head, including flow guide sections and mouth sections, is designed, combined with rheology theory and simulation calculations, the mold shape and size of the die head are optimized to ensure the uniform flow and molding quality of the rubber material.
It realizes high-precision molding of special-shaped rubber products, improves production efficiency and yield, ensures the consistency of the structure and performance of the products, and shortens the R&D cycle.
Smart Images

Figure CN118990980A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of rubber material processing, and in particular to a design method for a special-shaped rubber precision extrusion die head. Background Art
[0002] The rubber industry is one of the important basic industries of the national economy. It not only provides people with daily necessities, medical and other light industrial rubber products that are indispensable in daily life, but also provides various rubber production equipment or rubber parts to heavy industries and emerging industries such as mining, transportation, construction, machinery, and electronics.
[0003] The production of rubber products generally goes through several processes such as mixing, molding and vulcanization. The main methods of rubber molding are injection molding, compression molding, extrusion molding and die-casting molding. Extrusion molding, also known as compression molding, is a basic molding method in the production of rubber products. It is a processing method that preheats and plasticizes the rubber in the extruder, and continuously pushes the rubber through the rotation of the screw. Under the strong extrusion pressure of the screw tip and the barrel wall, and with the help of a basic mold (die head) with a certain shape, it becomes a semi-finished product with a certain geometric shape and size. The final molding also requires cutting the various films, tapes, etc. extruded into parts of different specifications according to the shape of the product, and then laminating them to make semi-finished products.
[0004] Special-shaped rubber refers to rubber extrusion products with irregular cross-sectional shapes. In the extrusion molding process, the shaping part of the die determines the cross-sectional shape of the rubber material. However, due to the unevenness of the flow field intensity and distribution, as well as the influence of the extrusion expansion effect, the precise control of the shape and size of special-shaped rubber products has always been a technical problem in the high-precision production of rubber products.
[0005] In the prior art, the design of the extrusion die mainly adopts the "trial and error" method to test the extrusion quality of the rubber compound. Since this design idea does not take into account the viscoelastic properties of the rubber compound, the shape accuracy of the extruded semi-finished product is poor, and the consistency of the internal structure and performance is not guaranteed. It is not only time-consuming and labor-intensive, but also has a low yield. In the rubber compound extrusion process, mastering the rheological behavior of the rubber compound and conducting a reasonable flow channel design have become new difficulties in improving the extrusion quality of tire rubber compound. Summary of the invention
[0006] The present invention is to overcome the defects in the prior art and provide a design method for a special-shaped rubber precision extrusion die head. To achieve the above-mentioned invention object, the present invention is implemented by the following technical solutions:
[0007] The present invention provides a die head design method for precise extrusion molding of special-shaped rubber products, which is characterized by comprising five steps:
[0008] (S.1) Characterize the rheological properties of materials;
[0009] (S.2) Converting the target shape and size of the special-shaped rubber product into a metal processable shape and size;
[0010] (S.3) Obtaining a preliminary design scheme for the die morphology through rheological theory calculation;
[0011] (S.4) Verification of simulation calculations to verify the rationality of the preliminary design of the die shape;
[0012] (S.5) Based on the simulation results, the die shape design is further optimized and the die metal sheet design is determined.
[0013] In one embodiment of the present invention, step S.1 includes using a rheological device to test the rheological properties and extrusion swell law of the rubber material, and clarifying the processing window, rheological characteristic parameters, extrusion swell rate and aspect ratio corresponding to the fully developed zone of the rubber material.
[0014] Rubber is a viscoelastic polymer material, and its rheological properties are closely related to the quality and efficiency of extrusion molding. During the extrusion process, the rubber material will be subjected to tensile and compressive forces, and a complex flow state will be formed inside the die. Therefore, when designing the geometry and size of the die, it is necessary to consider the viscoelastic properties of the rubber material to ensure the uniformity and stability of extrusion molding, thereby improving the quality and efficiency of extrusion molding.
[0015] In another embodiment of the present invention, in step S.2, the target shape size can be converted into a metal-machinable shape size by computer-aided software drawing. When drawing by computer-aided software, the following principles need to be observed: (1) The dimensional accuracy of the converted graphic shape and the target shape of the shaped rubber is ≥ 95%; (2) The cross-sectional area of the converted graphic shape and the target shape of the shaped rubber remains equal; (3) The sharp angles in the target shape of the shaped rubber need to be converted into small arcs that can be processed by metal; (4) The design of the die plate needs to take into account the parameters of the extruder and the extrusion die, including the maximum volume flow rate, pressure, flow rate and distribution of the die outlet, and pressure drop of the extruder.
[0016] The purpose of converting the target shape size of the shaped rubber into the metal machinable shape size is to facilitate the manufacture of metal molds for the production of shaped rubber products. Through computer-aided software drawing, the target shape size of the shaped rubber can be converted into a digital metal shape drawing, and then through CNC processing equipment, the digital metal shape drawing can be directly converted into an actual metal mold for the production of shaped rubber products. Converting the target shape size of the shaped rubber into the metal machinable shape size can improve the production efficiency and quality of shaped rubber products, while also reducing production costs and improving production benefits.
[0017] In another embodiment of the present invention, in step S.3, according to the metal machinable form determined in step S.2, the die head is decomposed into multiple regions and different geometric shapes, and according to the design of the die head geometric structure, the die heads of different regions and different shapes are calculated to obtain the size of the die head geometric structure. The specific steps include:
[0018] S.3.1 Die geometry
[0019] The design adopts a two-stage die head. The first section is the flow guide section and the second section is the die section. One end of the flow guide section is connected to the extruder and the other end is connected to the die section. The die section is used to achieve molding and shaping. Along the flow direction of the fluid, the height of the flow guide section gradually decreases, and the height of the die section gradually decreases.
[0020] The guide section is the first section of the die head, and its main function is to guide the rubber melt in the extruder to the die section of the die head. The gradual reduction in the height of the guide section can effectively increase the flow rate and pressure of the melt, so as to better guide the melt to flow into the die section and maintain the stability of the fluid. The die section is the second section of the die head, and its main function is to form the melt into the required shape and size. The gradual reduction in the height of the die section can be optimized according to the shape and size of the product to ensure that the product can be fully formed and shaped in the die section. The design of the die head needs to take into account the design of the guide section and the die section to ensure that the melt can flow evenly and reach the maximum flow rate and pressure, while ensuring that the product can obtain the best molding effect and quality. Through the reasonable design of the guide section and the die section, the production efficiency and quality of special-shaped rubber products can be improved.
[0021] S.3.2 Calculation of die size
[0022] (1) Shear rate Calculation
[0023] Determine the fluid tear strength σ of the material in the processing temperature window and calculate it according to formula 1
[0024]
[0025] In formula 1, S is the cross-sectional area of the rubber extrudate, which can be determined by measuring the dimensions of the extrudate, or measured and calculated by the dimension measurement system of the capillary rheometer; F is the tensile force corresponding to the material being broken, which is given by the tensile mode test of the capillary rheometer;
[0026] According to formula 2, the tensile rate corresponding to the fracture of rubber fluid is calculated
[0027]
[0028] In formula 2, η E It is the extensional viscosity of the rubber extrudate;
[0029] To prevent fluid breakage or edge tearing during stretching or extrusion processing, the stretching rate is selected is 50% of the tensile rate corresponding to the rupture of the rubber fluid, that is,
[0030] The shear rate was calculated according to Equation 3.
[0031]
[0032] In formula 3, Q is the volume flow rate, that is, the volume of rubber passing through the die per unit time. For a given extruder, its matching volume flow rate Q is given; according to Figure 3 , A is the cross-sectional area of the flow channel, which is calculated from the die design dimensions, among which the ellipse with the largest cross-sectional area (see Figure 3 The length of the minor axis of the dotted ellipse is 2a, the length of the major axis is 2b, and the length of the longest diagonal of the cross section is 2c;
[0033] According to the above parameters, define X=a / b≤1, Y=c / b≥1; for the tube-type flow channel, X=1 and Y=1, and for the slit-type flow channel, X=0 and Y=1.
[0034] (2) Calculation of die size
[0035] The total thickness of the die is L, the thickness of the first section is L1, the thickness of the second section is L2, the inlet angle of the first section is α, α≤45°, and the inlet angle of the second section is 2θ; the height of the flow channel outlet of the matching extrusion die is D in , the die outlet height is D out , the height D of the intersection of the two-stage lip design mid .
[0036] For a given extruder, the height D of the flow channel outlet of its matching extrusion die head is in and volume flow rate Q are given; the inlet angle of the second section is 2θ as a set value.
[0037] Calculate die outlet height D out , D out = height of the converted metal processable form / rubber extrusion swell ratio;
[0038] According to formula (4), the shear rate of the flow channel is calculated as
[0039]
[0040] Calculate Dmid , D mid =2a, calculate the height D of the intersection of the two-stage lip design according to equations 3 and 4 mid ;
[0041] According to formula (5), L1 is calculated.
[0042] L1=(D in -D mid ) / 2tan22.5° (Formula 5)
[0043] Set θ and calculate L2 according to formula (6),
[0044] L2=(D mid -D out ) / 2tanθ (Formula 6)
[0045] According to formula 7, L
[0046] L=L1+L2 (Formula 7).
[0047] By using the above calculation method, the dimensions of dies in different regions and shapes are calculated.
[0048] The flow channel of the die head should have appropriate length and angle to ensure the fluidity and uniformity of the rubber material, thereby reducing material compression and heat accumulation.
[0049] Preferably, a fluid flow factor m is introduced for correction, and the fluid flow factor m is obtained by capillary rheometer testing. Formula (3) is corrected, and formula (8) is used to calculate the shear rate of the tube-type flow channel, and formula (9) is used to calculate the shear rate of the slit-type flow channel.
[0050]
[0051]
[0052] In die design, the flow rate and pressure of the melt are usually determined by the geometry of the die and the parameters of the extruder. However, in actual production, the flow rate and pressure of the melt will be affected by many factors, such as the viscosity, density, temperature, etc. of the melt. These factors will cause nonlinear changes in the flow rate and pressure of the melt, thereby affecting the design accuracy of the die and the molding quality of the product. In order to solve this problem, the fluid flow factor m is introduced into the die design. The fluid flow factor m is a dimensionless parameter, which can be used to describe the nonlinear changes in the flow rate and pressure of the melt during the flow process inside the die. By introducing the fluid flow factor m for correction, the flow rate and pressure of the melt can be predicted more accurately, thereby improving the design accuracy of the die and the molding quality of the product.
[0053] In another embodiment of the present invention, in step S.4, a simulation verification is performed on the die plate designed based on the rheological theory calculation data. The process includes the following steps:
[0054] S.4.1 Design morphology and draw using computer-aided design software;
[0055] S.4.2 Meshing is performed using finite element analysis methods;
[0056] S.4.3 Construction of constitutive equation: Test the viscoelastic properties of the rubber to obtain rheological characteristic parameters, relaxation time τ and zero shear viscosity η0. Construct the constitutive equation through the PTT model or BKZ model, and perform multi-model fitting based on the rheological curve.
[0057] PTT model constitutive equation:
[0058]
[0059]
[0060] BKZ model constitutive equation:
[0061]
[0062]
[0063] S.4.4 Based on the above equations, select 3 to 5 relaxation models, perform simulation calculations, and obtain pressure and velocity distribution cloud diagrams to verify the rationality of the design.
[0064] Through numerical simulation analysis, the accuracy of the die plate designed based on rheological theory calculation data can be verified, and the design parameters of the die plate can be further optimized and adjusted to achieve the best molding effect and product yield.
[0065] In another embodiment of the present invention, in step S.5, the die head process morphology design scheme is further optimized according to step S.3 and step S.4, and the design scheme of the metal sheet is determined.
[0066] Therefore, the present invention has the following beneficial effects:
[0067] (1) The present invention constructs a design method with clear scientific principles and can accurately customize high-precision process morphology based on the rheological properties of rubber materials. The present invention combines the processing rheological properties and extrusion expansion characteristics of rubber materials, obtains the process morphology through rheological theory calculation, and finally obtains the design method of the process morphology through simulation calculation and verification based on the constitutive equation. This method saves time and effort, and the process morphology of the prepared rubber products is highly accurate, and the internal structure and performance have good consistency. It can shorten the R&D cycle, improve production efficiency, and improve product performance and yield rate. It is the key to breaking through the rubber precision manufacturing technology.
[0068] (2) The flow guide design is introduced into the die design, which has the characteristics of a two-stage structure. The advantage of this design is that it can effectively suppress the rupture of the fluid and widen the processing window. While ensuring that the thickness of the die plate is ≤20mm, it can provide a fully developed area to suppress the extrusion expansion rate of the material. Its extrusion expansion rate is equivalent to the effect of 3 to 4 times the thickness of the traditional die plate.
[0069] (3) The composition of rubber materials is complex, and its fluid behavior is non-Newtonian. Therefore, for products that require extremely high precision in extrusion, the fluid flow factor m is introduced for correction to ensure the precise molding of the shaped rubber. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Figure 1 This is an example diagram of the target shape of the special-shaped rubber product of the present invention.
[0071] Figure 2 This is an example diagram of a metal processable shape obtained by transforming the target shape of the special-shaped rubber product of the present invention.
[0072] Figure 3 It is a schematic diagram of the extrusion flow channel and die head of the present invention.
[0073] Figure 4 It is a schematic diagram of the die plate with flow guide design of the present invention. DETAILED DESCRIPTION
[0074] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments of the specification. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0075] The present invention first provides a die head design method for accurate extrusion molding of rubber product process morphology, which includes five steps:
[0076] (S.1) Characterize the rheological properties of materials;
[0077] (S.2) converting the target form into a metal processable form;
[0078] (S.3) Rheological theory calculation to obtain the preliminary design of the die shape;
[0079] (S.4) Verification of simulation calculations to verify the rationality of the preliminary design of the die shape;
[0080] (S.5) Based on the simulation results, the die head shape design is further optimized and the design of the metal sheet is determined.
[0081] Step S.1 includes using rheological equipment to test the rheological properties and extrusion expansion law of the rubber material, and clarifying the processing window, rheological characteristic parameters, extrusion expansion rate and aspect ratio corresponding to the fully developed zone of the rubber material.
[0082] In step S.2, the target shape size can be converted into a metal-machinable shape size by computer-aided software drawing. When drawing with computer-aided software, the following principles need to be observed: (1) The dimensional accuracy of the converted graphic shape and the target shape of the shaped rubber is ≥ 95%; (2) The cross-sectional area of the converted graphic shape and the target shape of the shaped rubber remains equal; (3) The sharp angles in the target shape of the shaped rubber need to be converted into small arcs that can be processed by metal; (4) The design of the die plate needs to consider the parameters of the extruder and the extrusion die, including the maximum volume flow rate, pressure, flow rate and distribution of the die outlet, and pressure drop of the extruder.
[0083] In step S.3, according to the metal processable form determined in step S.2, the die head is decomposed into multiple regions and different geometric shapes (tube type or slit type), and calculations are performed on the dies in different regions and shapes, including the shear rate, the geometric structure and size of the die plate.
[0084] The specific steps include:
[0085] S.3.1 Die geometry
[0086] The design adopts two stages, as shown in the attached Figure 4 As shown. The die head consists of two sections, the first section is the flow guide section, and the second section is the die section. One end of the flow guide section is connected to the extruder head, and the other end is formed and shaped through the die section. Along the flow direction of the fluid, the height of the flow guide section gradually decreases, and the height of the die section gradually decreases.
[0087] S.3.2 Calculation of die size
[0088] (1) Shear rate Calculation
[0089] Determine the fluid tear strength σ of the material in the processing temperature window and calculate it according to formula 1
[0090]
[0091] In formula 1, S is the cross-sectional area of the rubber extrudate, which can be determined by measuring the dimensions of the extrudate, or measured and calculated by the dimension measurement system of the capillary rheometer; F is the tensile force corresponding to the material being broken, which is given by the tensile mode test of the capillary rheometer;
[0092] According to formula 2, the tensile rate corresponding to the fracture of rubber fluid is calculated
[0093]
[0094] In formula 2, η E It is the extensional viscosity of the rubber extrudate;
[0095] To prevent fluid breakage or edge tearing during stretching or extrusion processing, the stretching rate is selected is 50% of the tensile rate corresponding to the rupture of the rubber fluid, that is,
[0096] The shear rate was calculated according to Equation 3.
[0097]
[0098] In formula 3, Q is the volume flow rate, that is, the volume of rubber passing through the die per unit time; Figure 3 , A is the cross-sectional area of the flow channel, which is calculated from the die design dimensions, among which the ellipse with the largest cross-sectional area (see Figure 3 The length of the minor axis of the dotted ellipse is 2a, the length of the major axis is 2b, and the length of the longest diagonal of the cross section is 2c;
[0099] According to the above parameters, define X = a / b ≤ 1, Y = c / b ≥ 1, then for the tube-type flow channel, X = 1 and Y = 1, for the slit-type flow channel, X = 0 and Y = 1;
[0100] (2) Calculation of die size
[0101] The total thickness of the die is L, the thickness of the first section is L1, the thickness of the second section is L2, the inlet angle of the first section is α, α≤45°, and the inlet angle of the second section is 2θ; the height of the flow channel outlet of the matching extrusion die is D in , the die outlet height is D out , the height D of the intersection of the two-stage lip design mid ;
[0102] Given an extruder, the height D of the flow channel outlet of its matching extrusion die head in and volume flow rate Q are given; the inlet angle of the second section is 2θ as the set value;
[0103] Calculate die outlet height D out , D out = height of the converted metal processable form / rubber extrusion swell ratio;
[0104] According to formula (4), the shear rate of the flow channel is calculated as
[0105]
[0106] Calculate D mid , D mid =2a value, calculate the height D of the intersection of the two-stage lip design according to equations 3 and 4 mid ;
[0107] According to formula (5), L1 is calculated.
[0108] L1=(D in -D mid ) / 2tan22.5° (Formula 5)
[0109] Set θ and calculate L2 according to formula (6),
[0110] L2=(D min -D out ) / 2tanθ (Formula 6)
[0111] According to formula 7, L
[0112] L=L1+L2 (Formula 7).
[0113] By using the above calculation method, the dimensions of dies in different regions and shapes are calculated.
[0114] The fluid flow factor m is introduced for correction, and the fluid flow factor m is obtained by capillary rheometer test. Formula (3) is corrected, and formula (8) is used to calculate the shear rate of the tube-type flow channel, and formula (9) is used to calculate the shear rate of the slit-type flow channel.
[0115]
[0116]
[0117] In step S.4, the die plate designed based on the rheological theory calculation data is simulated and verified. The process includes the following steps:
[0118] S.4.1 Design morphology and draw using computer-aided design software;
[0119] S.4.2 Meshing is performed using finite element analysis methods;
[0120] S.4.3 Construction of constitutive equation: Test the viscoelastic properties of the rubber to obtain rheological characteristic parameters, relaxation time τ and zero shear viscosity η0. Construct the constitutive equation through the PTT model or BKZ model, and perform multi-model fitting based on the rheological curve.
[0121] PTT model constitutive equation:
[0122]
[0123]
[0124] BKZ model constitutive equation:
[0125]
[0126]
[0127] S.4.4 Based on the above equations, select 3 to 5 relaxation models, perform simulation calculations, and obtain pressure and velocity distribution cloud diagrams to verify the rationality of the design.
[0128] In step S.5, according to step S.3 and step S.4, the die head process morphology design scheme is further optimized to determine the design scheme of the metal sheet.
[0129] The above embodiments are provided only to illustrate the present invention, and are not intended to limit the protection scope defined by the appended claims.
Claims
1. A die head design method for precise extrusion molding of special-shaped rubber products, characterized in that: It includes five steps: (S.1) Characterize the rheological properties of materials; (S.2) Converting the target shape and size of the special-shaped rubber product into a metal processable shape and size; (S.3) Obtaining a preliminary design scheme for the die morphology through rheological theory calculation; (S.4) Verification of simulation calculations to verify the rationality of the preliminary design of the die shape; (S.5) Based on the simulation results, the die shape design is further optimized and the die metal sheet design is determined.
2. The die head design method for precise extrusion molding of special-shaped rubber products according to claim 1, characterized in that: Step S.1 includes using rheological equipment to test the rheological properties and extrusion expansion law of the rubber material, and clarifying the processing window, rheological characteristic parameters, extrusion expansion rate and aspect ratio corresponding to the fully developed zone of the rubber material.
3. The die head design method for precise extrusion molding of special-shaped rubber products according to claim 1, characterized in that: In step S.2, the target shape size is converted into the metal processable shape size by computer-aided software drawing. The following principles need to be observed when drawing by computer-aided software: (1) The dimensional accuracy of the converted graphic shape and the target shape of the shaped rubber is ≥95%; (2) The cross-sectional area of the converted graphic shape and the target shape of the shaped rubber remains equal; (3) The sharp angles in the target shape of the shaped rubber need to be converted into small arcs that can be processed by metal; (4) The design of the die plate needs to take into account the parameters of the extruder and the extrusion die, including the maximum volume flow rate, pressure, flow rate and distribution of the die outlet, and pressure drop of the extruder.
4. The die head design method for precise extrusion molding of special-shaped rubber products according to claim 1, characterized in that: Step S.3 involves the design of the die geometry.
5. The die head design method for precise extrusion molding of special-shaped rubber products according to claim 4, characterized in that: The die head geometric structure is designed in a two-stage style. The die head includes two sections. The first section is the guide section, and the second section is the die section. One end of the guide section is connected to the extruder, and the other end is connected to the die section. Molding and shaping are achieved through the die section. Along the direction of fluid flow, the height of the guide section gradually decreases, and the height of the die section gradually decreases.
6. The die head design method for precise extrusion molding of special-shaped rubber products according to any one of claims 1, 4 or 5, characterized in that: Step S.3 includes decomposing the die head into multiple regions and different geometric shapes according to the metal machinable form determined in step S.2, and calculating the dies in different regions and shapes according to the design of the die head geometry to obtain the dimensions of the die head geometry.
7. The die head design method for precise extrusion molding of special-shaped rubber products according to claim 6, characterized in that: The calculation of the dimensions of the die geometry in step S.3 comprises the following steps: (1) Shear rate Calculation Determine the fluid tear strength σ of the material in the processing temperature window and calculate it according to formula 1 In formula 1, S is the cross-sectional area of the rubber extrudate, which can be determined by measuring the dimensions of the extrudate, or measured and calculated by the dimension measurement system of the capillary rheometer; F is the tensile force corresponding to the material being broken, which is given by the tensile mode test of the capillary rheometer; According to formula 2, the tensile rate corresponding to the fracture of rubber fluid is calculated In formula 2, η E It is the extensional viscosity of the rubber extrudate; To prevent fluid breakage or edge tearing during stretching or extrusion processing, the stretching rate is selected is 50% of the tensile rate corresponding to the rupture of the rubber fluid, that is, The shear rate was calculated according to Equation 3. In formula 3, Q is the volume flow rate, that is, the volume of the rubber material passing through the die per unit time, and A is the cross-sectional area of the flow channel, which is calculated from the design dimensions of the die. The length of the minor axis of the ellipse with the largest cross-sectional area is 2a, the length of the major axis is 2b, and the length of the longest diagonal of the cross section is 2c. According to the above parameters, define X = a / b ≤ 1, Y = c / b ≥ 1, then for the tube-type flow channel, X = 1 and Y = 1, for the slit-type flow channel, X = 0 and Y = 1; (2) Calculation of die size The total thickness of the die is L, the thickness of the first section is L1, the thickness of the second section is L2, the inlet angle of the first section is α, α≤45°, and the inlet angle of the second section is 2θ; the height of the flow channel outlet of the matching extrusion die is D in , the die outlet height is D out , the height D of the intersection of the two-stage lip design mid ; Given an extruder, the height D of the flow channel outlet of its matching extrusion die head in and volume flow rate Q are given; the inlet angle of the second section is 2θ as the set value; Calculate die outlet height D out , D out = height of the converted metal processable form / rubber extrusion swell ratio; According to formula (4), the shear rate of the flow channel is calculated as Calculate D mid , D mid =2a, calculate the height D of the intersection of the two-stage lip design according to equations 3 and 4 mid ; According to formula (5), L1 is calculated. L1 = (D in - D mid ) / 2tan22.5° (Equation 5) Set θ and calculate L2 according to formula (6), L2 = (D mid - D out ) / 2tanθ (Equation 6) According to formula 7, L L=L1+L2 (Formula 7). By using the above calculation method, the dimensions of dies in different regions and shapes are calculated.
8. The die head design method for precise extrusion molding of special-shaped rubber products according to claim 7, characterized in that: The fluid flow factor m is introduced for correction. The fluid flow factor m is obtained by capillary rheometer test and is used to correct formula (3). Among them, formula (8) is used to calculate the shear rate of the tube-type flow channel, and formula (9) is used to calculate the shear rate of the slit-type flow channel.
9. The die head design method for precise extrusion molding of special-shaped rubber products according to claim 1, characterized in that: In step S.4, the die plate designed based on the rheological theory calculation data is simulated and verified, and the process includes the following steps: S.4.1 Design morphology and draw using computer-aided design software; S.4.2 Meshing is performed using finite element analysis methods; S.4.3 Construction of constitutive equation: Test the viscoelastic properties of the rubber to obtain rheological characteristic parameters, relaxation time τ and zero shear viscosity η0; construct the constitutive equation through the PTT model or BKZ model, and perform multi-model fitting based on the rheological curve. PTT model constitutive equation: BKZ model constitutive equation: S.4.4 Based on the above equations, select 3 to 5 relaxation models, perform simulation calculations, and obtain pressure and velocity distribution cloud diagrams to verify the rationality of the design.
10. The die head design method for precise extrusion molding of special-shaped rubber products according to claim 1, characterized in that: In step S.5, according to step S.3 and step S.4, the die head process morphology design scheme is further optimized to determine the design scheme of the metal sheet.