Halogen-free high-frequency copper-clad plate and manufacturing method thereof

By adding fluorothiol-containing thiol-grafted polybutadiene and diamond-based flame retardant filler to the hydrocarbon resin-based copper clad plate, the problem of insufficient flame retardancy and thermal conductivity of the hydrocarbon resin-based copper clad plate is solved, and a suitable high frequency is prepared Halogen-free high-frequency copper clad plate in the field has excellent dielectric properties and heat dissipation properties.

CN118991177AActive Publication Date: 2024-11-22SHANGHAI SONG SEN SPECIAL METAL CO LTD

Patent Information

Application Number
CN202411116189.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing hydrocarbon resin-based copper clad plates are insufficient in the high-frequency field, which limits their application.

Method used

Using fluorothiol-containing thiol grafted polybutadiene, styrene-butadiene-styrene copolymer, dicyclopentadienol phenol epoxy resin and other materials, combined with diamond-based flame retardant filler and active ester curing agent, through thermal pressure Combined preparation of halogen-free high-frequency copper clad plates to improve their dielectric properties and heat dissipation properties.

Benefits of technology

It achieves low dielectric constant, excellent flame retardant performance, good heat dissipation performance and mechanical processing performance, and is suitable for electronic equipment in high-frequency fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993682460000091
    Figure BDA0004993682460000091
Patent Text Reader

Abstract

The invention discloses a halogen-free high-frequency copper-clad plate and a manufacturing method thereof, and belongs to the technical field of copper-clad plate preparation, and the manufacturing method comprises the following steps: adding fluorine-containing thiol grafted polybutadiene, a styrene-butadiene-styrene copolymer, dicyclopentadiene phenol epoxy resin, toluene, butanone and propylene glycol monomethyl ether into a mixing machine, stirring and mixing, adding a catalyst, and stirring to obtain a mixture; adding an initiator, an active ester curing agent and a diamond-based flame-retardant filler, and stirring and mixing for 2-4 hours to obtain a resin glue solution; soaking the glass cloth in the resin glue solution, taking out, and baking to obtain a prepreg; the copper-clad plate obtained by the invention has the advantages of relatively low dielectric constant, relatively good flame retardant property, relatively high heat dissipation performance, relatively low water absorption rate, good machining performance and the like; the circuit board has a wide application prospect in high-multilayer high-frequency circuit boards in the fields of communication, vehicle-mounted millimeter wave radars, Internet of Things, automotive electronics and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of copper clad laminate preparation, and in particular relates to a halogen-free high-frequency copper clad laminate and a preparation method thereof. Background Art

[0002] Copper clad laminate (CCL), also called circuit substrate, is a kind of plate formed by coating one or both sides with copper foil through a certain process flow of raw materials such as reinforcing materials, resins, fillers, and curing agents, and then hot pressing. With the advancement of electronic technology, modern communication equipment has been developing towards the 5G direction of high integration and high frequency. Copper clad laminate plays an important role as the basic material of electronic equipment and has attracted widespread attention. In order to be used at high frequencies, copper clad laminates are required to have low dielectric constants and low dielectric losses. The miniaturization and high density of electronic equipment at high frequencies lead to increased heat generation, resulting in higher requirements for the flame retardant and heat dissipation properties of copper clad laminates. With the enhancement of people's environmental awareness, halogen-free flame retardant products are more popular. Therefore, the research on low dielectric constant, high thermal conductivity halogen-free high-frequency copper clad laminates suitable for use in high-frequency fields is the current focus.

[0003] The CH in the hydrocarbon resin molecule has low polarity, and the zigzag arrangement of the molecular chain gives it excellent dielectric properties. It is one of the ideal matrix resins for high-frequency copper clad laminates. However, its flame retardancy and thermal conductivity need to be improved, which limits the application of copper clad laminates made from it in the high-frequency field. Summary of the invention

[0004] The object of the present invention is to provide a halogen-free high-frequency copper clad laminate and a manufacturing method thereof, so as to solve the problems of poor flame retardancy and thermal conductivity of existing hydrocarbon resin-based copper clad laminates.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for manufacturing a halogen-free high-frequency copper-clad laminate comprises the following steps:

[0007] S1. Add fluorinated mercaptan grafted polybutadiene, styrene-butadiene-styrene copolymer, dicyclopentadiene phenol epoxy resin, toluene, butanone, and propylene glycol monomethyl ether into a mixer, stir and mix for 30-60 minutes, then add initiator, active ester curing agent, and diamond-based flame retardant filler, stir and mix at a speed of 1500-2000 r / min for 2-4 hours to obtain a resin glue solution;

[0008] S2, immersing the glass arrangement in the resin glue solution prepared in S1 for 30-36 minutes, then taking it out, baking it in an oven at 150-160° C. for 5 minutes, and then cooling it to room temperature to obtain a prepreg;

[0009] S3. Cut the prepregs prepared in S2 into the same size, 2-8 sheets in a group, and then overlap with copper foil, and hot press for 260 minutes at a pressure of 1.8-2.5MPa and a temperature of 250-260°C to obtain a halogen-free high-frequency copper clad laminate.

[0010] Furthermore, the mass ratio of fluorinated mercaptan grafted polybutadiene, styrene-butadiene-styrene copolymer, initiator, dicyclopentadiene phenol epoxy resin, active ester curing agent, diamond-based flame retardant filler, toluene, butanone, and propylene glycol monomethyl ether in S1 is 100:50:6:30:5:50-60:80:20:10.

[0011] The diamond-based flame retardant filler is hyperbranched polyamide grafted nano-diamond, and the hyperbranched polyamide is obtained by reacting tri(3-aminophenyl)phosphine oxide and double-terminated carboxyl siloxane.

[0012] Furthermore, the preparation process of the diamond-based flame retardant filler is as follows:

[0013] Weigh tri(3-aminophenyl)phosphine oxide and double-terminated carboxyl siloxane into a flask, then add N-methylpyrrolidone, pyridine and triphenyl phosphite, stir at room temperature for 5-10 minutes, add carboxylated nanodiamond, ultrasonically disperse for 30 minutes, stir and react at room temperature for 2 hours, react at 70°C for 2 hours, and react at 130°C for 8 hours. After the reaction is completed, cool to room temperature, filter, wash the filter cake with acetone and then dry to obtain a diamond-based flame retardant filler;

[0014] The dosage ratio of tris(3-aminophenyl)phosphine oxide, double-terminated carboxyl siloxane, N-methylpyrrolidone, pyridine, triphenyl phosphite and carboxylated nanodiamond is 1.2g:1g:20-40mL:5mL:6mL:0.35-0.44g.

[0015] The invention uses tris(3-aminophenyl)phosphine oxide and double-terminated carboxyl siloxane as A3 and B2 type monomers, and in the presence of carboxylated nano-diamonds, an in-situ polymerization reaction occurs to graft hyperbranched polyamide molecules containing phosphorus and silicon elements onto the surface of the nano-diamonds, improves the dispersibility of the nano-diamonds in a resin matrix, and introduces active amino groups on the surface of the nano-diamonds, thereby improving the compatibility and interface effect between the nano-diamonds and the matrix. Under the condition of ensuring that the composite material has low dielectric loss, the composite material is endowed with excellent heat dissipation performance and flame retardancy. The heat dissipation performance mainly depends on the excellent thermal conductivity of the nano-diamonds. The flame retardancy is reflected in the synergistic flame retardancy of N, P and Si in the hyper-branched polyamide on the one hand, and in the physical barrier formed by the nano-diamond particles on the other hand, which isolates flames and flammable gases and slows down the spread of flames.

[0016] Furthermore, the dual-terminal carboxyl siloxane is obtained by hydrosilylation reaction of acrylic acid and 1,1,3,3-tetramethyldisiloxane, and the preparation process is as follows:

[0017] Weigh acrylic acid and add it into a flask, heat it to 40°C, first drop chloroplatinic acid isopropanol solution, then drop 1,1,3,3-tetramethyldisiloxane, after the dropwise addition is completed, heat to 70°C, stir and react for 2-3h, remove isopropanol and unreacted acrylic acid by vacuum distillation, and obtain double-terminal carboxyl siloxane;

[0018] The molar ratio of acrylic acid to 1,1,3,3-tetramethyldisiloxane is 2.1-2.3:1, the mass fraction of chloroplatinic acid isopropanol solution is 1%, and the amount of chloroplatinic acid isopropanol solution used is 10-20ppm of the total amount of 1,1,3,3-tetramethyldisiloxane and acrylic acid.

[0019] Further, the preparation process of carboxylated nanodiamond is as follows:

[0020] Weigh nanodiamonds and spread them evenly on the bottom of a porcelain boat. Then transfer them to a muffle furnace and oxidize them at high temperature in an air atmosphere. Set the heating rate to 5°C / min, heat the temperature from room temperature to 425°C, keep it for 1-3 hours, and then cool it to room temperature. Grind the obtained powder to obtain carboxylated diamond.

[0021] Further, the preparation process of fluorinated mercaptan grafted polybutadiene is as follows:

[0022] Weigh polybutadiene and add it to tetrahydrofuran. After magnetic stirring to dissolve, add fluorinated thiol and photoinitiator 907. React for 2 hours under nitrogen atmosphere and 365nm ultraviolet light irradiation. Then precipitate in anhydrous ethanol. The product is dried in a vacuum oven at 40°C for 24 hours to obtain fluorinated thiol-grafted polybutadiene. The mass ratio of polybutadiene, tetrahydrofuran, fluorinated thiol and photoinitiator 907 is 5:100:0.5-1.5:0.005. The number average molecular weight of polybutadiene is 2000. Through the click reaction of double bonds and thiol groups, thioether structure and fluorocarbon long chain are introduced into the molecular chain of polybutadiene, which not only gives the composite material good water resistance but also further improves its flame retardant properties.

[0023] Furthermore, the fluorine-containing thiol is a mixture of one or more of 1H,1H,2H,2H-perfluorooctanethiol, 1H,1H,2H,2H-perfluorododecanethiol and pentafluoropentanethiol.

[0024] Furthermore, the number average molecular weight of the styrene-butadiene-styrene copolymer is 7,000-30,000.

[0025] Furthermore, the active ester curing agent is a product model HPC-8000-65T active ester resin produced by DIC Corporation of Japan.

[0026] Furthermore, the initiator is composed of 2,3-dimethyl-2,3-diphenylbutane and di-tert-butyl peroxide isopropylbenzene in a mass ratio of 1:1.

[0027] Furthermore, the glass cloth is 2116 electronic grade glass fiber cloth.

[0028] A halogen-free high-frequency copper-clad laminate is prepared by the above-mentioned manufacturing method.

[0029] Beneficial effects of the present invention:

[0030] The invention uses fluorine-containing mercaptan grafted polybutadiene and styrene-butadiene-styrene copolymer as main resins, adds special epoxy resin to improve the anti-peeling performance of the copper clad laminate, adds diamond-based flame retardant filler to improve the flame retardant performance and heat dissipation performance, and then adds initiator, curing agent and solvent to prepare resin glue, so that the obtained copper clad laminate finally has the advantages of lower dielectric constant, better flame retardant performance, higher heat dissipation performance, lower water absorption rate and good mechanical processing, and has broad application prospects in high-layer and high-frequency circuit boards in the fields of communication, vehicle-mounted millimeter-wave radar, Internet of Things, automotive electronics, etc. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] This embodiment provides a diamond-based flame retardant filler, and the preparation process is as follows:

[0034] Weigh 1.2 g of tris(3-aminophenyl)phosphine oxide and 1 g of double-terminated carboxyl siloxane into a flask, then add 20 mL of N-methylpyrrolidone, 5 mL of pyridine and 6 mL of triphenyl phosphite, stir at room temperature for 5 min, add 0.35 g of carboxylated nanodiamond, ultrasonically disperse for 30 min, stir and react at room temperature for 2 h, react at 70 ° C for 2 h, and react at 130 ° C for 8 h. After the reaction is completed, cool to room temperature, filter, wash the filter cake with acetone and dry it to obtain a diamond-based flame retardant filler;

[0035] The preparation process of double-terminal carboxyl siloxane is as follows:

[0036] Weigh 2.1 mol acrylic acid into a flask, heat to 40°C, first drop 1 wt% chloroplatinic acid isopropanol solution, then drop 1 mol 1,1,3,3-tetramethyldisiloxane. After the addition is completed, heat to 70°C, stir and react for 2 hours, and remove isopropanol and unreacted acrylic acid by vacuum distillation to obtain dual-terminal carboxyl siloxane. The amount of chloroplatinic acid isopropanol solution used is 10 ppm of the total amount of 1,1,3,3-tetramethyldisiloxane and acrylic acid.

[0037] The preparation process of carboxylated nanodiamond is as follows:

[0038] Weigh nanodiamonds (purchased from Guangzhou Quanta Electromechanical Co., Ltd.) and spread them evenly on the bottom of a porcelain boat. Then transfer them to a muffle furnace and oxidize them at high temperature in an air atmosphere. Set the heating rate to 5°C / min, heat from room temperature to 425°C, keep it warm for 1h, and then cool it to room temperature. Grind the obtained powder to obtain carboxylated diamond.

[0039] Example 2

[0040] This embodiment provides a diamond-based flame retardant filler, and the preparation process is as follows:

[0041] Weigh 1.2 g of tris(3-aminophenyl)phosphine oxide and 1 g of double-terminated carboxyl siloxane into a flask, then add 40 mL of N-methylpyrrolidone, 5 mL of pyridine and 6 mL of triphenyl phosphite, stir at room temperature for 10 min, add 0.44 g of carboxylated nanodiamond, ultrasonically disperse for 30 min, stir and react at room temperature for 2 h, react at 70 ° C for 2 h, and react at 130 ° C for 8 h. After the reaction is completed, cool to room temperature, filter, wash the filter cake with acetone and dry it to obtain a diamond-based flame retardant filler;

[0042] The preparation process of double-terminal carboxyl siloxane is as follows:

[0043] Weigh 2.3 mol acrylic acid and add it into a flask. Heat it to 40°C, first drop 1 wt% chloroplatinic acid isopropanol solution, then drop 1 mol 1,1,3,3-tetramethyldisiloxane. After the addition is completed, heat to 70°C, stir and react for 3 hours, and remove isopropanol and unreacted acrylic acid by vacuum distillation to obtain dual-terminal carboxyl siloxane. The amount of chloroplatinic acid isopropanol solution used is 20 ppm of the total amount of 1,1,3,3-tetramethyldisiloxane and acrylic acid.

[0044] The preparation process of carboxylated nanodiamond is the same as that in Example 1.

[0045] Comparative Example 1

[0046] This embodiment provides a diamond-based flame retardant filler, and the preparation process is as follows:

[0047] 1.2 g of tris(3-aminophenyl)phosphine oxide and 0.55 g of adipic acid were weighed and added to a flask, followed by addition of 40 mL of N-methylpyrrolidone, 5 mL of pyridine and 6 mL of triphenyl phosphite. After stirring at room temperature for 5 min, 0.35 g of carboxylated nanodiamond was added, ultrasonically dispersed for 30 min, stirred at room temperature for 2 h, reacted at 70 ° C for 2 h, and reacted at 130 ° C for 8 h. After the reaction was completed, it was cooled to room temperature and filtered. The filter cake was washed with acetone and then dried to obtain a diamond-based flame retardant filler. The preparation process of carboxylated nanodiamond was the same as that of Example 1.

[0048] Example 3

[0049] A method for manufacturing a halogen-free high-frequency copper-clad laminate comprises the following steps:

[0050] S1, add 100g of fluorine-containing mercaptan grafted polybutadiene, 50g of styrene-butadiene-styrene copolymer, 30g of dicyclopentadiene phenol epoxy resin, 80g of toluene, 20g of butanone, and 10g of propylene glycol monomethyl ether into a mixer, stir and mix for 30min, then add 6g of initiator, 5g of active ester curing agent, and 50g of diamond-based flame retardant filler of Example 1, stir and mix at a speed of 1500r / min for 2h to obtain a resin glue;

[0051] S2, arranging 2116 electronic grade glass fiber in the resin glue prepared in S1, dipping for 30 minutes, taking it out, baking it in an oven at 150° C. for 5 minutes, and then cooling it to room temperature to obtain a prepreg;

[0052] S3. Cut the semi-cured sheets obtained in S2 into the same size, 2 sheets in a group, and then overlap with copper foil, and hot press for 260 minutes at a pressure of 1.8 MPa and a temperature of 260°C to obtain a halogen-free high-frequency copper clad laminate.

[0053] The preparation process of fluorinated mercaptan grafted polybutadiene is as follows:

[0054] Weigh 5 g of polybutadiene (number average molecular weight of 2000) and add it to 100 g of tetrahydrofuran. After dissolving under magnetic stirring, add 0.5 g of 1H,1H,2H,2H-perfluorooctanethiol and 0.005 g of photoinitiator 907. React for 2 h under nitrogen atmosphere and 365 nm ultraviolet light irradiation, then precipitate in anhydrous ethanol, and dry the product in a vacuum oven at 40 ° C for 24 h to obtain fluorine-containing thiol grafted polybutadiene.

[0055] Among them, the number average molecular weight of styrene-butadiene-styrene copolymer is 7000, the active ester curing agent is the product model HPC-8000-65T active ester resin of Japan DIC (DIC) Company, and the initiator is composed of 2,3-dimethyl-2,3-diphenylbutane and di-tert-butyl peroxide isopropylbenzene in a mass ratio of 1:1.

[0056] Example 4

[0057] A method for manufacturing a halogen-free high-frequency copper-clad laminate comprises the following steps:

[0058] S1, add 100g of fluorine-containing mercaptan grafted polybutadiene, 50g of styrene-butadiene-styrene copolymer, 30g of dicyclopentadiene phenol epoxy resin, 80g of toluene, 20g of butanone, and 10g of propylene glycol monomethyl ether into a mixer, stir and mix for 40min, then add 6g of initiator, 5g of active ester curing agent, and 55g of diamond-based flame retardant filler of Example 2, stir and mix at a speed of 1800r / min for 3h to obtain a resin glue;

[0059] S2, arranging 2116 electronic grade glass fiber in the resin glue prepared in S1, dipping for 33 minutes, taking it out, baking it in an oven at 155°C for 5 minutes, and then cooling it to room temperature to obtain a prepreg;

[0060] S3. Cut the semi-cured sheets obtained in S2 into the same size, 2 sheets in a group, and then overlap with copper foil, and hot press for 260 minutes at a pressure of 2.2 MPa and a temperature of 255°C to obtain a halogen-free high-frequency copper clad laminate.

[0061] The preparation process of fluorinated mercaptan grafted polybutadiene is as follows:

[0062] Weigh 5 g of polybutadiene (number average molecular weight of 2000) and add it to 100 g of tetrahydrofuran. After dissolving under magnetic stirring, add 1.0 g of 1H,1H,2H,2H-perfluorododecanethiol and 0.005 g of photoinitiator 907. React for 2 h under nitrogen atmosphere and 365 nm ultraviolet light irradiation, then precipitate in anhydrous ethanol, and dry the product in a vacuum oven at 40 ° C for 24 h to obtain fluorine-containing thiol grafted polybutadiene.

[0063] Among them, the number average molecular weight of styrene-butadiene-styrene copolymer is 1000, the active ester curing agent is the product model HPC-8000-65T active ester resin of Japan DIC (DIC) Company, and the initiator is composed of 2,3-dimethyl-2,3-diphenylbutane and di-tert-butyl peroxide isopropylbenzene in a mass ratio of 1:1.

[0064] Example 5

[0065] A method for manufacturing a halogen-free high-frequency copper-clad laminate comprises the following steps:

[0066] S1, add 100g of fluorine-containing mercaptan grafted polybutadiene, 50g of styrene-butadiene-styrene copolymer, 30g of dicyclopentadiene phenol epoxy resin, 80g of toluene, 20g of butanone, and 10g of propylene glycol monomethyl ether into a mixer, stir and mix for 60min, then add 6g of initiator, 5g of active ester curing agent, and 60g of diamond-based flame retardant filler of Example 2, stir and mix at a speed of 2000r / min for 4h to obtain a resin glue;

[0067] S2, arranging 2116 electronic grade glass fiber in the resin glue prepared in S1, dipping for 36 minutes, taking it out, baking it in an oven at 160° C. for 5 minutes, and then cooling it to room temperature to obtain a prepreg;

[0068] S3. Cut the semi-cured sheets obtained in S2 into the same size, 2 sheets in a group, and then overlap with copper foil, and hot press for 260 minutes at a pressure of 2.5 MPa and a temperature of 260°C to obtain a halogen-free high-frequency copper clad laminate.

[0069] The preparation process of fluorinated mercaptan grafted polybutadiene is as follows:

[0070] Weigh 5 g of polybutadiene (number average molecular weight of 2000) and add it to 100 g of tetrahydrofuran. After dissolving under magnetic stirring, add 1.5 g of 1H,1H,2H,2H-perfluorododecanethiol and 0.005 g of photoinitiator 907. React for 2 h under nitrogen atmosphere and 365 nm ultraviolet light irradiation, then precipitate in anhydrous ethanol, and dry the product in a vacuum oven at 40 ° C for 24 h to obtain fluorine-containing thiol grafted polybutadiene.

[0071] Among them, the number average molecular weight of styrene-butadiene-styrene copolymer is 30,000, the active ester curing agent is the product model HPC-8000-65T active ester resin of Japan DIC (DIC) Company, and the initiator is composed of 2,3-dimethyl-2,3-diphenylbutane and di-tert-butyl peroxide isopropylbenzene in a mass ratio of 1:1.

[0072] Comparative Example 2

[0073] A method for manufacturing a halogen-free high-frequency copper clad laminate. Compared with Example 3, the diamond-based flame retardant filler in Example 3 is replaced by the substance in Comparative Example 1, and the remaining raw materials and preparation process are the same as Example 3.

[0074] Comparative Example 3

[0075] A method for manufacturing a halogen-free high-frequency copper clad laminate. Compared with Example 3, the fluorine-containing mercaptan-grafted polybutadiene in Example 3 is replaced with polybutadiene with a number average molecular weight of 2000, and the remaining raw materials and preparation process are the same as Example 3.

[0076] The halogen-free high-frequency copper clad laminates obtained in Example 3-Example 5 and Comparative Example 2-Comparative Example 3 were tested, and the dielectric constant and dielectric loss were determined according to IPC TM-650 (2.5.5) with reference to the test method in the patent with the authorization announcement number CN116925446B. The peel strength was determined according to IPC-TM-650, version 2.4.8 of the "Copper Clad Laminate Peeling and Impact Test Method". The flame retardancy was tested according to the vertical burning method of the UL-94 standard, and the thermal conductivity was determined according to the ASTM D5470 standard. The water absorption of the copper clad laminate was tested according to IPC-TM-6502.6, and the test surface size was 50.8 mm × 50.8 mm, the test temperature was 25 ° C, the test time was 24 h, and the average of the three results was taken. The results are shown in Table 1:

[0077] Table 1

[0078]

[0079]

[0080] It can be seen from the data recorded in Table 1 that compared with Comparative Example 2 and Comparative Example 3, the copper clad laminates obtained in Example 3, Example 4, and Example 5 have better dielectric properties, anti-stripping properties, flame retardant properties, thermal conductivity and water resistance, and have broad application prospects in high-layer and high-frequency circuit boards in the fields of communications, vehicle-mounted millimeter-wave radar, Internet of Things, automotive electronics, etc.

[0081] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0082] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for manufacturing a halogen-free high-frequency copper-clad laminate, characterized in that: The following steps are involved: S1. Add fluorinated mercaptan grafted polybutadiene, styrene-butadiene-styrene copolymer, dicyclopentadiene phenol epoxy resin, toluene, butanone, and propylene glycol monomethyl ether into a mixer, stir and mix for 30-60 minutes, then add initiator, active ester curing agent, and diamond-based flame retardant filler, stir and mix for 2-4 hours to obtain a resin glue; S2, immersing the glass arrangement in the resin glue prepared in S1 for 30-36 minutes, then taking it out, baking it in an oven at 150-160° C. for 5 minutes, and then cooling it to room temperature to obtain a prepreg; S3, cutting the prepregs obtained in S2 into the same size, 2-8 sheets in a group, and then laminating them with copper foil, and hot pressing them at a pressure of 1.8-2.5MPa and a temperature of 250-260°C for 260min to obtain a halogen-free high-frequency copper clad laminate; The diamond-based flame retardant filler is hyperbranched polyamide grafted nano-diamond, and the hyperbranched polyamide is obtained by reacting tri(3-aminophenyl)phosphine oxide and double-terminated carboxyl siloxane.

2. The method for manufacturing a halogen-free high-frequency copper clad laminate according to claim 1, characterized in that: The mass ratio of fluorinated mercaptan grafted polybutadiene, styrene-butadiene-styrene copolymer, initiator, dicyclopentadiene phenol epoxy resin, active ester curing agent, diamond-based flame retardant filler, toluene, butanone, and propylene glycol monomethyl ether in S1 is 100:50:6:30:5:50-60:80:20:

10.

3. The method for manufacturing a halogen-free high-frequency copper clad laminate according to claim 1, characterized in that: The preparation process of diamond-based flame retardant filler is as follows: Weigh tri(3-aminophenyl)phosphine oxide and double-terminated carboxyl siloxane into a flask, then add N-methylpyrrolidone, pyridine and triphenyl phosphite, stir at room temperature for 5-10 minutes, add carboxylated nanodiamond, ultrasonically disperse for 30 minutes, stir and react at room temperature for 2 hours, react at 70°C for 2 hours, and react at 130°C for 8 hours. After the reaction is completed, cool to room temperature, filter, wash the filter cake with acetone and then dry to obtain a diamond-based flame retardant filler.

4. The method for manufacturing a halogen-free high-frequency copper-clad laminate according to claim 3, characterized in that: The dosage ratio of tri(3-aminophenyl)phosphine oxide, double-terminal carboxyl siloxane, N-methylpyrrolidone, pyridine, triphenyl phosphite and carboxylated nano-diamond is 1.2g:1g:20-40mL:5mL:6mL:0.35-0.44g.

5. The method for manufacturing a halogen-free high-frequency copper clad laminate according to claim 3, characterized in that: The preparation process of double-terminal carboxyl siloxane is as follows: Weigh acrylic acid and add it into a flask. Heat it to 40°C. First, add chloroplatinic acid isopropanol solution and then add 1,1,3,3-tetramethyldisiloxane. After the addition is completed, heat to 70°C and stir to react for 2-3 hours. Remove isopropanol and unreacted acrylic acid by vacuum distillation to obtain double-terminal carboxyl siloxane.

6. The method for manufacturing a halogen-free high-frequency copper-clad laminate according to claim 5, characterized in that: The molar ratio of acrylic acid to 1,1,3,3-tetramethyldisiloxane is 2.1-2.3:

1.

7. The method for manufacturing a halogen-free high-frequency copper clad laminate according to claim 1, characterized in that: The preparation process of fluorinated mercaptan grafted polybutadiene is as follows: Weigh polybutadiene and add it to tetrahydrofuran, stir magnetically to dissolve, then add fluorinated thiol and photoinitiator 907, react for 2 hours under nitrogen atmosphere and 365nm ultraviolet light, then precipitate in anhydrous ethanol, and dry the product in a vacuum oven at 40°C for 24 hours to obtain fluorinated thiol-grafted polybutadiene, the mass ratio of polybutadiene, tetrahydrofuran, fluorinated thiol and photoinitiator 907 is 5:100:0.5-1.5:0.005, and the number average molecular weight of polybutadiene is 2000.

8. The method for manufacturing a halogen-free high-frequency copper-clad laminate according to claim 7, characterized in that: The fluorine-containing mercaptan is a mixture of one or more of 1H,1H,2H,2H-perfluorooctanethiol, 1H,1H,2H,2H-perfluorododecanethiol and pentafluoropentanethiol.

9. A halogen-free high-frequency copper-clad laminate, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Thermosetting resin composition, prepreg containing same, laminated board and printed circuit board

    CN105419237A

  • High-thermal conductivity graphene oxide copper-clad plate and preparation method thereof

    CN110126391A

  • High thermal conductive composition and use thereof

    CN115651342A

  • High-frequency high-thermal-conductivity fluorine-containing resin-based copper-clad plate and preparation method thereof

    CN116554621A

  • High-Tg copper-clad plate

    CN117500151A

Cited By

  • Preparation method of modified liquid hydrocarbon polymer, resin composition and application thereof

    CN120647835A

  • A method for preparing a modified liquid hydrocarbon polymer, resin composition and use thereof

    CN120647835B