Sulfur-oxygen co-doped sodium-ion battery negative electrode material and preparation method thereof, and negative electrode plate and battery containing negative electrode material of sulfur-oxygen co-doped sodium-ion battery negative electrode material

Through sulfur and oxygen co-doping treatment, the carbon layer spacing and active sites are increased, the rate performance and capacity of sodium ion batteries are improved, and the problem of insufficient performance of existing sodium ion batteries is solved, thus achieving low cost and high efficiency Preparation of sodium ion battery negative electrode material.

CN118993019AActive Publication Date: 2024-11-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310575945.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-22
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

The existing sodium ion battery anode materials have shortcomings in terms of rate performance and capacity, and the preparation method is complex and costly, making it difficult to meet the needs of large-scale energy storage.

Method used

Using sulfur-oxygen co-doped sodium-ion battery negative electrode material, the pre-oxidation and calcination of the precursor containing sulfur elements is prepared by introducing sulfur and oxygen atoms, increasing the distance between carbon layers and forming more defects and active sites. Amorphous carbon-doped sulfur-oxygen material is used for the negative electrode of sodium ion battery.

Benefits of technology

It improves the reversible capacity and rate performance of sodium ion batteries, reduces product costs, is simple to operate, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993019A_ABST
    Figure CN118993019A_ABST
Patent Text Reader

Abstract

The invention relates to a sulfur-oxygen co-doped sodium ion battery negative electrode material and a preparation method thereof, and a negative electrode plate and a battery containing the negative electrode material, the method comprises the following steps: S1, pre-oxidizing a precursor containing a sulfur element in an air atmosphere to obtain a pre-oxidized precursor; s2, carrying out roasting treatment on the pre-oxidized precursor; the conditions of the pre-oxidation treatment in the S1 are as follows: the temperature is 150-350 DEG C, and the time is 12-48 hours; the roasting treatment conditions in the S2 are as follows: the roasting temperature is 600-900 DEG C, and the roasting time is 1-6 hours; the precursor containing the sulfur element comprises sulfonated lignin. The method disclosed by the invention is simple to operate and low in production cost, the prepared negative electrode material is amorphous carbon-doped sulfur oxygen, the reversible capacity of the battery can be effectively improved, and the battery has relatively high specific capacity at high rate of 10C (3A / g).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of negative electrode materials for sodium ion batteries, and in particular to a sulfur-oxygen co-doped negative electrode material for sodium ion batteries, a preparation method thereof, and a negative electrode sheet and a battery comprising the negative electrode material. Background Art

[0002] Compared with lithium-ion batteries, sodium-ion batteries have more abundant resources, and sodium and lithium are in the same main group, so the development cost is low. Sodium-ion batteries also have the advantages of higher capacity and better rate performance, making them more suitable for large-scale energy storage. However, the electrochemical performance of sodium-ion batteries is mainly limited by the development of electrode materials. Therefore, the rational design of the structure of electrode materials has become a research hotspot.

[0003] Carbon materials are often used as negative electrode materials for secondary batteries. Since the radius of sodium is larger than that of lithium, traditional graphite negative electrodes cannot achieve reversible sodium ion deintercalation. Therefore, finding a suitable negative electrode material for sodium ion deintercalation is the key to improving the performance of sodium ion batteries. Hard carbon materials are carbon that is difficult to graphitize. They have short-range order and long-range disordered carbon layer arrangement. The ordered carbon layer has a large interlayer spacing that can achieve reversible sodium ion deintercalation. At the same time, it has abundant nanopores and defect structures that can provide storage sites for sodium ions. In the prior art, most of the sodium ion battery negative electrode materials are prepared by combining biomass-based materials with other substances, which is complicated to operate and has high costs.

[0004] Biomass-based carbon materials have advantages such as wide sources and low prices, but they have defects such as poor rate performance and low capacity. Therefore, it is urgent to develop a simple and easy-to-operate preparation method to improve the rate performance of sodium-ion batteries. Summary of the invention

[0005] The purpose of the present disclosure is to provide a sulfur-oxygen co-doped sodium ion battery negative electrode material and a preparation method thereof, and a negative electrode plate and a battery containing the negative electrode material. The raw material components of the sodium ion battery negative electrode material are widely available and inexpensive, and can effectively reduce the cost of the product. The negative electrode material can be used in sodium ion batteries and can effectively improve the reversible capacity of the battery.

[0006] In order to achieve the above-mentioned object, the present disclosure provides a method for preparing a sulfur-oxygen co-doped sodium ion battery negative electrode material in a first aspect, the method comprising the following steps:

[0007] S1: pre-oxidizing a precursor containing sulfur element in an air atmosphere to obtain a pre-oxidized precursor;

[0008] S2: calcining the pre-oxidized precursor;

[0009] The conditions of the pre-oxidation treatment in S1 include: a temperature of 150 to 350° C. and a time of 12 to 48 hours;

[0010] The conditions for the calcination treatment in S2 include: a calcination temperature of 600 to 900° C. and a calcination time of 1 to 6 hours;

[0011] The sulfur-containing precursor includes sulfonated lignin.

[0012] Optionally, the sulfonated lignin is selected from one or more of sodium lignin sulfonate, calcium lignin sulfonate and magnesium lignin sulfonate.

[0013] Optionally, the pre-oxidation treatment conditions in S1 include: a temperature of 200 to 300° C.; and a time of 24 to 30 hours.

[0014] Optionally, the conditions for the calcination treatment in S2 include: a calcination temperature of 650 to 850° C.; a calcination time of 2 to 4 hours;

[0015] The calcination treatment is carried out under an inert atmosphere; the inert atmosphere includes one or more of nitrogen, helium and argon; the flow rate of the inert atmosphere is 50 to 300 mL / min, preferably 50 to 150 mL / min.

[0016] Optionally, the method further comprises: acid washing, water washing and drying the product after the calcination treatment in S2;

[0017] The pickling comprises mixing the product after the calcination treatment in S2 with an inorganic acid; the inorganic acid is selected from one of hydrochloric acid, sulfuric acid and acetic acid; the concentration of the inorganic acid is 1 to 12 mol / L, preferably 4 to 12 mol / L.

[0018] The second aspect of the present disclosure provides a sulfur-oxygen co-doped sodium ion battery negative electrode material prepared by the method described in the first aspect of the present disclosure.

[0019] The third aspect of the present disclosure provides a sulfur-oxygen co-doped sodium ion battery negative electrode material, wherein, based on the weight of the negative electrode material, the weight content of the sulfur element is 1-8wt%, the weight content of the oxygen element is 4-15wt%, and the weight content of the carbon element is 80-95wt%; in the Raman spectrum of the sodium ion battery negative electrode material, I D / I G The ratio is above 1.5; the carbon element exists as amorphous carbon.

[0020] Optionally, based on the weight of the negative electrode material, the weight content of the sulfur element is 5-8wt%, the weight content of the oxygen element is 5-13wt%, and the weight content of the carbon element is 82-90wt%;

[0021] In the XPS S2p spectrum of the sodium ion battery negative electrode material, characteristic peaks exist at 168-170 eV, 164-166 eV and 162-164 eV respectively;

[0022] In the XPS O1s spectrum of the sodium ion battery negative electrode material, characteristic peaks exist at 533-535 eV, 532-534 eV and 530-532 eV, respectively.

[0023] A fourth aspect of the present disclosure provides a negative electrode plate for a sodium ion battery, the negative electrode plate comprising: a current collector, a binder and the negative electrode material described in the third aspect of the present disclosure.

[0024] A fifth aspect of the present disclosure provides a sodium ion battery, comprising the negative electrode sheet according to the fourth aspect of the present disclosure, a positive electrode, an electrolyte, and a separator between the positive electrode and the negative electrode sheet;

[0025] The positive electrode is one of sodium manganate, sodium cobaltate, sodium vanadium phosphate or sodium iron phosphate.

[0026] Through the above technical scheme, the method disclosed in the present invention introduces sulfur and oxygen atoms into the negative electrode material by pre-oxidizing and calcining the biomass precursor, thereby increasing the carbon layer spacing, forming more defects and active sites, and providing more reversible storage sites for sodium ions. The method disclosed in the present invention is simple to operate, and the prepared negative electrode material is amorphous carbon doped with sulfur and oxygen, which can effectively improve the reversible capacity of the battery, improve the rate performance of the battery, and have a higher specific capacity at a high rate of 10C (3A / g).

[0027] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:

[0029] Figure 1 This is a charge and discharge curve diagram of the sodium ion battery of Example 1 of the present disclosure during the first three weeks.

[0030] Figure 2 This is the narrow spectrum of the S2p element of the XPS test of the negative electrode material prepared in Example 1 of the present disclosure.

[0031] Figure 3 This is the narrow spectrum of O1s element in XPS test of the negative electrode material prepared in Example 1 of the present disclosure.

[0032] Figure 4 This is the XRD spectrum of the negative electrode material prepared in Example 1 of the present disclosure. DETAILED DESCRIPTION

[0033] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.

[0034] The first aspect of the present disclosure provides a method for preparing a sulfur-oxygen co-doped sodium ion battery negative electrode material, the method comprising the following steps:

[0035] S1: pre-oxidizing a precursor containing sulfur element in an air atmosphere to obtain a pre-oxidized precursor;

[0036] S2: calcining the pre-oxidized precursor;

[0037] The conditions of the pre-oxidation treatment in S1 include: a temperature of 150 to 350° C. and a time of 12 to 48 hours;

[0038] The conditions for the calcination treatment in S2 include: a calcination temperature of 600 to 900° C. and a calcination time of 1 to 6 hours;

[0039] The sulfur-containing precursor includes sulfonated lignin.

[0040] The method disclosed herein introduces sulfur and oxygen atoms into the negative electrode material for co-doping, increases the distance between carbon layers, forms more defects and active sites, and thus provides more reversible storage sites for sodium ions. The method disclosed herein is simple to operate, and the prepared negative electrode material is amorphous carbon doped with sulfur and oxygen, which can effectively improve the reversible capacity of the battery, improve the rate performance of the battery, and has a higher specific capacity at a high rate of 10C (3A / g).

[0041] According to one embodiment of the present disclosure, the sulfonated lignin is selected from one or more of sodium lignin sulfonate, calcium lignin sulfonate and magnesium lignin sulfonate. The present application adopts a biomass precursor with a wide range of sources and low prices, so that the method of the present application is simple, highly operable, and has a high practical application value. At the same time, it is conducive to the prepared negative electrode material having a large number of defects, further improving the reversible capacity and rate performance of the battery.

[0042] According to an embodiment of the present disclosure, the pre-oxidation treatment conditions in S1 include: a temperature of 200 to 300°C; a time of 24 to 30 hours. The above embodiment is conducive to increasing the carbon layer spacing, and at the same time is conducive to making the oxygen content in the precursor within an appropriate range, so that the biomass precursor reaches a better oxidation degree, and further improves the reversible capacity of the battery.

[0043] According to an embodiment of the present disclosure, the conditions of the calcination treatment in S2 include: a calcination temperature of 650 to 850°C; a calcination time of 2 to 4 hours; the calcination treatment is carried out under an inert atmosphere; the inert atmosphere includes one or more of nitrogen, helium and argon; the inert atmosphere flow rate is 50 to 300 mL / min, preferably 50 to 150 mL / min. The above embodiment is conducive to the formation of a large number of defects and active sites, which is conducive to keeping the sulfur content in the negative electrode material within an appropriate range, and further improving the reversible sodium storage capacity of the battery.

[0044] According to one embodiment of the present disclosure, the product after calcination in S2 is subjected to pickling, water washing and drying; in a further embodiment, the pickling comprises mixing the product after calcination in S2 with an inorganic acid; the inorganic acid is selected from one of hydrochloric acid, sulfuric acid and acetic acid; the concentration of the inorganic acid is 1 to 12 mol / L, preferably 4 to 12 mol / L; the water washing comprises washing the product after pickling with water until the pH of the filtrate is 6.5 to 7.5, followed by filtering. The drying conditions include: the temperature can be 80 to 120°C, preferably 90 to 120°C; the time can be 20 to 26h, preferably 22 to 26h. The drying device can be a conventional drying device in the art, for example, it can be a blast drying oven. The above embodiment is conducive to removing impure metal ions in the negative electrode material.

[0045] The second aspect of the present disclosure provides a sulfur-oxygen co-doped sodium ion battery negative electrode material prepared by the method described in the first aspect of the present disclosure.

[0046] The third aspect of the present disclosure provides a sulfur-oxygen co-doped sodium ion battery negative electrode material, wherein, based on the weight of the negative electrode material, the weight content of the sulfur element is 1-8wt%, the weight content of the oxygen element is 4-15wt%, and the weight content of the carbon element is 80-95wt%; in the Raman spectrum of the sodium ion battery negative electrode material, I D / I G The ratio of is greater than 1.5; the carbon element exists as amorphous carbon. D is the intensity of the D peak, I G is the intensity of the G peak.

[0047] According to one embodiment of the present disclosure, in the XPS S2p spectrum of the sodium ion battery negative electrode material, characteristic peaks exist at 168-170eV, 164-166eV and 162-164eV, respectively, indicating the presence of thiophene-type sulfur and oxidized sulfur.

[0048] XPS O1 of the sodium-ion battery anode material SIn the spectrum, characteristic peaks exist at 533-535eV, 532-534eV and 530-532eV respectively. The characteristic peak at 530-532eV is attributed to inorganic C=O bonds, the characteristic peak at 532-534eV is attributed to organic C=O bonds, and the characteristic peak at 533-535eV is attributed to CO bonds. The CO bond content is low and the C=O bond content is high, indicating that CO gradually transforms into C=O bonds during the oxidation process, and more oxygen elements are fixed in the negative electrode material in the form of C=O.

[0049] According to an embodiment of the present disclosure, based on the weight of the negative electrode material, the weight content of the sulfur element is 5-8wt%, the weight content of the oxygen element is 5-13wt%, and the weight content of the carbon element is 82-90wt%. The above preferred implementation range is conducive to obtaining a negative electrode material with amorphous carbon having a large defect concentration, further improving the adsorption capacity of the battery, and at the same time improving the reversible sodium storage capacity and rate performance of the battery.

[0050] According to one embodiment of the present disclosure, the pre-oxidation temperature is 200-300°C, the pre-oxidation time is 24-30h; the calcination temperature is 650-850°C, the calcination time is 2-4h, and in the Raman spectrum of the sodium ion battery negative electrode material, I D / I G The above-mentioned embodiment shows that the negative electrode material of the present application has a large amount of amorphous carbon with defect concentration, which further improves the adsorption capacity of the battery and improves the reversible sodium storage capacity and rate performance of the battery.

[0051] According to one embodiment of the present disclosure, in the XRD spectrum of the sodium ion battery negative electrode material, characteristic peaks exist between 2θ of 20-25° and 40-45°, respectively, and the carbon layer spacing is 0.38-0.41 nm.

[0052] According to one embodiment of the present disclosure, in the charge and discharge curve diagram of the sodium ion battery negative electrode material, the charge and discharge curves of the sodium ion battery negative electrode material have only slopes, indicating that the negative electrode material of the present application is amorphous carbon.

[0053] A fourth aspect of the present disclosure provides a negative electrode plate for a sodium ion battery, the negative electrode plate comprising: a current collector, a binder and the negative electrode material described in the third aspect of the present disclosure.

[0054] A fifth aspect of the present disclosure provides a sodium ion battery, comprising the negative electrode sheet according to the fourth aspect of the present disclosure, a positive electrode, an electrolyte, and a separator between the positive electrode and the negative electrode sheet;

[0055] The positive electrode is one of sodium manganate, sodium cobaltate, sodium vanadium phosphate or sodium iron phosphate.

[0056] According to one embodiment of the present disclosure, the electrolyte may be a conventional electrolyte in the art, for example, the electrolyte salt may be one of sodium hexafluorophosphate, sodium perchlorate, sodium bistrifluoromethanesulfonyl imide or sodium bisfluorosulfonyl imide, and the electrolyte solvent may be one or more of ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether (DEGDME) and ethyl methyl carbonate (EMC); the diaphragm may be a conventional diaphragm in the art, for example, it may be one of a glass fiber diaphragm or a polyolefin porous membrane.

[0057] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.

[0058] In the following embodiments of the present disclosure, the X-ray scanning diffractometer (XRD) model used is an X-ray powder diffractometer produced by Philips Corporation of the United States, and the method is to use a Cu target anode Kα radiation source, a step width of 0.02°, a scanning speed of 2° / min, and 2θ=10°-80°.

[0059] Raman spectroscopy (Raman) was performed on an Advantage 532 benchtop Raman spectrometer;

[0060] XPS was performed on an instrument model Thermo Fisher Thermo ESCALAB 250;

[0061] The electrochemical performance test was carried out on a CT3001A1U-5V 5mA instrument from Wuhan Blue Electric Company;

[0062] Sodium lignin sulfonate and lignin were purchased from Beijing Innochem Technology Co., Ltd. under the brand name Innochem;

[0063] The electrolyte was a sodium ion battery electrolyte purchased from Suzhou Duoduo Reagent Co., Ltd.;

[0064] The binder is a product of Beijing Innochem Technology Co., Ltd. under the brand name Innochem;

[0065] The raw materials and reagents used in the following examples and comparative examples are all battery grade;

[0066] Unless otherwise specified, the chemical reagents used in the following examples and comparative examples are commercially available products.

[0067] Example 1

[0068] (1) 10 g of sodium lignin sulfonate was evenly placed in a corundum ark, placed in a muffle furnace, and pre-oxidized at 250° C. for 24 h in an air atmosphere to obtain a pre-oxidized precursor, which was recorded as LNa250.

[0069] (2) The above-mentioned pre-oxidized precursor was evenly placed in a corundum ark, placed in a tube furnace, introduced with nitrogen, and calcined at 800°C for 2h to obtain an amorphous carbon material co-doped with sulfur and oxygen, which was recorded as LNa250-800.

[0070] (3) Preparation of negative electrode sheets for sodium ion batteries. Weigh the above-mentioned negative electrode material for sodium ion batteries and 20% sodium alginate binder according to a mass ratio of 9:1, stir under magnetic stirring for 6 hours, allow the negative electrode material for sodium ion batteries and the sodium alginate binder to be fully mixed, and then apply them on copper foil with a scraper, with a scraper thickness of 150μm. Dry the coated copper foil in a blast drying oven at 80°C for 12 hours, then use a sheet puncher to punch the coated copper foil into electrode sheets with a diameter of 12mm, and select the electrode sheets with uniform coating and similar mass by microbalance to obtain the negative electrode for sodium ion batteries. The sodium alginate binder is prepared by first placing sodium alginate powder in a 25*25mm weighing bottle, adding an appropriate amount of deionized water, and stirring the sodium alginate and deionized water into a uniform gel solution under magnetic stirring.

[0071] (4) Assembly of sodium ion half-cell. Metallic sodium was used as the counter electrode, 1 mol / L NaPF6-DEGDME was used as the electrolyte, the above-mentioned sodium ion negative electrode sheet was used as the working electrode, and the battery separator was Whatman GF / D glass fiber separator. A CR2032 experimental button symmetrical battery was assembled in a glove box filled with argon atmosphere to evaluate the electrochemical performance of the above-mentioned sodium ion battery negative electrode material.

[0072] Example 2

[0073] (1) Take 10g of sodium lignin sulfonate and place it evenly in a corundum ark, put it in a muffle furnace, and pre-oxidize it at 200°C for 24h under air atmosphere to obtain a pre-oxidized precursor, which is recorded as LNa200.

[0074] (2) The above-mentioned pre-oxidized precursor was evenly placed in a corundum ark, placed in a tube furnace, introduced with nitrogen, and calcined at 800° C. for 2 h to obtain an amorphous carbon material co-doped with sulfur and oxygen, which was recorded as LNa200-800.

[0075] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0076] Example 3

[0077] (1) 10 g of sodium lignin sulfonate was evenly placed in a corundum ark, placed in a muffle furnace, and pre-oxidized at 300° C. for 24 h in an air atmosphere to obtain a pre-oxidized precursor, which was recorded as LNa300.

[0078] (2) The above-mentioned pre-oxidized precursor was evenly placed in a corundum ark, placed in a tube furnace, introduced with nitrogen, and calcined at 800° C. for 2 h to obtain an amorphous carbon material co-doped with sulfur and oxygen, which was recorded as LNa300-800.

[0079] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0080] Example 4

[0081] (1) 10 g of sodium lignin sulfonate was evenly placed in a corundum ark, placed in a muffle furnace, and pre-oxidized at 250° C. for 36 h in an air atmosphere to obtain a pre-oxidized precursor.

[0082] (2) The above-mentioned pre-oxidized precursor is evenly placed in a corundum ark, placed in a tube furnace, introduced with nitrogen, and calcined at 800° C. for 2 h to obtain an amorphous carbon material co-doped with sulfur and oxygen.

[0083] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0084] Example 5

[0085] (1) 10 g of sodium lignin sulfonate was evenly placed in a corundum ark, placed in a muffle furnace, and pre-oxidized at 150° C. for 24 h in an air atmosphere to obtain a pre-oxidized precursor, which was recorded as LNa150.

[0086] (2) The above-mentioned pre-oxidized precursor was evenly placed in a corundum ark, placed in a tube furnace, introduced with nitrogen, and calcined at 800°C for 2h to obtain an amorphous carbon material co-doped with sulfur and oxygen, which was recorded as LNa150-800.

[0087] Example 6

[0088] (1) 10 g of sodium lignin sulfonate was evenly placed in a corundum ark, placed in a muffle furnace, and pre-oxidized at 250° C. for 24 h in an air atmosphere to obtain a pre-oxidized precursor.

[0089] (2) The above-mentioned pre-oxidized precursor is evenly placed in a corundum ark, placed in a tube furnace, introduced with nitrogen, and calcined at 900° C. for 2 h to obtain an amorphous carbon material co-doped with sulfur and oxygen.

[0090] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0091] Example 7

[0092] (1) 10 g of sodium lignin sulfonate was evenly placed in a corundum ark, placed in a muffle furnace, and pre-oxidized at 250° C. for 24 h in an air atmosphere to obtain a pre-oxidized precursor.

[0093] (2) The above-mentioned pre-oxidized precursor is evenly placed in a corundum ark, placed in a tube furnace, introduced with nitrogen, and calcined at 800° C. for 5 h to obtain an amorphous carbon material co-doped with sulfur and oxygen.

[0094] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0095] Comparative Example 1

[0096] (1) 10 g of lignin was evenly placed in a corundum ark, placed in a muffle furnace, and pre-oxidized at 250 °C for 24 h in an air atmosphere to obtain a pre-oxidized precursor, which was recorded as L250.

[0097] (2) The above pre-oxidized precursor was evenly placed in a corundum ark, placed in a tube furnace, introduced with nitrogen, and calcined at 800° C. for 2 h to obtain an amorphous carbon material, which was recorded as L250-800.

[0098] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0099] Comparative Example 2

[0100] (1) 10 g of lignin was evenly placed in a corundum ark, placed in a tubular furnace, and after nitrogen was introduced, a segmented calcination program was set up, calcined at 250 °C for 24 h, then the temperature was raised to 800 °C and calcined for another 2 h to obtain an amorphous carbon material, recorded as D250-800.

[0101] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0102] Comparative Example 3

[0103] (1) 10 g of sodium lignin sulfonate was evenly placed in a corundum ark, placed in a tubular furnace, and after nitrogen was introduced, a segmented calcination program was set up, calcined at a temperature of 250 ° C for 24 h, and then the temperature was raised to 800 ° C and calcined for another 2 h to obtain an amorphous carbon material, recorded as DNa250-800.

[0104] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0105] Comparative Example 4

[0106] (1) Take 10 g of lignin and 5 g of thiourea, evenly place them in a corundum ark, put them in a muffle furnace, and pre-oxidize them at 250 °C for 24 h in an air atmosphere to obtain a pre-oxidized precursor, which is recorded as LNa250.

[0107] (2) The above-mentioned pre-oxidized precursor is evenly placed in a corundum ark, placed in a tube furnace, introduced with nitrogen, and calcined at 800° C. for 2 h to obtain an amorphous carbon material.

[0108] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0109] Comparative Example 5

[0110] (1) 10 g of sodium lignin sulfonate was evenly placed in a corundum ark, placed in a muffle furnace, and pre-oxidized at 100 °C for 24 h in an air atmosphere to obtain a pre-oxidized precursor, which was recorded as LNa100.

[0111] (2) The above-mentioned pre-oxidized precursor was evenly placed in a corundum ark, placed in a tube furnace, introduced with nitrogen, and calcined at 800° C. for 2 h to obtain an amorphous carbon material, which was recorded as LNa100-800.

[0112] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0113] Comparative Example 6

[0114] (1) 10 g of sodium lignin sulfonate was evenly placed in a corundum ark, placed in a tubular furnace, introduced with nitrogen, and calcined at 800 °C for 2 h to obtain an amorphous carbon material.

[0115] The preparation of the negative electrode sheet of the sodium ion battery and the assembly of the sodium ion half-cell are the same as in Example 1.

[0116] Test Example 1

[0117] XPS, elemental analysis and Raman spectroscopy were performed on the negative electrode materials obtained in Examples 1 to 7 and Comparative Examples 1 to 6. The results are shown in Table 1.

[0118] Table 1

[0119] Carbon content (wt%) Sulfur content (wt%) Oxygen content (wt%) <![CDATA[I D / I G ]]> Example 1 83.96 6.62 9.42 2.65 Example 2 82.48 5.28 12.24 1.71 Example 3 85.63 5.23 9.14 1.85 Example 4 84.45 1.02 14.53 1.95 Example 5 94.21 1.17 4.62 1.57 Example 6 89.25 3.37 9.38 1.89 Example 7 92.28 3.35 6.37 1.51 Comparative Example 1 92.54 0.23 7.23 1.75 Comparative Example 2 99.43 0.08 0.49 1.08 Comparative Example 3 98.56 1.12 0.32 1.62 Comparative Example 4 90.2 2.02 7.78 1.92 Comparative Example 5 89.92 1.25 8.83 1.76 Comparative Example 6 93.12 0.51 6.37 1.05

[0120] According to the data in Table 1, the weight content of oxygen in the negative electrode material prepared by the method of the present invention is between 4 and 15wt%, the weight content of sulfur is between 1 and 8wt%, and the weight content of carbon is 80 to 95wt%. By comparing Example 1 with Example 4, it can be seen that within the preferred pre-oxidation time range of the present invention, the oxygen content of the obtained negative electrode material is between 5 and 13wt%, and the rate performance of the obtained negative electrode material is better. By comparing Example 1 with Example 5, it can be seen that within the preferred pre-oxidation temperature range of the present invention, the oxygen content of the obtained negative electrode material is between 5 and 13wt%, and the rate performance of the obtained negative electrode material is better. By comparing Example 1 with Example 6, it can be seen that within the preferred calcination temperature range of the present invention, the sulfur content of the obtained negative electrode material is between 5 and 8wt%, and the rate performance of the obtained negative electrode material is better. By comparing Example 1 with Example 7, it can be seen that within the preferred calcination time range of the present invention, the sulfur content of the obtained negative electrode material is between 5 and 8wt%, and the rate performance of the obtained negative electrode material is better.

[0121] Test Example 2

[0122] The electrochemical performance of the battery cells of Examples 1 to 7 and Comparative Examples 1 to 6 was tested under the following conditions: -1 ) rate, the cut-off voltage range is 0.01V~3V, and the constant current charge and discharge are performed. The test results are shown in Table 2.

[0123] Table 2

[0124]

[0125]

[0126] According to the data in Table 3, the preparation method disclosed in the present invention is simple, highly operable, and has low production cost. The negative electrode material prepared by the method disclosed in the present invention has a high first discharge specific capacity, a high first-week coulombic efficiency, and a high specific capacity at 10C. By comparing Example 1 with Example 4, it can be seen that within the preferred pre-oxidation time range of the present invention, the rate performance of the obtained negative electrode material is better. By comparing Example 1 with Example 5, it can be seen that within the preferred pre-oxidation temperature range of the present invention, the rate performance of the obtained negative electrode material is better. By comparing Example 1 with Example 6, it can be seen that within the preferred calcination temperature range of the present invention, the rate performance of the obtained negative electrode material is better. By comparing Example 1 with Example 7, it can be seen that within the preferred calcination time range of the present invention, the rate performance of the obtained negative electrode material is better.

[0127] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0128] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0129] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A method for preparing sulfur-oxygen co-doped sodium ion battery negative electrode material, characterized in that: The method comprises the following steps: S1: pre-oxidizing a precursor containing sulfur element in an air atmosphere to obtain a pre-oxidized precursor; S2: calcining the pre-oxidized precursor; The conditions of the pre-oxidation treatment in S1 include: a temperature of 150 to 350° C. and a time of 12 to 48 hours; The conditions for the calcination treatment in S2 include: a calcination temperature of 600 to 900° C. and a calcination time of 1 to 6 hours; The sulfur-containing precursor includes sulfonated lignin.

2. The method according to claim 1, wherein: The sulfonated lignin is selected from one or more of sodium lignin sulfonate, calcium lignin sulfonate and magnesium lignin sulfonate.

3. The method according to claim 1, wherein: The conditions of the pre-oxidation treatment in S1 include: a temperature of 200 to 300° C.; and a time of 24 to 30 hours.

4. The method according to claim 1, wherein: The conditions of the calcination treatment in S2 include: a calcination temperature of 650 to 850°C; a calcination time of 2 to 4 hours; The calcination treatment is carried out under an inert atmosphere; the inert atmosphere includes one or more of nitrogen, helium and argon; the flow rate of the inert atmosphere is 50 to 300 mL / min, preferably 50 to 150 mL / min.

5. The method according to claim 1, wherein: The method further comprises: acid washing, water washing and drying the product after the calcination treatment in S2; The pickling comprises mixing the product after the roasting treatment in S2 with an inorganic acid; the inorganic acid is selected from one of hydrochloric acid, sulfuric acid and acetic acid; the concentration of the inorganic acid is 1 to 12 mol / L, preferably 4 to 12 mol / L.

6. Sulfur-oxygen co-doped sodium ion battery negative electrode material prepared by the method according to any one of claims 1 to 5.

7. A sulfur-oxygen co-doped sodium ion battery negative electrode material, characterized in that: Based on the weight of the negative electrode material, the weight content of the sulfur element is 1-8wt%, the weight content of the oxygen element is 4-15wt%, and the weight content of the carbon element is 80-95wt%; In the Raman spectrum of the sodium ion battery negative electrode material, I D / I G The ratio is above 1.5; the carbon element exists as amorphous carbon.

8. The negative electrode material for sodium ion batteries according to claim 7, wherein: Based on the weight of the negative electrode material, the weight content of the sulfur element is 5-8wt%, the weight content of the oxygen element is 5-13wt%, and the weight content of the carbon element is 82-90wt%; In the XPS S2p spectrum of the sodium ion battery negative electrode material, characteristic peaks exist at 168-170 eV, 164-166 eV and 162-164 eV respectively; In the XPS O1s spectrum of the sodium ion battery negative electrode material, characteristic peaks exist at 533-535 eV, 532-534 eV and 530-532 eV, respectively.

9. A negative electrode plate for a sodium ion battery, characterized in that: The negative electrode sheet comprises: a current collector, a binder and the battery negative electrode material according to any one of claims 6 to 8.

10. A sodium ion battery, characterized in that: The invention comprises the negative electrode sheet according to claim 9, a positive electrode, an electrolyte and a separator between the positive electrode and the negative electrode sheet; The positive electrode is one of sodium manganate, sodium cobaltate, sodium vanadium phosphate or sodium iron phosphate.

Citation Information

Patent Citations

  • Preparation method of porous hollow carbon microsphere co-doped with oxygen and nitrogen

    CN108511204A

  • Sulfur / nitrogen / silicon co-doped graphite composite negative electrode material and preparation method thereof

    CN109659546A

  • Negative electrode composite material for zinc secondary battery as well as preparation method and application of negative electrode composite material

    CN115548316A

  • Preparation method of nitrogen-phosphorus co-doped carbon-coated modified silicon monoxide negative electrode material

    CN115832263A

  • Cluster-shaped nitrogen-sulfur-oxygen co-doped sodium ion battery negative electrode material and preparation method thereof

    CN115849342A