Artificial graphite material as well as preparation method and application thereof

Through pretreatment, boron doping and nitrogen doping steps, the problem of insufficient electrochemical performance of needle-shaped coke in the battery is solved, and the first Coulomb efficiency, capacity and rate performance of the battery is improved, achieving a more efficient electrochemical reaction.

CN118993055AInactive Publication Date: 2024-11-22福建龙净储能电池有限公司

Patent Information

Application Number
CN202411084794.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

As an artificial graphite negative electrode material, needle coke is prone to irreversible reaction with the electrolyte, reduced charge and discharge efficiency, and insufficient electrochemical performance, resulting in its consumption of a large amount of positive electrode material in industrial production, increasing costs.

Method used

Through three steps of pretreatment, boron doping and nitrogen doping, the repulsion between lithium ions and embedded lithium ions is reduced, the active sites of the material are increased, and the first-time Coulomb efficiency, capacity and rate performance of the battery is improved.

Benefits of technology

It improves the electrochemical performance of artificial graphite materials, enhances the first-time Coulomb efficiency, capacity and rate performance of the battery, reduces the migration resistance of lithium ions, and improves the stability and reversible specific capacity of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004984866490000151
    Figure BDA0004984866490000151
  • Figure BDA0004984866490000161
    Figure BDA0004984866490000161
Patent Text Reader

Abstract

The invention provides an artificial graphite material and a preparation method and application thereof, the preparation method comprises the following steps: mixing a graphite material precursor with a binder for pretreatment to obtain a pretreated product; carrying out boron doping and graphitization on the pretreated product to obtain a boron-doped product; and carrying out nitrogen doping on the boron-doped product to obtain the artificial graphite material. According to the preparation method disclosed by the invention, through cooperation of the three steps of pretreatment, boron doping and nitrogen doping, the repulsive force between lithium ions and embedded lithium ions is reduced, and active sites and the like in the material are also increased, so that the obtained artificial graphite material can improve the first coulombic efficiency, the capacity and the rate capability of a battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to an artificial graphite material and a preparation method and application thereof. Background Art

[0002] Artificial graphite materials are prepared from petroleum coke or pitch coke raw materials through processes such as crushing, high-temperature graphitization, and screening. Therefore, the performance of artificial graphite materials is directly related to the selected coke raw materials and preparation methods. Artificial graphite coke raw materials are mainly divided into two categories: needle coke and petroleum coke. Ordinary petroleum coke raw materials are abundant and low in cost, but they have problems such as high sulfur, high ash content, and disordered microcrystalline structure, and cannot be used in lithium battery negative electrode materials. At present, although ordinary low-sulfur petroleum coke can be used to prepare lithium battery negative electrode materials, because the petroleum coke raw materials have not been passivated and lack the control process of intermediate phase growth, its microcrystalline structure is disordered, the anisotropic structure content is low, and the degree of graphitization is low. The electrochemical performance of negative electrode materials needs to be improved. Needle coke has the advantages of low sulfur, low ash content, and low metal content in graphite negative electrode materials. At the same time, it also has a good anisotropic microcrystalline structure, which is highly ordered and easier to graphitize. Therefore, it can be used as the main raw material for the production of high-end artificial stone black.

[0003] For example, CN 117638032A discloses a composite graphite negative electrode material for lithium-ion power batteries, a preparation method thereof, and a lithium-ion power battery. The composite graphite negative electrode material for lithium-ion power batteries includes a negative electrode sheet and a negative electrode active layer, and the negative electrode active layer includes the following mass components: 60 to 75 parts of needle coke; 10 to 20 parts of modified coke balls; 10 to 20 parts of single crystal silicon powder; and 1 to 10 parts of a binder. The added needle coke, single crystal silicon powder, and binder in the composite graphite negative electrode material for lithium-ion power batteries can form a multi-channel three-dimensional woven mesh structure with a relatively suitable strength, so that the added modified coke balls can be well filled in the pores of the multi-channel three-dimensional woven mesh structure with a relatively suitable strength, forming a conductive mesh with more channels and suitable strength.

[0004] For example, CN 117800330A discloses a method for preparing an artificial graphite negative electrode material, comprising the following steps: ① crushing a needle coke raw material, ball milling and screening, and obtaining a needle coke material with a D50 of 1.0 to 3.0 μm; ② uniformly mixing the needle coke material with a binder, adding a modified few-layer graphene conductive slurry, heating and kneading, and pressing into a block to obtain a molded body; ③ heating the molded body to 900 to 1200° C. at a rate of 1 to 5° C. / min, and carbonizing for 9 to 15 h to obtain a carbonized product; ④ treating the carbonized product at 2600 to 2900° C. for 20 to 40 h to obtain a graphitized product; ⑤ grinding and screening the graphitized product to remove large particles to obtain an artificial graphite negative electrode material, wherein the prepared artificial graphite negative electrode material has a small internal resistance and excellent conductivity.

[0005] For example, CN 115249796A discloses a graphite-nitrogen-doped carbon composite negative electrode material and a preparation method thereof, comprising the following steps: (1) granulating, graphitizing, demagnetizing and sieving needle coke that has been ground and spheroidized and high-temperature asphalt that has been ground in sequence to obtain artificial graphite; (2) using urea as a nitrogen source and acrylic acid and glucose as hard carbon materials, the artificial graphite prepared in step (1) is dispersed in a mixed solution of urea, acrylic acid and glucose, and then heated, stirred, dried, carbonized, ball-milled, dispersed, demagnetized and sieving to obtain a graphite-nitrogen-doped carbon composite negative electrode material.

[0006] However, needle coke as an artificial graphite negative electrode material still has some disadvantages, such as the irreversible reaction with the electrolyte that causes the reduction of charge and discharge efficiency, the reduction of battery reversible capacity due to solvent co-embedding, and poor cycle performance, which have become bottlenecks hindering its further development. In addition, due to the unique streamlined fiber structure of needle coke, its orientation degree in various directions is different. The primary particle negative electrode material prepared by needle coke alone still has certain defects in electrochemical performance, with general rate performance and low first coulomb efficiency. In industrial production, it will lead to a large consumption of positive electrode materials, thereby increasing costs.

[0007] Based on the above research, it is necessary to provide a method for preparing an artificial graphite material, and the artificial graphite material obtained by the preparation method can improve the first coulombic efficiency, capacity and rate performance of the battery. Summary of the invention

[0008] The object of the present invention is to provide an artificial graphite material and a preparation method and application thereof. The preparation method reduces the repulsive force between lithium ions and embedded lithium ions and increases the active sites in the material through the coordination of three steps of pretreatment, boron doping and nitrogen doping, so that the obtained artificial graphite material can improve the first coulombic efficiency, capacity and rate performance of the battery.

[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a method for preparing an artificial graphite material, the preparation method comprising the following steps:

[0011] (1) mixing a graphite material precursor with a binder for pretreatment to obtain a pretreated product;

[0012] (2) boron-doping and graphitizing the pretreated product of step (1) to obtain a boron-doped product;

[0013] (3) Nitrogen-doping the boron-doped product of step (2) to obtain the artificial graphite material.

[0014] The present invention comprises the steps of pretreatment, boron doping and nitrogen doping. The pretreatment can realize one-time granulation, and then boron doping is performed, so that boron atoms can enter the lattice of graphite microcrystals to replace a part of carbon positions. Because boron atoms have an electron-deficient effect, the repulsive force between lithium ions and embedded lithium ions can be reduced by boron doping, thereby increasing the lithium insertion capacity and further improving the electrical properties of graphite. In addition, the boron element doping process is promoted to the coking process instead of boron doping after graphitization, so that doped needle coke can be obtained, and the prepared element doping can be made more uniform. Finally, the present invention can further improve the capacity and rate performance of the material by nitrogen doping, because N atoms are close in size to C atoms and have smaller electronegativity, and doping N atoms in graphite can increase active sites, improve the reversible specific capacity and large current charge and discharge performance of the material, and the incorporation of N atoms can reduce the migration resistance of lithium ions, so the first coulomb efficiency, capacity and rate performance of the battery can be improved.

[0015] In the present invention, boron doping and nitrogen doping are carried out in steps, and boron doping is carried out before graphitization, and nitrogen doping is carried out after graphitization. If boron and nitrogen are doped together in one step, although the one-step doping manufacturing process is simple, the doping effect and the substitution site of doping are difficult to control. Since the doping of B is difficult, the present invention modifies the graphite by first doping B to construct more active sites and defects. During the subsequent N doping, N atoms can more easily replace carbon atoms, thereby making the uniformity of the doping of the two elements better, and the electronic synergy of B and C is more fully exerted, thereby improving the material performance and making the material have better stability and electrochemical performance.

[0016] Preferably, the graphite material precursor in step (1) comprises calcined coal-based needle coke.

[0017] Preferably, the graphite material precursor in step (1) is first crushed and then mixed with the binder.

[0018] Preferably, the particle size D50 of the pulverized graphite material precursor is 4-8 μm, for example, 4 μm, 5 μm, 6 μm, 7 μm or 8 μm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] Preferably, the amount of the binder added in step (1) is 6-8wt% of the mass of the graphite material precursor, for example, it can be 6wt%, 7wt% or 8wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the binder in step (1) comprises coal tar pitch.

[0021] Preferably, the mixing time in step (1) is 1-2h, for example, 1h, 1.5h or 2h, the rotation speed is 300-500r / min, for example, 300r / min, 400r / min or 500r / min, and the frequency is 60-80Hz, for example, 60Hz, 70Hz or 80Hz, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0022] Preferably, the boron doping in step (2) comprises stirring and mixing the boron source and the pre-treated product in step (1).

[0023] Preferably, the mass ratio of the pretreated product to the boron source in step (1) is (10-30):1, for example, 10:1, 20:1 or 30:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] The mass ratio of the pretreatment product and the boron source described in the present invention reflects the amount of boron doping. If the amount of boron doping is too little, the boron doping effect decreases. If the boron doping is too much, since B has three valence electrons, it can act as an electron acceptor to promote the charge transfer between the carbon atoms adjacent to it. B doping is generally accompanied by the introduction of part of O to form BC3, BCO2, BC2O and other substances. If the boron doping is too much, firstly, the doping difficulty of B is greater than that of N doping, and excessive doping is difficult to implement and the cost is high. Secondly, excessive substitution will lead to a large change in the material structure, poor stability, and easy side reactions, which is not conducive to improving the long cycle life of the material.

[0025] Preferably, the stirring and mixing is carried out at a rotation speed of 300-400 r / min, such as 300 r / min, 350 r / min or 400 r / min, for 50-60 min, such as 50 min, 55 min or 60 min, and is carried out under protective gas.

[0026] Preferably, the boron source includes any one of boric acid, boron oxide, boron carbide or boron trioxide, or a combination of at least two thereof.

[0027] Preferably, a secondary granulation step is performed between the boron doping and graphitization in step (2).

[0028] The secondary granulation process of the present invention can enrich Li + The number of embedding and de-embedding channels in the lattice increases the isotropy of the negative electrode material and improves the battery's first coulombic efficiency and rate performance.

[0029] Preferably, the secondary granulation step comprises heat treating the boron-doped material under stirring.

[0030] Preferably, the heat treatment comprises heating to 250-450°C, for example 250°C, 350°C or 450°C, at a speed of 2-3°C / min, for example 2°C / min, 2.5°C / min or 3°C / min, stirring at a speed of 200-300r / min, for example 200r / min, 250r / min or 300r / min, stirring at a constant temperature for 2-3h, for example 2h, 2.5h or 3h, and then heating to 600-700°C, for example 600°C, 650°C or 700°C, at a heating rate of 2-3°C / min, for example 2°C / min, 2.5°C / min or 3°C / min, and keeping the temperature constant for 3-7h, for example 3h, 4h, 5h, 6h or 7h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] Preferably, the graphitization temperature in step (2) is 2600-3100°C, for example, 2600°C, 2800°C, 3000°C or 3100°C, and the time is 60-100h, for example, 60h, 80h or 100h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] Preferably, after the graphitization in step (2) and before the nitrogen doping in step (3), the method further includes mixing, screening and demagnetization steps.

[0033] Preferably, the mixing rate is 5-20 r / min, for example, 5 r / min, 10 r / min, 15 r / min or 20 r / min, and the mixing time is 80-120 min, for example, 80 min, 100 min or 120 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the mesh size of the sieve used for the screening is 400-500 mesh, for example, 400 mesh, 450 mesh or 500 mesh, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, the nitrogen doping in step (3) comprises mixing and calcining a nitrogen source and the boron doping product in step (2).

[0036] Preferably, the mass ratio of the boron-doped product to the nitrogen source in step (2) is 1:(20-30), for example, 1:20, 1:25 or 1:30, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] The mass ratio of the boron-doped product and the nitrogen source described in the present invention can reflect the amount of nitrogen doping. If the amount of nitrogen doping is too little, the effect of nitrogen doping cannot be effectively exerted. Since the radius of nitrogen atoms and carbon atoms is similar, but the electronegativity of nitrogen is 3.04 and the electronegativity of carbon is 2.55, theoretically, C / nitrogen atoms are replaced one-to-one. After the substitution, vacancies and dangling bonds can be formed around N, and SP2 hybridization will also produce polarization to enhance the electron and ion conduction rates. However, when nitrogen atoms are doped too much, the doping is difficult and costly, and excessive doping will result in excessive substitution, resulting in poor material stability, which is particularly unfavorable for long cycle life. At the same time, if the nitrogen doping amount is too much, too many active sites are introduced, which will cause more active lithium to be consumed during the first SEI generation, increase the irreversible capacity, and cause a low first effect.

[0038] Preferably, the rate of mixing the nitrogen source and the boron-doped product of step (2) is 300-400 r / min, for example, 300 r / min, 350 r / min or 400 r / min, and the time is 30-50 min, for example, 30 min, 40 min or 50 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] Preferably, the calcination temperature is 700-1000°C, for example, 700°C, 800°C, 900°C or 1000°C, and the calcination time is 3-6h, for example, 3h, 4h, 5h or 6h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, the nitrogen source includes any one of aniline, ethylenediamine, melamine or polyimide, or a combination of at least two of them.

[0041] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps:

[0042] (1) pulverizing the calcined coal-based needle coke to a particle size D50 of 4-8 μm, and then mixing the pulverized material with a binder at a speed of 300-500 r / min and a frequency of 60-80 Hz for 1-2 hours to obtain a pretreated product, wherein the amount of the binder added is 6-8 wt% of the mass of the graphite material precursor;

[0043] (2) Mix the pretreated product of step (1) and the boron source at a mass ratio of (10-30):1 under protective gas at a stirring rate of 300-400r / min for 50-60min, then heat to 250-450°C at a rate of 2-3°C / min, stir at a constant temperature for 2-3h at a stirring rate of 200-300r / min, then heat to 600-700°C at a heating rate of 2-3°C / min, and keep the temperature constant for 3-7h. Then heat to 2600-3100°C at a heating rate of 5-10°C / min, graphitize for 60-100h, and then mix the graphitized product at a rate of 5-20r / min for 80-120min, sieve and demagnetize to obtain a boron-doped product;

[0044] (3) mixing the nitrogen source and the boron-doped product of step (2) at a rate of 300-400 r / min for 30-50 min, and then calcining at a temperature of 700-1000° C. for 3-6 h for nitrogen doping to obtain the artificial graphite material.

[0045] In a second aspect, the present invention provides an artificial graphite material, which is prepared by the preparation method described in the first aspect.

[0046] In a third aspect, the present invention provides a negative electrode plate, wherein the negative electrode plate comprises the artificial graphite material as described in the second aspect.

[0047] In a fourth aspect, the present invention provides a battery, comprising the negative electrode plate as described in the third aspect.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] The present invention can improve various properties of artificial graphite materials through the combination of pretreatment, boron doping secondary granulation and nitrogen doping. Among them, the secondary granulation process can enrich Li +The number of channels for embedding and de-embedding in the lattice increases the isotropy of the negative electrode material and improves the first coulomb efficiency and rate performance of the battery; boron atoms can enter the lattice of graphite microcrystals and replace part of the carbon position. Because boron atoms have an electron-deficient effect, boron doping can reduce the repulsion between lithium ions and embedded lithium ions, thereby increasing the lithium insertion capacity and further improving the electrical properties of graphite. In addition, the boron element doping process is promoted to the coking process to obtain doped needle coke, which can make the prepared element doping more uniform. At the same time, nitrogen doping can further improve the capacity and rate performance of the material, because N atoms are close in size to C atoms and have a smaller electronegativity. Doping N atoms in graphite can increase active sites, improve the reversible specific capacity and high current charge and discharge performance of the material, and the incorporation of N atoms can reduce the migration resistance of lithium ions; in summary, the present invention can improve the first coulomb efficiency, capacity and rate performance of the battery. DETAILED DESCRIPTION

[0050] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0051] Example 1

[0052] This embodiment provides a method for preparing an artificial graphite material, the preparation method comprising the following steps:

[0053] (1) Pretreatment

[0054] The calcined coal-based needle coke was ground to a D50 of 5 μm using a jet mill, 500 g of the ground material was added with 7 wt % of coal tar as a binder, and stirred in a VC mixer at 350 r / min and a frequency of 65 Hz for 1.5 h to obtain material A;

[0055] (2) Boron doping secondary granulation

[0056] Mixing: placing material A and boric acid in a mass ratio of 12:1 in a reaction kettle, stirring at 330 r / min for 55 min under argon gas protection and room temperature to obtain a mixed material;

[0057] Granulation: The mixed material was heated from room temperature to 250°C at a rate of 2°C / min, and stirred at a constant temperature for 2 hours at a stirring speed of 220r / min; then the temperature was raised to 650°C at a heating rate of 2°C / min, and kept at a constant temperature for 3.5 hours to obtain the granulated material;

[0058] Graphitization: The granulated material is placed in a graphitization furnace, heated to 2800°C at a heating rate of 5°C / min, and graphitized for 65 hours. The graphitized material is mixed (at a rate of 8r / min, for 80 minutes), sieved (using a 400-mesh screen) and demagnetized to obtain a boron-doped secondary granulated negative electrode material;

[0059] (3) Nitrogen doping

[0060] Mixing: Place the boron-doped secondary granulated negative electrode material and melamine in a mass ratio of 1:23 in a stirred mill and stir at 330 r / min for 35 min at room temperature;

[0061] Calcination: Calcinate at 770° C. for 4 h under argon gas conditions to obtain the artificial graphite material.

[0062] Example 2

[0063] This embodiment provides a method for preparing an artificial graphite material, the preparation method comprising the following steps:

[0064] (1) Pretreatment

[0065] The calcined coal-based needle coke was crushed to a D50 of 6 μm using a jet mill, 500 g of the crushed material was added with 8 wt% coal tar as a binder, and stirred for 1 h in a VC mixer at 400 r / min and a frequency of 70 Hz to obtain material A;

[0066] (2) Boron doping secondary granulation

[0067] Mixing: placing material A and boron carbide in a mass ratio of 18:1 in a reaction kettle, stirring at 360 r / min for 55 min under argon gas protection and room temperature to obtain a mixed material;

[0068] Granulation: The mixed material was heated from room temperature to 280°C, stirred at constant temperature for 2.5 hours at a stirring speed of 260 r / min; then heated to 680°C at a heating rate of 2.5°C / min, and kept at constant temperature for 4 hours to obtain the granulated material;

[0069] Graphitization: The granulated material is placed in a graphitization furnace, heated to 3000°C at a heating rate of 7°C / min, and graphitized at high temperature for 80 hours. The graphitized material is mixed (at a rate of 15r / min, for 90 minutes), sieved (using a 400-mesh screen), and demagnetized to obtain a boron-doped secondary granulated negative electrode material;

[0070] (3) Nitrogen doping

[0071] Mixing: Place the boron-doped secondary granulated negative electrode material and ethylenediamine in a mass ratio of 1:28 in a stirred mill and stir at 350 r / min for 40 min at room temperature;

[0072] Calcination: Calcinate at 800° C. for 6 h under argon gas conditions to obtain the artificial graphite.

[0073] Example 3

[0074] This embodiment provides a method for preparing an artificial graphite material, the preparation method comprising the following steps:

[0075] (1) Pretreatment

[0076] The calcined coal-based needle coke was ground to a D50 of 8 μm using a jet mill, 500 g of the ground material was added with 7 wt % of coal tar as a binder, and stirred in a VC mixer at 450 r / min and a frequency of 75 Hz for 2 h to obtain material A;

[0077] (2) Boron doping secondary granulation

[0078] Mixing: placing material A and boron trioxide in a mass ratio of 25:1 in a reaction kettle, stirring at 380 r / min for 60 min under argon protection and room temperature to obtain a mixed material;

[0079] Granulation: The mixed material was heated from room temperature to 300°C, stirred at a constant temperature for 2.5 hours at a stirring speed of 300 r / min; then heated to 650°C at a heating rate of 2°C / min, and kept at a constant temperature for 4 hours to obtain the granulated material;

[0080] Graphitization: The granulated material is placed in a graphitization furnace, heated to 3000°C at a heating rate of 5°C / min, and graphitized for 70 hours. The graphitized material is mixed (at a rate of 18r / min, for 100 minutes), sieved (using a 500-mesh screen), and demagnetized to obtain a boron-doped secondary granulated negative electrode material;

[0081] (3) Nitrogen doping

[0082] Mixing: Place the boron-doped secondary granulated negative electrode material and melamine in a mass ratio of 1:25 in a stirred mill and stir at 380 r / min for 50 min at room temperature;

[0083] Calcination: Calcinate at 800° C. for 5 h under argon gas conditions to obtain the artificial graphite material.

[0084] Example 4

[0085] This embodiment provides a method for preparing an artificial graphite material, the preparation method comprising the following steps:

[0086] (1) Pretreatment

[0087] The calcined coal-based needle coke was ground to a D50 of 5 μm using a jet mill, 500 g of the ground material was added with 7 wt % of coal tar as a binder, and stirred in a VC mixer at 350 r / min and a frequency of 65 Hz for 1.5 h to obtain material A;

[0088] (2) Boron doping secondary granulation

[0089] Mixing: placing material A and boric acid in a mass ratio of 30:1 in a reaction kettle, stirring at 330 r / min for 55 min under argon gas protection and room temperature to obtain a mixed material;

[0090] Granulation: The mixed material was heated from room temperature to 450°C at a rate of 2°C / min, and stirred at a constant temperature for 2 hours at a stirring rate of 220 r / min; then the temperature was raised to 700°C at a heating rate of 2°C / min, and kept at a constant temperature for 3.5 hours to obtain the granulated material;

[0091] Graphitization: The granulated material is placed in a graphitization furnace, heated to 2800°C at a heating rate of 5°C / min, and graphitized for 65 hours. The graphitized material is mixed (at a rate of 8r / min, for 80 minutes), sieved (using a 400-mesh screen) and demagnetized to obtain a boron-doped secondary granulated negative electrode material;

[0092] (3) Nitrogen doping

[0093] Mixing: Place the boron-doped secondary granulated negative electrode material and melamine in a mass ratio of 1:20 in a stirred mill and stir at 330 r / min for 35 min at room temperature;

[0094] Calcination: Calcinate at 1000° C. for 3 h under argon gas conditions to obtain the artificial graphite material.

[0095] Example 5

[0096] This embodiment provides a method for preparing an artificial graphite material. The preparation method is the same as that of Embodiment 1 except that the mass ratio of material A to boric acid in step (2) is 35:1.

[0097] Example 6

[0098] This embodiment provides a method for preparing an artificial graphite material. The preparation method is the same as that of Embodiment 1 except that the mass ratio of material A to boric acid in step (2) is 5:1.

[0099] Example 7

[0100] This embodiment provides a method for preparing an artificial graphite material. The preparation method is the same as that of Embodiment 1 except that the mass ratio of the boron-doped secondary granulated negative electrode material to melamine in step (3) is 1:35.

[0101] Example 8

[0102] This embodiment provides a method for preparing an artificial graphite material. The preparation method is the same as that of Embodiment 1 except that the mass ratio of the boron-doped secondary granulated negative electrode material to melamine in step (3) is 1:15.

[0103] Example 9

[0104] This embodiment provides a method for preparing an artificial graphite material. The preparation method is the same as that of Embodiment 1 except that granulation is not performed in step (2).

[0105] Comparative Example 1

[0106] This comparative example provides a method for preparing an artificial graphite material, wherein the method is to prepare artificial graphite by primary granulation after graphitization of coal-based needle coke;

[0107] The preparation method described in this comparative example specifically comprises the following steps:

[0108] The calcined coal-based needle coke was crushed to a median particle size (D50) of 15 μm using a jet mill, placed in a carbonization furnace, heated to 1000°C at a rate of 5°C / min, and kept at a constant temperature for 5 hours to obtain a carbonized product. The carbonized product was placed in a graphitization furnace, heated to 3000°C at a rate of 10°C / min for high-temperature graphitization for 70 hours, and the graphitized material was mixed (at a rate of 10 r / min, for 100 minutes), sieved (using a 400-mesh screen), and demagnetized to obtain a graphitized product.

[0109] Comparative Example 2

[0110] This comparative example provides a method for preparing an artificial graphite material. The preparation method is the same as Example 1 except that boron doping is not performed in step (2), that is, the mixing step is not performed in step (2).

[0111] Comparative Example 3

[0112] This comparative example provides a method for preparing an artificial graphite material. The preparation method is the same as Example 1 except that step (3) is not performed.

[0113] Comparative Example 4

[0114] This comparative example provides a method for preparing an artificial graphite material, which is the same as Example 1 except that boron doping is not performed in step (2), that is, the mixing step is not performed in step (2), and step (3) is not performed.

[0115] Comparative Example 5

[0116] This comparative example provides a method for preparing an artificial graphite material. The preparation method is the same as Example 1 except that step (3) is not performed and the melamine in step (3) is added to step (2) and mixed with boric acid.

[0117] Comparative Example 6

[0118] This comparative example provides a method for preparing an artificial graphite material. The preparation method is the same as that of Example 1, except that boric acid and melamine are mixed and doped together and both are performed after graphitization.

[0119] Comparative Example 7

[0120] This comparative example provides a method for preparing an artificial graphite material. The preparation method is the same as Example 1 except that the boric acid in step (2) and the melamine in step (3) are interchanged so that nitrogen is doped first and then boron is doped.

[0121] The artificial graphite materials obtained in the above examples and comparative examples were subjected to material performance tests, and the test methods were as follows:

[0122] (1) The D50 median particle size of the artificial graphite negative electrode material was measured using a laser particle size distribution analyzer.

[0123] (2) Use a tap density tester to test the tap density of the graphite negative electrode material.

[0124] (3) Use a powder automatic compaction density meter to test the compaction density of the graphite negative electrode material.

[0125] (4) Use a specific surface area meter to test the specific surface area of ​​the graphite negative electrode material.

[0126] The test results of artificial graphite material formation are shown in Table 1:

[0127] Table 1

[0128]

[0129]

[0130] The artificial graphite materials obtained in the above examples and comparative examples were prepared into button cells and lithium iron phosphate soft pack batteries, as follows:

[0131] The artificial graphite (95.0wt%) prepared above was mixed with a conductive agent (1wt% SP), a binder (1.5wt% CMC and 2.5wt% SBR) and deionized water to form a slurry. The prepared slurry was evenly coated on a copper foil with a thickness of 12μm. The coated electrode was placed in a vacuum drying oven at 90°C and dried for 4h. The dried electrode was rolled and then cut into a circular electrode with a diameter of 14mm, and then baked in a vacuum drying oven at 90°C for 2h to obtain an artificial graphite electrode. Under an argon atmosphere, the glove box was assembled in the order of |negative electrode shell|spring sheet|gasket|lithium sheet|electrolyte|diaphragm|electrolyte|artificial graphite electrode|positive electrode shell|to form a CR2032 button battery.

[0132] The artificial graphite material (95.0wt%) obtained in the above examples and comparative examples, conductive agent (1wt% SP), binder (1.5wt% CMC and 2.5wt% SBR) and deionized water were mixed into negative electrode slurry, and negative electrode sheets were obtained after coating and drying; lithium iron phosphate (95.5wt%), CNT (1.5wt%), conductive agent (1wt% SP), binder (2wt% PVDF) and NMP solution were mixed into positive electrode slurry, and positive electrode sheets were obtained after coating and drying. Finally, they were cut and assembled with the separator into soft-pack batteries.

[0133] test:

[0134] (1) The capacity of the obtained button battery is tested, and the test method is as follows:

[0135] Leave for 12h→discharge at 0.1C rate to 0.005V→discharge at 0.05mA constant current to 0.005V→leave for 5min→discharge at 0.01mA constant current to 0.005V→leave for 5min→charge at 0.1C rate to 2V→leave for 5min.

[0136] (2) The obtained soft pack battery is subjected to an electrical performance test, and the test method is as follows:

[0137] First week coulomb efficiency test:

[0138] At 25°C, charge to 3.65V at 0.2C constant current and constant voltage, cut off current to 0.05C, leave for 30 minutes, and discharge to 2.5V at 0.2C constant current.

[0139] Rate performance test:

[0140] At 25℃, charge to 3.65V at 0.2C constant current and constant voltage, cut-off current 0.05C; discharge to 2.5V at 3C, repeat 5 times.

[0141] The battery performance test results are shown in Table 2:

[0142] Table 2

[0143] Discharge capacity (mAh / g) First week coulomb efficiency 3C / 0.2C capacity retention rate Example 1 350.7 93.6% 93.8% Example 2 349.4 94.2% 94.2% Example 3 351.8 93.8% 93.3% Example 4 350.9 94.0% 94.1% Example 5 346.7 93.2% 91.2% Example 6 348.1 93.5% 90.7% Example 7 347.4 92.9% 92.5% Example 8 345.8 93.1% 91.3% Example 9 343.8 91.9% 90.7% Comparative Example 1 340.1 90.5% 86.7% Comparative Example 2 344.6 91.7% 89.5% Comparative Example 3 345.5 92.2% 90.1% Comparative Example 4 342.64 91.3% 88.9% Comparative Example 5 345.5 92.2% 90.5% Comparative Example 6 342.1 92.7% 91.3% Comparative Example 7 347.9 92.5% 92.5%

[0144] From Table 1 and Table 2, we can see that:

[0145] (1) From the material performance test data, the D50 of the embodiment is relatively large, and the D50 of the comparative example 1 is the smallest, indicating that the small-sized substrate can be granulated by secondary granulation to obtain a larger-sized product; from the perspective of tap density and compaction density, the secondary granulation particles have higher tap and compaction densities, which can make the distribution of the pore size and pores of the electrode more uniform, the distribution of the conductive agent and the binder more uniform, reduce the contact resistance and charge exchange impedance of the electrode, increase the active area that can participate in the reaction, and thus significantly improve the electrochemical performance of the material; from the perspective of specific surface area, the specific surface area of ​​the embodiment is much smaller than that of the comparative example 1, and is basically smaller than that of the comparative examples 2-4. The embodiment has the characteristics of large particles and small specific surface area, small contact area with the electrolyte, small area for forming the SEI film, and can improve the first-cycle coulomb efficiency.

[0146] (2) It can be seen from Example 1 and Comparative Examples 1-4 that the battery performance data of Comparative Example 1 are the worst, the battery performance of the embodiment doped with boron and nitrogen is better than that of Comparative Examples 2, 3, and 4, and the battery performance of Comparative Example 3 doped with only boron is better than that of Comparative Example 2 doped with only nitrogen. From the above electrical performance data, it can be seen that the present invention can improve the discharge capacity, first coulomb efficiency, cycle performance and rate performance of the battery; it can be seen from Example 1 and Comparative Example 5 that if boron and nitrogen are doped at the same time, the doping effect is poor, because more active sites and defects can be formed by first doping B in the reactor, and these sites and defects are conducive to the subsequent doping of N; it can be seen from Example 1 and Comparative Example 5 that if boron and nitrogen are doped at the same time, the doping effect is poor, because more active sites and defects can be formed by first doping B in the reactor, and these sites and defects are conducive to the subsequent doping of N; 6 It can be seen that the present invention doped boron before graphitization, and promoted the boron doping process to the coking process to obtain doped needle coke, which can make the prepared element doping more uniform and the obtained battery electrochemical performance more excellent; from Example 1 and Comparative Example 7, it can be seen that if the doping order of boron and nitrogen is interchanged, N can be easily introduced in the first step, but the introduction effect of B in the secondary granulation process is very poor, and the order interchange causes the doping of B to be affected; from Example 1 and Examples 5-8, it can be seen that the doping amount of boron and nitrogen in the present invention will affect the doping effect and the performance of graphite materials, thereby affecting the battery performance; from Example 1 and Example 9, it can be seen that the secondary granulation of the present invention can enrich Li + The number of embedding and de-embedding channels in the lattice increases the isotropy of the negative electrode material, improving the battery's first coulombic efficiency and rate performance, etc.

[0147] In summary, the present invention provides an artificial graphite material and a preparation method and application thereof. The preparation method reduces the repulsive force between lithium ions and embedded lithium ions and increases the active sites in the material through the coordination of three steps of pretreatment, boron doping and nitrogen doping, so that the obtained artificial graphite material can improve the first coulombic efficiency, capacity and rate performance of the battery.

[0148] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing an artificial graphite material, It is characterized in that The preparation method comprises the following steps: (1) mixing a graphite material precursor with a binder for pretreatment to obtain a pretreated product; (2) boron-doping and graphitizing the pretreated product of step (1) to obtain a boron-doped product; (3) Nitrogen-doping the boron-doped product of step (2) to obtain the artificial graphite material.

2. The preparation method according to claim 1, It is characterized in that The graphite material precursor in step (1) includes calcined coal-based needle coke; Preferably, the graphite material precursor in step (1) is first crushed and then mixed with a binder; Preferably, the particle size D50 of the graphite material precursor crushed is 4-8 μm; Preferably, the amount of the binder added in step (1) is 6-8wt% of the mass of the graphite material precursor; Preferably, the binder in step (1) comprises coal tar pitch; Preferably, the mixing time in step (1) is 1-2 hours, the rotation speed is 300-500 r / min, and the frequency is 60-80 Hz.

3. The preparation method according to claim 1 or 2, It is characterized in that The boron doping in step (2) comprises stirring and mixing the boron source and the pre-treated product in step (1); Preferably, the mass ratio of the pretreated product to the boron source in step (1) is (10-30):1; Preferably, the stirring and mixing is carried out at a speed of 300-400 r / min, for 50-60 min, and under protective gas; Preferably, the boron source includes any one of boric acid, boron oxide, boron carbide or boron trioxide, or a combination of at least two thereof.

4. The preparation method according to any one of claims 1 to 3, It is characterized in that In step (2), a secondary granulation step is also performed between the boron doping and graphitization; Preferably, the secondary granulation step comprises heat treating the boron-doped material under stirring; Preferably, the heat treatment comprises heating to 250-450°C at a rate of 2-3°C / min, stirring at a constant temperature for 2-3h at a stirring rate of 200-300r / min, then heating to 600-700°C at a heating rate of 2-3°C / min, and maintaining the constant temperature for 3-7h.

5. The preparation method according to any one of claims 1 to 4, It is characterized in that The graphitization heating rate in step (2) is 5-10°C / min, the temperature is 2600-3100°C, and the reaction time is 60-100h; Preferably, after the graphitization in step (2) and before the nitrogen doping in step (3), the process further includes mixing, screening and demagnetization steps; Preferably, the mixing rate is 5-20r / min and the mixing time is 80-120min; Preferably, the mesh size of the sieve used for the screening is 400-500 meshes.

6. The preparation method according to any one of claims 1 to 5, It is characterized in that The nitrogen doping in step (3) comprises mixing and calcining a nitrogen source and the boron doping product in step (2); Preferably, the mass ratio of the boron-doped product to the nitrogen source in step (2) is 1:(20-30); Preferably, the mixing rate of the nitrogen source and the boron-doped product of step (2) is 300-400 r / min, and the time is 30-50 min; Preferably, the calcination temperature is 700-1000°C and the time is 3-6h; Preferably, the nitrogen source includes any one of aniline, ethylenediamine, melamine or polyimide, or a combination of at least two of them.

7. The preparation method according to any one of claims 1 to 6, It is characterized in that The preparation method comprises the following steps: (1) pulverizing the calcined coal-based needle coke to a particle size D50 of 4-8 μm, and then mixing the pulverized material with a binder at a speed of 300-500 r / min and a frequency of 60-80 Hz for 1-2 hours to obtain a pretreated product, wherein the amount of the binder added is 6-8 wt% of the mass of the graphite material precursor; (2) mixing the pretreated product of step (1) and the boron source at a mass ratio of (10-30):1 under protective gas at a stirring rate of 300-400 r / min for 50-60 min, then heating to 250-450°C at a rate of 2-3°C / min, stirring at a constant temperature of 200-300 r / min for 2-3 h, then heating to 600-700°C at a heating rate of 2-3°C / min, keeping the temperature constant for 3-7 h, then heating to 2600-3100°C at a heating rate of 5-10°C / min, graphitizing for 60-100 h, and then mixing the graphitized product at a rate of 5-20 r / min for 80-120 min, sieving and demagnetizing to obtain a boron-doped product; (3) mixing the nitrogen source and the boron-doped product of step (2) at a rate of 300-400 r / min for 30-50 min, and then calcining at a temperature of 700-1000° C. for 3-6 h for nitrogen doping to obtain the artificial graphite material.

8. An artificial graphite material, It is characterized in that The artificial graphite material is prepared by the preparation method according to any one of claims 1 to 7.

9. A negative electrode sheet, It is characterized in that The negative electrode plate comprises the artificial graphite material as claimed in claim 8.

10. A battery, It is characterized in that The battery comprises the negative electrode sheet as claimed in claim 9.

Citation Information

Patent Citations

  • Doped pitch coke, graphite negative electrode material, preparation method and application of graphite negative electrode material, and lithium ion battery

    CN116022781A

  • Soft Carbon Anode Material, Its Preparation Method for Lithium Ion Battery and Lithium Ion Battery

    KR1020150077258A

  • Negative electrode material and method of preparing the same

    US20230147558A1

  • Composite graphite material and preparation method therefor, negative electrode plate, secondary battery, battery module, battery pack, and powered device

    WO2023040319A1

Cited By

  • Lithium ion battery and electric device comprising same

    CN120453298A