Lithium hydroxide monohydrate and preparation method thereof

By mixing the positive electrode powder of the waste lithium iron phosphate battery with dilute sulfuric acid, solid-liquid separation and subsequent treatment, high-purity lithium hydroxide is prepared, which solves the efficiency and environmental problems of lithium resource recycling and achieves high efficiency and environmental protection lithium resource recycling and recycling.

CN118993111APending Publication Date: 2024-11-22QINGHAI INST OF SALT LAKES OF CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410956785.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

After the retirement of waste lithium iron phosphate batteries, lithium resources were not effectively recycled, resulting in environmental pressure and waste of resources. The existing lithium resource recycling process has high carbon emissions and environmental pollution problems.

Method used

By mixing the positive electrode powder of the waste lithium iron phosphate battery with dilute sulfuric acid, solid-liquid separation is performed to obtain a lithium-containing leaching liquid, and high-purity lithium monohydrate is prepared by removing impurities, concentrating, electrodialysis and evaporation crystallization. The use of carbonate and the addition of precipitant are avoided, and efficient separation of lithium and recycling of resources are achieved.

Benefits of technology

The efficient separation and leaching rate of lithium is achieved exceeding 95%, the dissolution rate of iron is less than 0.1%, and the carbonate-free process reduces carbon emissions, high product purity, simple and easy to control process, avoids environmental pollution, and realizes Efficient recycling and recycling of lithium resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993111A_ABST
    Figure CN118993111A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing lithium hydroxide monohydrate by using a waste lithium iron phosphate battery. The method comprises the following steps: obtaining a lithium-containing leaching solution by using the waste lithium iron phosphate battery and dilute sulphuric acid; performing impurity removal and concentration treatment on the lithium-containing leachate to obtain a concentrated refined lithium sulfate solution; preparing a lithium hydroxide solution from the concentrated and refined lithium sulfate solution; and carrying out evaporative crystallization treatment on the lithium hydroxide solution to obtain lithium hydroxide monohydrate. The invention also discloses the lithium hydroxide monohydrate prepared by the preparation method. According to the method disclosed by the invention, efficient separation of lithium and iron in the positive electrode of the waste lithium iron phosphate battery is realized, the lithium concentration of the obtained leachate is relatively high, the dissolution loss rate of iron is relatively low, the obtained lithium hydroxide monohydrate product is not converted by a precipitator and is relatively high in purity, secondary pollution to the environment is completely eradicated, the use of direct raw materials is reduced, and the production cost is reduced. The process is relatively simple, easy to control and high in operation reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium, and in particular, relates to a method for preparing lithium hydroxide monohydrate by using waste lithium iron phosphate batteries and the lithium hydroxide monohydrate prepared by the method. Background Art

[0002] Lithium iron phosphate batteries are widely used in various electric vehicles due to their advantages such as high specific energy, long cycle life and good safety performance. Compared with nickel-cobalt-manganese ternary batteries, lithium iron phosphate materials are cheaper and the sources of the elements they contain are more extensive. The market share of lithium iron phosphate batteries will further increase in the future.

[0003] However, the service life of lithium iron phosphate power batteries is about 5-8 years, so every year, lithium iron phosphate batteries are retired on a large scale. Moreover, the lithium abundance in waste lithium iron phosphate is much higher than that of primary mineral resources. Lithium usually accounts for 1.1% of the weight of waste lithium iron phosphate batteries. The weight of the battery in an electric car with a mass of about 1.5 tons is about 500 kilograms.

[0004] Therefore, it is necessary to safely and effectively recycle waste lithium iron phosphate batteries, which can not only alleviate the environmental pressure caused by battery waste, but also achieve efficient recycling of lithium resources, energy conservation and environmental protection, and will also bring certain social and economic benefits. Summary of the invention

[0005] In order to solve the technical problems existing in the above-mentioned prior art, according to an embodiment of the present invention, a method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries and lithium hydroxide monohydrate prepared by the method are provided.

[0006] According to one aspect of an embodiment of the present invention, a method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries includes: obtaining a lithium-containing leachate using waste lithium iron phosphate batteries and dilute sulfuric acid; removing impurities and concentrating the lithium-containing leachate to obtain a concentrated and refined lithium sulfate solution; preparing a lithium hydroxide solution using the concentrated and refined lithium sulfate solution; and evaporating and crystallizing the lithium hydroxide solution to obtain lithium hydroxide monohydrate.

[0007] In an example of the method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries provided in the above aspect, the method for obtaining a lithium-containing leachate using the positive electrode of the waste lithium iron phosphate battery and dilute sulfuric acid includes: mixing and stirring dilute sulfuric acid, the positive electrode powder of the waste lithium iron phosphate battery and hydrogen peroxide to obtain a solid-liquid mixture; and performing solid-liquid separation treatment on the solid-liquid mixture to obtain a lithium-containing leachate.

[0008] In an example of the method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries provided in the above aspect, the method for obtaining a lithium-containing leachate using the positive electrode of the waste lithium iron phosphate battery and dilute sulfuric acid includes: mixing the positive electrode powder of the waste lithium iron phosphate battery and dilute sulfuric acid with a concentration of 0.05-0.5 mol / L according to a molar ratio of lithium to sulfur of 1.5-3.5:1, wherein the solid-liquid ratio in the mixture is 3-20 g / ml; adding hydrogen peroxide with a mass ratio of 15%-30% to the mixture according to a molar ratio of lithium to hydrogen peroxide of 1:0.5-3 to obtain a solid-liquid mixture; and performing solid-liquid separation on the solid-liquid mixture to obtain a lithium-containing leachate with a lithium concentration of 2.5-7 g / L.

[0009] In an example of the method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries provided in the above aspect, the method for removing impurities and concentrating the lithium-containing leachate includes: increasing the pH value of the lithium-containing leachate, and performing solid-liquid separation treatment on the lithium-containing leachate after the pH value is increased to obtain a primary refined lithium-containing leachate from which impurities are initially removed; increasing the pH value of the primary refined lithium-containing leachate, and adding an imprinting resin to the primary refined lithium-containing leachate after the pH value is increased to obtain a secondary refined lithium-containing leachate from which impurities are secondary removed; and performing reverse osmosis and electrodialysis treatment on the secondary refined lithium-containing leachate to concentrate the secondary refined lithium-containing leachate into a refined lithium-containing leachate.

[0010] In an example of the method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries provided in the above aspect, the method for evaporating and crystallizing the lithium hydroxide solution includes: adjusting the pH value of the lithium-containing leachate from 2-4 to 5.5-6, and performing solid-liquid separation treatment on the lithium-containing leachate with a pH value adjusted to 5.5-6 to obtain a primary refined lithium-containing leachate with impurities initially removed; adjusting the pH value of the primary refined lithium-containing leachate from 5.5-6 to 8-12, and adding an imprinting resin to the primary refined lithium-containing leachate with a pH value adjusted to 8-12 to obtain a secondary refined lithium-containing leachate with impurities secondary removed, wherein the lithium concentration in the secondary refined lithium-containing leachate is 2-6 g / L; performing reverse osmosis and electrodialysis treatment on the secondary refined lithium-containing leachate to concentrate the secondary refined lithium-containing leachate into a refined lithium-containing leachate with a lithium concentration of 10-15 g / L.

[0011] In an example of the method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries provided in the above aspect, the method for preparing a lithium hydroxide solution using the concentrated refined lithium sulfate solution includes: passing the refined lithium-containing leachate into a bipolar membrane electrodialysis device for electrolysis to prepare a lithium hydroxide solution.

[0012] In an example of the method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries provided in the above aspect, the method for preparing a lithium hydroxide solution using the concentrated refined lithium sulfate solution includes: passing the refined lithium-containing leachate into a bipolar membrane electrodialysis device for electrolysis to prepare a lithium hydroxide solution with a concentration of 1.5-3.0 mol / L.

[0013] In an example of the method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries provided in the above aspect, the method of evaporating and crystallizing the lithium hydroxide solution includes: performing a primary vacuum evaporation and concentration treatment on the lithium hydroxide solution to obtain a lithium hydroxide mixture after the primary vacuum evaporation and concentration treatment; performing solid-liquid separation on the lithium hydroxide mixture after the primary vacuum evaporation and concentration treatment to obtain primary crystallized lithium hydroxide; re-dissolving the primary crystallized lithium hydroxide, and performing a secondary vacuum evaporation and concentration treatment on the re-dissolved lithium hydroxide solution to obtain a lithium hydroxide mixture after the secondary vacuum evaporation and concentration treatment; performing solid-liquid separation on the lithium hydroxide mixture after the secondary vacuum evaporation and concentration treatment to obtain secondary crystallized lithium hydroxide; and drying the secondary crystallized lithium hydroxide to obtain lithium hydroxide monohydrate.

[0014] In an example of the method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries provided in the above aspect, the method for evaporating and crystallizing the lithium hydroxide solution includes: adding the lithium hydroxide solution with a concentration of 1.5-3.0 mol / L to a rotary evaporator for primary vacuum evaporation and concentration treatment to obtain a lithium hydroxide mixture after the primary vacuum evaporation and concentration treatment with a solid phase content volume ratio of 10%-25%; performing solid-liquid separation on the lithium hydroxide mixture after the primary vacuum evaporation and concentration treatment to obtain primary crystallized lithium hydroxide; re-dissolving the primary crystallized lithium hydroxide, and adding the re-dissolved lithium hydroxide solution to a rotary evaporator for secondary vacuum evaporation and concentration treatment to obtain a lithium hydroxide mixture after the secondary vacuum evaporation and concentration treatment with a solid phase content volume ratio of 10%-25%; performing solid-liquid separation on the lithium hydroxide mixture after the secondary vacuum evaporation and concentration treatment to obtain secondary crystallized lithium hydroxide; and drying the secondary crystallized lithium hydroxide under a nitrogen atmosphere to obtain lithium hydroxide monohydrate.

[0015] According to another aspect of an embodiment of the present invention, lithium hydroxide monohydrate is prepared by the above method.

[0016] Beneficial effects: According to the embodiments of the present invention, efficient separation of lithium and iron in the positive electrode powder of waste lithium iron phosphate batteries is achieved, the lithium concentration of the obtained leaching solution is high, and the iron dissolution rate is relatively low. The dilute sulfuric acid produced as a by-product in the process of preparing lithium hydroxide with a bipolar membrane is returned to the leaching section for direct use, so that the acid is produced and sold by itself. The produced brine is subjected to high-pressure reverse osmosis to obtain produced water and concentrated liquid that are continuously reused. The entire process does not use carbonates, which is beneficial to the reduction of carbon emissions compared to lithium carbonate production. The obtained monohydrate lithium hydroxide product is not converted with a precipitant and has a high purity. The mother liquor and condensed water obtained by evaporation can be recycled and not discharged, thereby eliminating secondary pollution to the environment and reducing the use of direct raw materials. The process is relatively simple, easy to control, and has high operational reliability. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The above and other aspects, features and advantages of the embodiments of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:

[0018] Figure 1 The present invention is a flowchart of a method for preparing lithium hydroxide monohydrate by using waste lithium iron phosphate batteries according to an embodiment of the present invention. DETAILED DESCRIPTION

[0019] Hereinafter, specific embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the present invention may be implemented in many different forms, and the present invention should not be construed as being limited to the specific embodiments set forth herein. On the contrary, these embodiments are provided to explain the principles of the present invention and their practical applications, so that other persons skilled in the art can understand the various embodiments of the present invention and various modifications suitable for specific intended applications.

[0020] As used herein, the term "including" and its variations represent open terms, meaning "including but not limited to". The terms "based on", "according to", etc. mean "based at least in part on", "based at least in part on". The terms "one embodiment" and "an embodiment" mean "at least one embodiment". The term "another embodiment" means "at least one other embodiment". The terms "first", "second", etc. may refer to different or the same objects. Other definitions may be included below, whether explicit or implicit. Unless the context clearly indicates otherwise, the definition of a term is consistent throughout the specification.

[0021] Figure 1 The present invention is a flowchart of a method for preparing lithium hydroxide monohydrate by using waste lithium iron phosphate batteries according to an embodiment of the present invention.

[0022] Reference Figure 1 According to an embodiment of the present invention, the method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries includes:

[0023] Step S110: obtaining a lithium-containing leaching solution using waste lithium iron phosphate battery positive electrode powder and dilute sulfuric acid;

[0024] Step S120: removing impurities and concentrating the lithium-containing leaching solution to obtain a concentrated and refined lithium sulfate solution;

[0025] Step S130: preparing a lithium hydroxide solution using the concentrated and refined lithium sulfate solution;

[0026] Step S140: performing evaporation and crystallization treatment on the lithium hydroxide solution to obtain lithium hydroxide monohydrate.

[0027] Furthermore, the step S110 includes: mixing and stirring dilute sulfuric acid, positive electrode powder of waste lithium iron phosphate batteries and hydrogen peroxide to obtain a solid-liquid mixture; and performing solid-liquid separation treatment on the solid-liquid mixture to obtain a lithium-containing leaching solution.

[0028] Specifically, one implementation method of step S110 includes: first, according to the molar ratio of lithium content in the positive electrode powder of the waste lithium iron phosphate battery to dilute sulfuric acid (i.e., lithium-sulfur molar ratio) of 1.5-3.5:1, a dilute sulfuric acid solution with a concentration of 0.05-0.5 mol / L is added to the positive electrode powder of the waste lithium iron phosphate battery according to a metered amount, and the solid and liquid are mixed evenly under rapid stirring, wherein the solid-liquid ratio in the mixed mixture is 3-20 g / mL; secondly, according to the molar ratio of lithium to hydrogen peroxide of 1:0.5-3, hydrogen peroxide with a mass ratio of 15%-30% is added to the mixture, and the reaction is continued to be stirred at room temperature for 1-3 hours to obtain a solid-liquid mixture; finally, the solid-liquid mixture is subjected to solid-liquid filtration separation treatment to obtain a lithium-containing leaching solution (wherein the lithium concentration is 2.5-7 g / L).

[0029] As an example, the separated solid sample is rinsed with 3-6 times the mass of the solid sample in deionized water, and the lithium concentration in the obtained eluent is 0.2-1.5 g / L, which is used to dilute sulfuric acid in the next leaching reaction to ensure the high lithium content of the lithium-containing leachate, while recycling lithium ions, the lithium leaching rate reaches 95%, and the iron dissolution rate is less than 0.1%

[0030] Further, the step S120 includes: increasing the pH value of the lithium-containing leachate, and performing solid-liquid separation treatment on the lithium-containing leachate after the pH value is increased to obtain a primary refined lithium-containing leachate from which impurities are initially removed; increasing the pH value of the primary refined lithium-containing leachate, and adding an imprinting resin to the primary refined lithium-containing leachate after the pH value is increased to obtain a secondary refined lithium-containing leachate from which impurities are secondary removed; and performing reverse osmosis and electrodialysis treatment on the secondary refined lithium-containing leachate to concentrate the secondary refined lithium-containing leachate into a refined lithium-containing leachate.

[0031] Specifically, one implementation of step S120 includes: first, adjusting the pH value of the lithium-containing leachate from 2-4 to 5.5-6 using a 0.5-2 mol / L lithium hydroxide solution, performing solid-liquid separation after sufficient reaction to obtain an initial removal of impurities (e.g., Al 3+ The invention relates to a method for preparing a primary refined lithium-containing leachate in which impurities are removed in the form of Al(OH)3; secondly, adjusting the pH value of the primary refined lithium-containing leachate from 5.5-6 to 8-12 to remove ions such as iron, copper, and manganese in the primary refined lithium-containing leachate, and removing trace phosphorus in the primary refined lithium-containing leachate by imprinting resin (wherein the flow rate is controlled to be 3-6BV / h during the phosphorus treatment process) to obtain a secondary refined lithium leachate with secondary impurity removal (wherein the lithium concentration is 2-6g / L); finally, treating the secondary refined lithium leachate by high-pressure reverse osmosis (e.g., by a reverse osmosis unit) and electrodialysis (e.g., by an electrodialysis membrane unit) to concentrate the secondary refined lithium leachate into a refined lithium-containing leachate with a lithium concentration of 10-15g / L.

[0032] As an example, the desalinated liquid formed after the secondary refined lithium leaching solution is concentrated is returned to the reverse osmosis unit for further concentration and recycling.

[0033] Furthermore, the step S130 includes: passing the refined lithium-containing leachate into a bipolar membrane electrodialysis device for electrolysis to prepare a lithium hydroxide solution.

[0034] As an example, the bipolar membrane electrodialysis device according to an embodiment of the present invention comprises: an acid chamber, an alkali chamber, a desalination chamber, an electrode chamber, a cation exchange membrane, an anion exchange membrane and a bipolar membrane. Under the action of a DC electric field, water molecules on the surface of the bipolar membrane are electrolyzed under the catalytic action of the catalytic layer inside the bipolar membrane to produce H + and OH - Through the action of electrostatic field and anion and cation membranes, sulfuric acid solution is generated in the acid chamber and lithium hydroxide solution is generated in the alkali chamber.

[0035] Therefore, one embodiment of step S130 includes: sending the refined lithium-containing leachate to a bipolar membrane electrodialysis device for electrolysis to prepare lithium hydroxide, so as to prepare a lithium hydroxide solution with a concentration of about 1.5-3.0 mol / L. During the preparation process, the flow rate of each chamber of the bipolar membrane electrodialysis device is adjusted to control the pressure difference balance between the inlet and outlet materials, maintaining it at about 0.04-0.08Mpa, setting the voltage, and maintaining the current density at 500-1000A / m 2, the conductivity of alkaline water is controlled to 200-300ms / cm, the conductivity of acid solution is 400-600ms / cm, and the concentration of prepared lithium hydroxide can reach 1.5-3.0mol / L and the concentration of sulfuric acid can reach 0.5-1.5mol / L through circulation enrichment in the liquid tank. At the same time, the lithium concentration in the desalination chamber can be reduced to below 3g / L.

[0036] Further, the step S140 includes: performing a primary vacuum evaporation and concentration treatment on the lithium hydroxide solution to obtain a lithium hydroxide mixture after the primary vacuum evaporation and concentration treatment; performing solid-liquid separation on the lithium hydroxide mixture after the primary vacuum evaporation and concentration treatment to obtain primary crystallized lithium hydroxide; re-dissolving the primary crystallized lithium hydroxide, and performing a secondary vacuum evaporation and concentration treatment on the re-dissolved lithium hydroxide solution to obtain a lithium hydroxide mixture after the secondary vacuum evaporation and concentration treatment; performing solid-liquid separation on the lithium hydroxide mixture after the secondary vacuum evaporation and concentration treatment to obtain secondary crystallized lithium hydroxide; and drying the secondary crystallized lithium hydroxide to obtain lithium hydroxide monohydrate.

[0037] Specifically, one implementation method of step S140 includes: first, adding a lithium hydroxide solution with a concentration of 1.5-3.0 mol / L to a rotary evaporator for initial vacuum evaporation and concentration treatment, controlling the evaporation temperature to 70-85° C., gradually adding a feed liquid (i.e., a lithium hydroxide solution with a concentration of 1.5-3.0 mol / L) during the evaporation process, and evaporating and concentrating the lithium hydroxide solution to 5-10 times to obtain a lithium hydroxide mixture after initial vacuum evaporation and concentration treatment with a solid phase volume ratio of 10%-25%; then, performing solid-liquid separation on the initially obtained lithium hydroxide mixture to obtain primary crystallized lithium hydroxide; Next, the primary crystallized lithium hydroxide is redissolved with distilled water, and the redissolved lithium hydroxide solution is added to a rotary evaporator for secondary vacuum evaporation and concentration treatment to obtain a lithium hydroxide mixture after secondary vacuum evaporation and concentration treatment with a solid phase volume ratio of 10%-25%; then, the lithium hydroxide mixture after the secondary vacuum evaporation and concentration treatment is subjected to solid-liquid separation treatment to obtain secondary crystallized lithium hydroxide; finally, the entrained liquid on the secondary crystallized lithium hydroxide can be rinsed with distilled water, and dried at 90°C in a nitrogen atmosphere to obtain a lithium hydroxide monohydrate product with a lithium hydroxide content greater than 56.6%.

[0038] As an example, the separated liquid obtained after solid-liquid separation of the initially obtained lithium hydroxide mixture and the separated liquid obtained after solid-liquid separation of the lithium hydroxide mixture after the secondary vacuum evaporation concentration treatment can be diluted to form the above-mentioned lithium hydroxide solution with a concentration of about 0.5-2.0 mol / L.

[0039] The following describes an implementation of preparing lithium hydroxide monohydrate using a method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries according to an embodiment of the present invention.

[0040] <Implementation Method 1>

[0041] The waste lithium iron phosphate batteries of a certain enterprise were used as raw materials. After stripping and crushing, a sulfuric acid solution with a concentration of 0.28 mol / L was added to the positive electrode powder of the waste lithium iron phosphate battery at a lithium-sulfur molar ratio of 2:1, and the solid-liquid ratio was controlled to be 10g / mL. The solid and liquid were mixed evenly under rapid stirring, and hydrogen peroxide with a mass ratio of 30% was slowly added at room temperature at a lithium-hydrogen peroxide molar ratio of 1:2. The reaction time was 2h. After the reaction was completed, it was filtered and separated, and the acidified leachate (i.e., lithium-containing leachate with a pH value of 2.31) was collected. The leached residue was washed with deionized water, and the washing water was collected for the next dilution of sulfuric acid. The leaching rate of lithium was 95.48%, and the dissolution rate of iron was less than 0.1%. The chemical components in the raw materials and acidified leachate were shown in Table 1.

[0042] Table 1

[0043] Components lithium manganese iron phosphorus aluminum Positive electrode powder% 4.14 0.006 34.28 17.95 0.036 Leachate g / L 3.58 0.011 0.036 0.17 0.047

[0044] The pH value of the acidified leaching solution was adjusted to 6 with a 1 mol / L lithium hydroxide solution. 3+ It is removed by precipitation in the form of Al(OH)3; after solid-liquid separation, the pH value of the liquid sample is further adjusted to 10.5 to remove the iron and manganese content in the solution, and the phosphorus in the solution is removed by imprinting resin. During the phosphorus removal process, the solution flow rate is controlled at 5BV / h to obtain a refined lithium sulfate solution with impurity ion concentrations less than 1 mg / L.

[0045] The refined lithium sulfate solution is concentrated through a high-pressure reverse osmosis unit and an electrodialysis membrane unit. After the lithium content reaches 12g / L, the concentrate is sent to a bipolar membrane electrodialysis unit for electrolysis. The concentrate passes through the bipolar membrane electrolysis unit and the circulation flow is adjusted to maintain the feed pressure of each chamber at about 0.04Mpa and the current density at 600A / m 2 , the alkaline water conductivity is controlled at 220ms / cm, the acid solution conductivity is controlled at 420ms / cm, and the feed liquid tank is enriched by circulation to obtain lithium hydroxide solution and by-product acid, wherein the concentration of lithium hydroxide solution is 1.8mol / L, and the concentration of by-product sulfuric acid is 0.9mol / L. When the lithium ion concentration in the light brine drops below 3g / L, it returns to the reverse osmosis unit for further concentration.

[0046] The by-product acid is returned for positive electrode powder leaching and resin regeneration process, and the lithium hydroxide solution is added to the rotary evaporator for vacuum evaporation and concentration. The evaporation temperature is controlled at 75°C, and the feed liquid (lithium hydroxide solution) is gradually added during the evaporation process. The lithium hydroxide solution is evaporated and concentrated to a solid content volume ratio of 15%, and solid-liquid separation is performed. The separated liquid phase continues to evaporate in a cycle, and the solid phase is redissolved with distilled water and evaporated and concentrated again. The crystal liquid is separated and the entrained liquid is eluted with distilled water. The solid phase is dried at 80°C for 4 hours under nitrogen protection to obtain a monohydrate lithium hydroxide product with a lithium hydroxide content of 56.6%.

[0047] <Implementation Method 2>

[0048] The waste lithium iron phosphate batteries of a certain enterprise were used as raw materials. After stripping and crushing, a sulfuric acid solution with a concentration of 0.3 mol / L was added to the positive electrode powder of the waste lithium iron phosphate battery at a lithium-sulfur molar ratio of 1.8:1, and the solid-liquid ratio was controlled to be 9g / mL. The solid and liquid were mixed evenly under rapid stirring, and hydrogen peroxide with a mass ratio of 30% was slowly added at room temperature at a lithium-hydrogen peroxide molar ratio of 1:1.75. The reaction time was 2h. After the reaction was completed, it was filtered and separated, and the acidified leachate (i.e., lithium-containing leachate with a pH value of 2.12) was collected. The leached residue was washed with deionized water, and the washing water was collected for the next dilution of sulfuric acid. The leaching rate of lithium was 95.13%, and the dissolution rate of iron was less than 0.1%. The chemical components in the raw materials and acidified leachate were shown in Table 2.

[0049] Table 2

[0050] Components lithium manganese iron phosphorus aluminum Positive electrode powder% 4.14 0.006 34.28 17.95 0.036 Leachate g / L 4.10 0.01 0.031 0.21 0.042

[0051] The pH value of the acidified leaching solution was adjusted to 6.5 with a 1 mol / L lithium hydroxide solution. 3+ It is removed by precipitation in the form of Al(OH)3; after solid-liquid separation, the pH value of the liquid sample is further adjusted to 10 to remove the iron and manganese content in the solution, and the phosphorus in the solution is removed by imprinting resin. During the phosphorus removal process, the solution flow rate is controlled at 5BV / h to obtain a refined lithium sulfate solution with impurity ion concentrations less than 1mg / L.

[0052] The refined lithium sulfate solution is concentrated through a high-pressure reverse osmosis unit and an electrodialysis membrane unit. After the lithium content reaches 13g / L, the concentrate is sent to a bipolar membrane electrodialysis unit for electrolysis. The concentrate passes through the bipolar membrane electrolysis unit and the circulation flow is adjusted to maintain the feed pressure of each chamber at about 0.05Mpa and the current density at 600A / m 2, the alkaline water conductivity is controlled at 250ms / cm, the acid solution conductivity is controlled at 450ms / cm, and the feed liquid tank is enriched by circulation to obtain lithium hydroxide solution and by-product acid, wherein the concentration of lithium hydroxide solution is 2mol / L, and the concentration of by-product sulfuric acid is 1mol / L. When the lithium ion concentration in the light brine drops below 3g / L, it returns to the reverse osmosis unit for further concentration.

[0053] The by-product acid is returned for positive electrode powder leaching and resin regeneration process, and the lithium hydroxide solution is added to the rotary evaporator for vacuum evaporation and concentration. The evaporation temperature is controlled at 80°C, and the feed liquid (lithium hydroxide solution) is gradually added during the evaporation process. The lithium hydroxide solution is evaporated and concentrated to a solid content volume ratio of 20%, and solid-liquid separation is performed. The separated liquid phase continues to evaporate in a cycle, and the solid phase is redissolved with distilled water and evaporated and concentrated again. The crystal liquid is separated and the entrained liquid is eluted with distilled water. The solid phase is dried at 85°C for 3 hours under nitrogen protection to obtain a monohydrate lithium hydroxide product with a lithium hydroxide content of 56.6%.

[0054] <Implementation Method 3>

[0055] The waste lithium iron phosphate batteries of a certain enterprise were used as raw materials. After stripping and crushing, the positive electrode powder of the waste lithium iron phosphate battery was measured at a lithium-sulfur molar ratio of 1.75:1, and a sulfuric acid solution with a concentration of 0.3 mol / L was added to the positive electrode powder, and the solid-liquid ratio was controlled to be 10 g / mL. After the solid and liquid were stirred and mixed evenly, at room temperature, a 30% mass ratio of hydrogen peroxide was slowly added at a lithium-hydrogen peroxide molar ratio of 1:1.8, and the reaction time was 2.5 hours. After the reaction was completed, the solid and liquid were separated by filtration, and the acidified leachate (i.e., lithium-containing leachate with a pH value of 3.72) was collected. The leached residue was washed with deionized water, and the washing water was collected for the next dilution of sulfuric acid. The leaching rate of lithium was 95.08%, and the dissolution rate of iron was less than 0.05%. The chemical components detected in the acidified leachate are shown in Table 3.

[0056] Table 3

[0057] Components lithium manganese cobalt nickel copper aluminum iron phosphorus Positive electrode powder% 3.87 1.23 0.16 0.41 0.39 0.91 35.05 17.34 Leachate g / L 3.18 0.52 0.038 0.095 0.049 0.028 0.002 0.038

[0058] The pH value of the acidified leaching solution was adjusted to 6.5 with a 1 mol / L lithium hydroxide solution. 3+ The precipitate formed by Al(OH)3 is removed; after solid-liquid separation, the pH value of the liquid sample is further adjusted to 12, and other ions in the solution (such as iron, copper, manganese and other ions) that generate corresponding hydroxide precipitates are also removed, and the phosphorus in the solution is removed by imprinting resin. During the phosphorus removal process, the solution flow rate is controlled at 5BV / h to obtain a refined lithium sulfate solution, and the content of each impurity ion is less than 1 mg / L.

[0059] The refined lithium sulfate solution is concentrated by a high-pressure reverse osmosis unit and an electrodialysis membrane unit. When the lithium ion content in the concentrate reaches 10g / L, it is sent to a bipolar membrane electrodialysis unit for electrolysis. The concentrate passes through the bipolar membrane electrolysis unit, and the flow rate is controlled to adjust the feed pressure of each chamber to maintain at about 0.06Mpa, and the current density is 500A / m 2 The conductivity of alkaline water is controlled at 200ms / cm, and the conductivity of acid solution is controlled at 400ms / cm. Lithium hydroxide solution and by-product acid are obtained by circulating enrichment in the liquid tank. The concentration of lithium hydroxide solution is 1.7mol / L, the concentration of by-product sulfuric acid is 0.8mol / L, and the lithium ions in the light brine are reduced to 2.5g / L.

[0060] The by-product acid is returned for positive electrode powder leaching and resin regeneration process, and the lithium hydroxide solution is added to the rotary evaporator for vacuum evaporation and concentration. The evaporation temperature is controlled at 80°C, and the feed liquid (lithium hydroxide solution) is gradually added during the evaporation process. The lithium hydroxide solution is evaporated and concentrated to a solid content volume ratio of 15%, and solid-liquid separation is performed. The separated liquid phase continues to evaporate in a cycle, and the solid phase is redissolved with distilled water and evaporated and concentrated again. The crystal liquid is separated and the entrained liquid is eluted with distilled water. The solid phase is dried at 80°C for 4 hours under nitrogen protection to obtain a monohydrate lithium hydroxide product with a lithium hydroxide content of 56.6%.

[0061] According to an embodiment of the present invention, there is also provided a Figure 1 The monohydrated lithium hydroxide prepared by the preparation method shown.

[0062] In summary, according to the embodiments of the present invention, the lithium element in the waste lithium iron phosphate battery is selectively extracted by low-concentration sulfuric acid, and efficient separation of lithium and iron is achieved. The leaching reaction is carried out at room temperature. The raw materials are dilute sulfuric acid obtained as a by-product of hydrogen peroxide and bipolar membrane electrolysis. The raw materials are easy to obtain and consume less reagents.

[0063] Furthermore, according to the embodiment of the present invention, high-purity lithium hydroxide monohydrate is prepared using the positive electrode powder of waste lithium iron phosphate batteries as raw material. No precipitant or conversion agent is added during the preparation of lithium hydroxide, avoiding the influence of conventional ions such as sodium, calcium, and chlorine ions on product indicators. The evaporation and crystallization process is easy to control, the obtained product has high purity, the process is easy to operate and control, the equipment and material selection are simple, and it is easy to apply industrially. At the same time, the loss of lithium ions in the impurity removal process during conventional lithium extraction is avoided, and the recovery rate of lithium is greatly improved. The lithium leaching rate in the preparation process exceeds 95%, and the iron dissolution rate is less than 0.1%.

[0064] Furthermore, according to the embodiments of the present invention, the amount of alkali used for impurity removal and refining of the leachate, as well as the regenerated acid and alkali solution and rinsing water in the process of impurity removal using resin can be self-supplied, and the raw materials are self-produced and sold without external purchase, thereby reducing the impact of the discharged liquid on the environment, achieving "zero discharge" of wastewater, and also reducing the production cost.

[0065] Furthermore, according to an embodiment of the present invention, a method is provided for producing high-quality lithium hydroxide monohydrate, and lithium resources are recycled. The separation, enrichment, concentration, and preparation of lithium salts of lithium ions are achieved, the use of raw acid and alkali is reduced, and the by-product acid is reused. The lithium-containing solution is concentrated by combining high-pressure reverse osmosis / electrodialysis to make the lithium concentration reach 10-15g / L. The dilute sulfuric acid produced as a by-product of bipolar membrane electrodialysis is returned to the waste lithium iron phosphate positive electrode black powder leaching section and can be directly used. The light brine after bipolar membrane electrodialysis is recycled to achieve closed-loop use, improve separation and concentration effects, and the entire process has green and low-carbon characteristics.

[0066] Furthermore, since there are more chloride ions in the lithium hydroxide solution obtained from the salt lake brine, the evaporation concentration process has high requirements for equipment materials. However, according to the embodiment of the present invention, the lithium hydroxide solution prepared by bipolar membrane electrodialysis of lithium sulfate solution does not contain chloride ions, and the evaporation concentration process has relatively low requirements for equipment materials.

[0067] The terms "exemplary," "example," and the like used throughout this specification mean "used as an example, instance, or illustration" and do not mean "preferred" or "advantageous" over other embodiments. The detailed description includes specific details for the purpose of providing an understanding of the described techniques. However, these techniques can be implemented without these specific details. In some instances, in order to avoid obscuring the concepts of the described embodiments, well-known structures and devices are shown in block diagram form.

[0068] The optional implementation modes of the embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the embodiments of the present invention are not limited to the specific details in the above implementation modes. Within the technical concept of the embodiments of the present invention, various simple modifications can be made to the technical solutions of the embodiments of the present invention, and these simple modifications all belong to the protection scope of the embodiments of the present invention.

[0069] The above description of the contents of this specification is provided to enable any person of ordinary skill in the art to implement or use the contents of this specification. Various modifications to the contents of this specification will be apparent to those of ordinary skill in the art, and the general principles defined herein may be applied to other variations without departing from the scope of protection of the contents of this specification. Therefore, the contents of this specification are not limited to the examples and designs described herein, but are consistent with the widest range of principles and novel features disclosed herein.

Claims

1. A method for preparing lithium hydroxide monohydrate using waste lithium iron phosphate batteries, characterized in that: The method comprises: Using waste lithium iron phosphate batteries and dilute sulfuric acid to obtain lithium-containing leaching solution; The lithium-containing leaching solution is subjected to impurity removal and concentration treatment to obtain a concentrated and refined lithium sulfate solution; Using the concentrated and refined lithium sulfate solution to prepare a lithium hydroxide solution; The lithium hydroxide solution is subjected to evaporation and crystallization treatment to obtain lithium hydroxide monohydrate.

2. The method according to claim 1, characterized in that The method for obtaining a lithium-containing leaching solution by using the positive electrode of a waste lithium iron phosphate battery and dilute sulfuric acid comprises: Mix and stir dilute sulfuric acid, cathode powder of waste lithium iron phosphate batteries and hydrogen peroxide to obtain a solid-liquid mixture; The solid-liquid mixture is subjected to solid-liquid separation treatment to obtain a lithium-containing leaching solution.

3. The method according to claim 1, characterized in that The method for obtaining a lithium-containing leaching solution by using the positive electrode of a waste lithium iron phosphate battery and dilute sulfuric acid comprises: According to the molar ratio of lithium to sulfur of 1.5-3.5:1, the positive electrode powder of the waste lithium iron phosphate battery and the dilute sulfuric acid with a concentration of 0.05-0.5 mol / L are mixed, wherein the solid-liquid ratio in the mixture is 3-20 g / ml; According to the molar ratio of lithium to hydrogen peroxide being 1:0.5-3, 15%-30% hydrogen peroxide is added to the mixture to obtain a solid-liquid mixture; The solid-liquid mixture is subjected to solid-liquid separation treatment to obtain a lithium-containing leaching solution with a lithium concentration of 2.5-7 g / L.

4. The method according to claim 1, characterized in that: The method for removing impurities and concentrating the lithium-containing leachate comprises: The pH value of the lithium-containing leachate is increased, and the lithium-containing leachate after the pH value is increased is subjected to solid-liquid separation treatment to obtain a primary refined lithium-containing leachate from which impurities are initially removed; The pH value of the primary refined lithium-containing leachate is increased, and an imprinting resin is added to the primary refined lithium-containing leachate after the pH value is increased to obtain a secondary refined lithium-containing leachate from which impurities are secondary removed; The secondary refined lithium-containing leachate is subjected to reverse osmosis and electrodialysis treatment to concentrate the secondary refined lithium-containing leachate into a refined lithium-containing leachate.

5. The method according to claim 1, characterized in that The method for performing evaporation and crystallization treatment on the lithium hydroxide solution comprises: The pH value of the lithium-containing leachate is adjusted from 2-4 to 5.5-6, and the lithium-containing leachate with the pH value adjusted to 5.5-6 is subjected to solid-liquid separation treatment to obtain a primary refined lithium-containing leachate from which impurities are initially removed; The pH value of the primary refined lithium-containing leachate is adjusted from 5.5-6 to 8-12, and an imprinting resin is added to the primary refined lithium-containing leachate with the pH value adjusted to 8-12 to obtain a secondary refined lithium-containing leachate with secondary impurity removal, wherein the lithium concentration in the secondary refined lithium-containing leachate is 2-6 g / L; The secondary refined lithium-containing leachate is subjected to reverse osmosis and electrodialysis treatment to concentrate the secondary refined lithium-containing leachate into a refined lithium-containing leachate with a lithium concentration of 10-15 g / L.

6. The method according to claim 1, characterized in that The method for preparing a lithium hydroxide solution by using the concentrated and refined lithium sulfate solution comprises: The refined lithium-containing leachate is passed into a bipolar membrane electrodialysis device for electrolysis to prepare a lithium hydroxide solution.

7. The method according to claim 1, characterized in that The method for preparing a lithium hydroxide solution by using the concentrated and refined lithium sulfate solution comprises: The refined lithium-containing leaching solution is passed into a bipolar membrane electrodialysis device for electrolysis to prepare a lithium hydroxide solution with a concentration of 1.5-3.0 mol / L.

8. The method according to claim 1, characterized in that The method for performing evaporation and crystallization treatment on the lithium hydroxide solution comprises: Performing a primary vacuum evaporation and concentration treatment on the lithium hydroxide solution to obtain a lithium hydroxide mixture after the primary vacuum evaporation and concentration treatment; performing solid-liquid separation on the lithium hydroxide mixture after the initial vacuum evaporation concentration treatment to obtain primary crystallized lithium hydroxide; Re-dissolving the initially crystallized lithium hydroxide, and performing a secondary vacuum evaporation and concentration treatment on the re-dissolved lithium hydroxide solution to obtain a secondary vacuum evaporation and concentration treated lithium hydroxide mixture; performing solid-liquid separation on the lithium hydroxide mixture after the secondary vacuum evaporation concentration treatment to obtain secondary crystallized lithium hydroxide; The secondary crystallized lithium hydroxide is dried to obtain lithium hydroxide monohydrate.

9. The method according to claim 1, characterized in that: The method for performing evaporation and crystallization treatment on the lithium hydroxide solution comprises: Adding the lithium hydroxide solution with a concentration of 1.5-3.0 mol / L to a rotary evaporator for primary vacuum evaporation and concentration treatment to obtain a lithium hydroxide mixture after primary vacuum evaporation and concentration treatment with a solid phase content volume ratio of 10%-25%; performing solid-liquid separation on the lithium hydroxide mixture after the initial vacuum evaporation concentration treatment to obtain primary crystallized lithium hydroxide; Re-dissolving the initially crystallized lithium hydroxide, and adding the re-dissolved lithium hydroxide solution to a rotary evaporator for secondary vacuum evaporation and concentration treatment to obtain a lithium hydroxide mixture after secondary vacuum evaporation and concentration treatment with a solid phase content volume ratio of 10%-25%; performing solid-liquid separation on the lithium hydroxide mixture after the secondary vacuum evaporation concentration treatment to obtain secondary crystallized lithium hydroxide; The secondary crystallized lithium hydroxide is dried under a nitrogen atmosphere to obtain lithium hydroxide monohydrate.

10. Lithium hydroxide monohydrate prepared by the method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Method for recovering lithium and ammonium from waste lithium battery leachate and application

    CN122235736A