Lithium cobalt oxide production process

By using nano-level barium oxide additives in the lithium cobalt oxide production process, the sintering process is optimized, and the residual alkali problem caused by insufficient atmosphere during lithium cobalt oxide sintering is solved, the diffusion capacity of lithium ions is improved, and the rate performance is significantly improved. Battery performance.

CN118993161APending Publication Date: 2024-11-22安徽巡鹰新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411344666.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the sintering process of lithium cobalt oxide, the residual alkali is too high due to insufficient atmosphere, which affects the product quality, and the lithium ion diffusion barrier is large, limiting the rate performance.

Method used

In the lithium cobalt oxide production process, nano-scale barium oxide is added as an additive. Through the primary and secondary sintering process, the dehydration and oxygen storage functions of barium oxide are used to increase the contact area between materials and air, promote reactions, reduce residual alkali content and Improve the diffusion coefficient of lithium ions.

Benefits of technology

It effectively reduces the residual alkali content of lithium cobalt oxide products, improves the rate performance, enhances the diffusion ability of lithium ions, and improves the charge and discharge rate and battery performance of lithium cobalt oxide positive electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005060628160000071
    Figure BDA0005060628160000071
Patent Text Reader

Abstract

The invention discloses a lithium cobalt oxide production process, and belongs to the field of lithium ion battery electrode materials. Barium oxide is doped in a lithium cobalt oxide raw material, and the lithium cobalt oxide raw material, lithium carbonate and cobaltosic oxide are mixed and sintered twice to prepare a high-quality lithium cobalt oxide product. By means of the characteristics of barium oxide, moisture and carbon dioxide in materials are removed in the one-time sintering process, and barium peroxide is formed through reaction with oxygen, so that the purpose of oxygen storage is achieved. Barium peroxide gradually releases oxygen at the temperature of 600 DEG C or above, formation of lithium cobalt oxide in the sintering reaction is promoted, holes are punched in each lattice of materials in the bowl filling step, the materials can make full contact with air, the reaction is more complete, and the content of residual alkali in the lithium cobalt oxide product is reduced. And doping of barium can enlarge the interlayer spacing of lithium cobalt oxide, migration of lithium ions is facilitated, and the rate capability of the lithium cobalt oxide positive electrode material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery electrode materials, and in particular relates to a lithium cobalt oxide production process. Background Art

[0002] As electric vehicles and portable electronic devices become increasingly popular, lithium-ion batteries have become an indispensable part of modern life. From the development trend of existing lithium-ion battery cathode materials, with the explosive development of smart phones and ultra-thin notebook computers, high-voltage lithium cobalt oxide materials will continue to develop in line with market trends. As one of the key materials for lithium-ion batteries, lithium cobalt oxide plays a decisive role in improving battery performance with its advantages such as high energy density and long cycle life.

[0003] At present, the preparation methods of lithium cobalt oxide mainly include solid-phase synthesis and soft chemical methods. The industrialized lithium cobalt oxide positive electrode materials are basically based on solid-phase synthesis. The solid-phase synthesis method is to fully mix the powder raw materials of cobalt and lithium through ball milling and high-speed stirring, and then obtain the final lithium cobalt oxide product through high-temperature sintering, crushing, screening and iron removal processes.

[0004] The sintering process is the process of high-temperature solid-phase reaction of lithium cobalt oxide, and it is the most critical step affecting the quality of lithium cobalt oxide products. From the reaction equation of lithium cobalt oxide, the high-temperature solid-phase reaction of lithium cobalt oxide requires the participation of oxygen and the discharge of carbon dioxide. In the actual sintering process, the purpose of the first sintering is to release the water in the raw materials and the carbon dioxide decomposed by lithium carbonate, and melt the lithium carbonate. The flowing lithium carbonate gradually wraps around the surface of the surrounding cobalt oxide particles and begins to penetrate and diffuse into the interior of the cobalt oxide particles. At the same time, under the influence of the surrounding oxidizing atmosphere, the divalent cobalt ions in the cobalt oxide are gradually oxidized to trivalent by oxygen, and lithium cobalt oxide crystals begin to form. As the external temperature continues to increase, the number of lithium ions diffusing into the interior of the cobalt oxide gradually increases. When the temperature rises to about 1000 degrees and is kept warm, the lithium ions are fully embedded and the lithium cobalt oxide crystals grow. The secondary sintering is to make the lithium and cobalt compounds fully contact and the sintering reaction fully and completely. During the entire sintering reaction process, timely discharge of water and carbon dioxide, and full contact between oxygen and reactants will promote the forward reaction.

[0005] The atmosphere during the sintering process has a great influence on the product quality. The accumulation of materials in the sagger will cause obstruction of gas circulation in the kiln. The internal materials cannot fully contact with the air. Not only can they not get enough oxygen, but the waste gas generated cannot be discharged in time, which will lead to incomplete reaction and high residual alkali in the finished lithium cobalt oxide product, which will have an adverse effect on product quality. Summary of the invention

[0006] The object of the present invention is to provide a lithium cobalt oxide production process, which reduces the residual alkali content of the lithium cobalt oxide product and improves the rate performance.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] The present invention provides a lithium cobalt oxide production process, comprising the following steps:

[0009] (1) Mixing: lithium carbonate, cobalt tetroxide and additives are put into a high-speed mixer and mixed;

[0010] (2) Loading: Load the mixed materials into the sagger, shake, level and draw grids, and make holes in each grid of the material;

[0011] (3) Primary sintering: Push the loaded materials into the tunnel kiln for sintering;

[0012] (4) Secondary sintering: The materials after primary sintering are crushed, mixed and put into a bowl, and then pushed into a tunnel kiln for sintering;

[0013] (5) Crushing: crushing the sintered material coarsely, finely and sieving in sequence, and cooling to room temperature to obtain a lithium cobalt oxide product;

[0014] The additive includes nano-scale barium oxide. The atomic molar ratio of barium to cobalt in the lithium cobalt oxide product is 3-5:200. The barium oxide has the functions of dehydration and oxygen storage.

[0015] Furthermore, in the lithium carbonate and cobalt oxide, the molar ratio of lithium to cobalt is 1.02-1.05.

[0016] Furthermore, the particle size of the lithium cobalt oxide product is 4-7 μm.

[0017] Furthermore, the mixing time of the mixture is 5-8 minutes, the speed of the high-speed mixer is 500-650r / min, the mixing amount is 50% of the volume of the high-speed mixer, the density of cobalt tetroxide is relatively large, and the density of lithium carbonate is relatively small. During the mixing process, the two raw materials will undergo convection homogenization. If the mixing time is too short, the convection is insufficient, and if the mixing time is too long, reverse mixing will occur.

[0018] Furthermore, the filling amount of the potting is 45%-55% of the volume of the sagger.

[0019] Furthermore, the horizontal surface area of ​​the holes in the sagger is 10%-20% of the horizontal surface area of ​​each grid of the material, the height of the holes is the same as the height of the material in the sagger, and the area of ​​the holes should not be too large, which will affect the filling amount of the sagger, and too small is not conducive to sufficient contact with the air.

[0020] Furthermore, the temperature of the primary sintering is set as follows: the room temperature is raised to 450-500° C. and kept for 1 hour, then raised to 800-850° C. and kept for 2 hours, and finally raised to 950-1100° C. and kept for 10-12 hours.

[0021] Furthermore, the temperature of the secondary sintering is set as: the temperature is raised from room temperature to 950-110° C. and kept for 10-12 hours.

[0022] Furthermore, the tap density of the lithium cobalt oxide product is ≥2.2 g / cm 3 .

[0023] Furthermore, the air intake volume in the tunnel kiln is 350-450m 3 / h.

[0024] Beneficial effects of the present invention:

[0025] (1) Add nano-scale barium oxide to the raw materials of lithium cobalt oxide. During the primary sintering process, part of the barium oxide will absorb moisture and carbon dioxide in the material to form barium carbonate, and part of the barium oxide will first react with oxygen to form barium peroxide. As the temperature rises to 600°C, lithium carbonate gradually penetrates into cobalt tetroxide to react, and barium peroxide will release oxygen to promote the reaction and reduce the residual alkali content produced by incomplete reaction.

[0026] (2) The barium element with a large ionic radius can be used to occupy the site of the Co element, thereby expanding the interlayer spacing of LiCoO2 and reducing the Li + The diffusion barrier increases the Li + The diffusion coefficient increases the charge and discharge rate. The diffusion coefficient of lithium ions is increased, thereby improving the rate performance of lithium cobalt oxide positive electrode materials.

[0027] (3) During the potting process, holes are punched in each grid of the material behind the drawing to increase the contact area between the material and the air without basically affecting the potting amount, so that the material and oxygen can fully react during the sintering process and reduce the residual alkali content. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] (1) Mixing: The raw materials of lithium carbonate, cobalt oxide and nano-barium oxide are put into a high-speed mixer for mixing. The mixing time is 5 minutes. The speed of the high-speed mixer is 650 r / min. The mixing amount is 50% of the volume of the high-speed mixer. Lithium carbonate and cobalt oxide are added at a lithium-cobalt molar ratio of 1.02. The barium oxide in the raw materials is added at a barium-cobalt atomic molar ratio of 3:200.

[0031] (2) Loading: Load the mixed materials into the sagger, shake, level and draw grids. Make holes in each grid of the material. The height of the holes should be the same as the height of the material in the sagger. The horizontal surface area of ​​the holes should be 10%-20% of the horizontal surface area of ​​each grid of the material. The loading amount should be 45% of the sagger volume.

[0032] (3) Primary sintering: The loaded materials are pushed into the tunnel kiln for sintering. The air intake in the tunnel kiln is 350m 3 / h, the temperature of the tunnel kiln is raised from room temperature to 450℃ and kept for 1h, then raised to 800℃ and kept for 2h, and finally raised to 950℃ and kept for 12h.

[0033] (4) Secondary sintering: The materials after primary sintering are crushed, mixed and put into a bowl, and then pushed into the tunnel kiln for sintering. The air intake in the tunnel kiln is 450m 3 / h, the temperature of the tunnel kiln rises from room temperature to 950℃ and is kept for 12h.

[0034] (5) Crushing: The sintered material is crushed coarsely, finely and sieved in sequence, and cooled to room temperature to obtain a lithium cobalt oxide product.

[0035] The tap density of the obtained lithium cobalt oxide product is ≥2.2g / cm 3 , particle size is 4-7μm.

[0036] Example 2

[0037] The amount of barium oxide added was increased, and the atomic molar ratio of barium to cobalt in the raw materials was adjusted to 4:200 during mixing. The other steps were the same as in Example 1.

[0038] The tap density of the obtained lithium cobalt oxide product is ≥2.2g / cm 3 , particle size is 4-7μm.

[0039] Example 3

[0040] The amount of barium oxide added was increased, and the atomic molar ratio of barium to cobalt in the raw materials was adjusted to 5:200 during mixing. The other steps were the same as in Example 1.

[0041] The tap density of the obtained lithium cobalt oxide product is ≥2.2g / cm 3 , particle size is 4-7μm.

[0042] Example 4

[0043] (1) Mixing: The raw materials of lithium carbonate, cobalt oxide and nano-barium oxide are put into a high-speed mixer for mixing. The mixing time is 7 minutes, the speed of the high-speed mixer is 550 r / min, and the mixing amount is 50% of the volume of the high-speed mixer. Lithium carbonate and cobalt oxide are added at a lithium-cobalt molar ratio of 1.04, and barium oxide in the raw materials is added at a barium-cobalt atomic molar ratio of 3:200.

[0044] (2) Loading: Load the mixed materials into the sagger, shake, level and draw grids. Make holes in each grid of the material. The height of the holes should be the same as the height of the material in the sagger. The horizontal surface area of ​​the holes should be 10%-20% of the horizontal surface area of ​​each grid of the material. The loading amount should be 50% of the volume of the sagger.

[0045] (3) Primary sintering: The loaded materials are pushed into the tunnel kiln for sintering. The air intake in the tunnel kiln is 380m 3 / h, the temperature of the tunnel kiln is raised from room temperature to 480℃ and kept for 1h, then raised to 830℃ and kept for 2h, and finally raised to 1050℃ and kept for 11h.

[0046] (4) Secondary sintering: The materials after primary sintering are crushed, mixed and put into a bowl, and then pushed into the tunnel kiln for sintering. The air intake in the tunnel kiln is 450m 3 / h, the temperature of the tunnel kiln rises from room temperature to 1050℃ and is kept for 11h.

[0047] (5) Crushing: The sintered material is crushed coarsely, finely and sieved in sequence, and cooled to room temperature to obtain a lithium cobalt oxide product.

[0048] The tap density of the obtained lithium cobalt oxide product is ≥2.2g / cm 3 , particle size is 4-7μm.

[0049] Example 5

[0050] (1) Mixing: The raw materials of lithium carbonate, cobalt oxide and nano-barium oxide are put into a high-speed mixer for mixing. The mixing time is 8 minutes, the speed of the high-speed mixer is 500 r / min, and the mixing amount is 50% of the volume of the high-speed mixer. Lithium carbonate and cobalt oxide are added at a lithium-cobalt molar ratio of 1.05, and barium oxide in the raw materials is added at a barium-cobalt atomic molar ratio of 3:200.

[0051] (2) Loading: Load the mixed materials into the sagger, shake, level and draw grids. Make holes in each grid of the material. The height of the holes should be the same as the height of the material in the sagger. The horizontal surface area of ​​the holes should be 10%-20% of the horizontal surface area of ​​each grid of the material. The loading amount should be 50% of the volume of the sagger.

[0052] (3) Primary sintering: The loaded materials are pushed into the tunnel kiln for sintering. The air intake in the tunnel kiln is 450m 3 / h, the temperature of the tunnel kiln is raised from room temperature to 500℃ and kept for 1h, then raised to 850℃ and kept for 2h, and finally raised to 1100℃ and kept for 12h.

[0053] (4) Secondary sintering: The materials after primary sintering are crushed, mixed and put into a bowl, and then pushed into the tunnel kiln for sintering. The air intake in the tunnel kiln is 450m 3 / h, the temperature of the tunnel kiln rises from room temperature to 1100℃ and is kept for 12h.

[0054] (5) Crushing: The sintered material is crushed coarsely, finely and sieved in sequence, and cooled to room temperature to obtain a lithium cobalt oxide product.

[0055] The tap density of the obtained lithium cobalt oxide product is ≥2.2g / cm 3 , particle size is 4-7μm.

[0056] Comparative Example 1

[0057] The difference from Example 1 is that no holes are punched on each grid of the material when filling the bowl. The other steps are the same as Example 1. The tap density of the obtained lithium cobalt oxide product is ≥2.2g / cm 3 , particle size is 4-7μm.

[0058] Comparative Example 2

[0059] The difference from Example 1 is that no additive is added to the mixture. The other steps are the same as Example 1. The tap density of the obtained lithium cobalt oxide product is ≥2.2g / cm 3 , particle size is 4-7μm.

[0060] Comparative Example 3

[0061] The difference from Example 1 is that the additive in the mixture is barium carbonate, and the barium carbonate in the raw material is added according to the atomic molar ratio of barium to cobalt of 3:200. The other steps are the same as Example 1, and the tap density of the obtained lithium cobalt oxide product is ≥2.2g / cm 3 , particle size is 4-7μm.

[0062] Comparative Example 4

[0063] The difference from Example 1 is that the additive in the mixture is magnesium oxide, and the magnesium oxide in the raw material is added according to the atomic molar ratio of magnesium to cobalt of 3:200. The other steps are the same as Example 1, and the tap density of the obtained lithium cobalt oxide product is ≥2.2g / cm 3 , particle size is 4-7μm.

[0064] The lithium cobalt oxide products prepared in Examples 1 to 5 and Comparative Examples 1 to 4 were sampled and tested, and the results are shown in Table 1.

[0065] Table 1

[0066]

[0067] As can be seen from Table 1, in Example 1 and Example 3, due to the increase in the content of barium oxide, the absorption of carbon dioxide and moisture and the release of oxygen can promote the reaction, reduce the content of unreacted lithium carbonate and lithium hydroxide, reduce the residual alkali content, and improve the rate performance. Example 4 and Example 5 increase the lithium-cobalt molar ratio in the raw material by 1.05. Compared with Example 1, the discharge specific capacity at low and high rates is increased, but the amount of unreacted lithium carbonate will also increase, and the residual alkali content will increase. In Comparative Example 1, the residual alkali content of the product increases and the discharge specific capacity decreases after the material is not pierced. The raw materials of Comparative Example 2 do not add any additives, and the comprehensive quality of the prepared lithium cobalt oxide product is poor. In Comparative Example 3, barium carbonate is used as a doping additive, and its effect is obviously not as good as that of Example 1. In Comparative Example 4, magnesium oxide, which is also an alkaline earth metal oxide, is used as an additive. Compared with the absence of additives in Comparative Example 2, its rate performance is improved, but it is obviously not as good as that of Example 1, and the reduction of residual alkali content is less.

[0068] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0069] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A lithium cobalt oxide production process, characterized in that: The steps include: (1) Mixing: putting raw materials lithium carbonate, cobalt tetroxide and additives into a high-speed mixer and mixing; (2) Loading: Load the mixed materials into the sagger, shake, level and draw grids, and make holes in each grid of the material; (3) Primary sintering: Push the loaded materials into the tunnel kiln for sintering; (4) Secondary sintering: The materials after primary sintering are crushed, mixed and put into a bowl, and then pushed into a tunnel kiln for sintering; (5) Crushing: crushing the sintered material coarsely, finely and sieving in sequence, and cooling to room temperature to obtain a lithium cobalt oxide product; The additive is nano-scale barium oxide, and the atomic molar ratio of barium to cobalt in the raw material is 3-5:

200.

2. A lithium cobalt oxide production process according to claim 1, characterized in that: The molar ratio of lithium to cobalt in the lithium carbonate and cobalt tetroxide is 1.02-1.

05.

3. A lithium cobalt oxide production process according to claim 1, characterized in that: The particle size of the lithium cobalt oxide product is 4-7 μm.

4. A lithium cobalt oxide production process according to claim 1, characterized in that: The mixing time of the mixing material is 5-8 minutes, the speed of the high-speed mixer is 500-650 r / min, and the mixing amount is 50% of the volume of the high-speed mixer.

5. A lithium cobalt oxide production process according to claim 1, characterized in that: The filling amount of the sagger is 45%-55% of the volume of the sagger.

6. A lithium cobalt oxide production process according to claim 1, characterized in that: The horizontal surface area of ​​the holes in the sagger is 10%-20% of the horizontal surface area of ​​each grid of the material, and the height of the holes is the same as the height of the material in the sagger.

7. A lithium cobalt oxide production process according to claim 1, characterized in that: The temperature of the primary sintering is set as follows: the room temperature is raised to 450-500° C. and kept for 1 hour, then the temperature is raised to 800-850° C. and kept for 2 hours, and finally the temperature is raised to 950-1100° C. and kept for 10-12 hours.

8. A lithium cobalt oxide production process according to claim 1, characterized in that: The temperature of the secondary sintering is set as follows: the temperature rises from room temperature to 950-110° C. and is kept for 10-12 hours.

9. A lithium cobalt oxide production process according to claim 1, characterized in that: The air intake volume in the tunnel kiln is 350-450m 3 / h.

10. A lithium cobalt oxide production process according to claim 1, characterized in that: The tap density of the lithium cobalt oxide product is ≥2.2 g / cm 3 .