Chemically strengthened glass, method for producing same, and glass
By performing multi-stage ion exchange treatment in the manufacturing process of chemically strengthened glass, using a specific molten salt composition to maximize the improvement of CS90, the problem of insufficient directional drop strength in the prior art is solved, and efficient glass strengthening effect is achieved.
Patent Information
- Application Number
- CN202410615179.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-17
- Publication Date
- 2024-11-22
AI Technical Summary
When existing chemically reinforced glasses increase directional drop strength, they can easily lead to a sharp increase in the number of crushings during spontaneous damage to the glass, and it is difficult to achieve sufficient directional drop strength.
By performing ion exchange treatment for more than two stages in the manufacturing process of chemically strengthened glass, the first ion exchange is performed with the glass using the first molten salt composition containing Li ions, and a larger alkali metal ions are used in the second stage. The second molten salt composition is subjected to a second ion exchange, thereby maximizing the compression stress value CS90 at a depth of 90 μm from the surface.
It is achieved to significantly improve the directional drop strength while avoiding the increase in the number of crushing when the glass is spontaneously damaged, and to suppress the internal tensile stress, achieving excellent directional drop strength.
Smart Images

Figure CN118993572A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to chemically strengthened glass, a method for producing the same, and the glass. Background Art
[0002] Chemically strengthened glass has been used in cover glass of electronic equipment terminals such as computers, smartphones, and tablets. Chemically strengthened glass forms a compressive stress layer on the surface of the glass by an ion exchange treatment in which the glass is brought into contact with a molten salt composition such as sodium nitrate or potassium nitrate. The ion exchange treatment generates ion exchange between alkali metal ions contained in the glass and alkali metal ions with a larger ion radius contained in the molten salt composition, thereby forming a compressive stress layer on the surface of the glass.
[0003] The strength of chemically strengthened glass depends on the stress distribution diagram represented by compressive stress (hereinafter also abbreviated as CS) with the depth from the glass surface as a variable. When two or more stages of ion exchange treatment are performed, as the above-mentioned compressive stress layer, a "surface compressive stress layer" formed mainly by potassium ions etc. introduced into the glass and a "deep compressive stress layer" formed mainly by sodium ions etc. introduced into the glass are formed.
[0004] On the other hand, if a compressive stress layer is formed on the surface of the glass, a tensile stress (hereinafter also abbreviated as CT) corresponding to the total amount of compressive stress will inevitably be generated in the center of the glass. If the CT value is too large, the glass article will break violently and scatter fragments when it breaks. If the CT value exceeds its threshold value (hereinafter also abbreviated as CT limit), the number of crushing when the glass is spontaneously damaged will increase sharply. The CT limit is a value inherent to the glass composition.
[0005] Therefore, the total amount of compressive stress in the surface layer of chemically strengthened glass is designed so as to increase the surface compressive stress and form a compressive stress layer to a deeper part, while not exceeding the CT limit. For example, Patent Document 1 discloses a chemically strengthened glass in which CT is controlled within a specific range. In addition, Patent Document 2 discloses a chemically strengthened glass having CS and DOC within a specific range. Patent Document 3 discloses a chemically strengthened glass in which the total amount of compressive stress is less than a certain value.
[0006] One of the indicators for evaluating the strength of glass materials used in smartphones is the sandpaper directional drop strength test. The sandpaper directional drop strength test is a test in which a sample made by laminating a smartphone housing or a simulated plate simulating a smartphone with a glass material is dropped onto #60 to #200 sandpaper, and the drop height at which cracks occur (hereinafter also referred to as "crack height" or "directional drop strength") is used as an indicator of strength.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: U.S. Patent No. 9359251
[0010] Patent Document 2: U.S. Patent No. 10150698
[0011] Patent Document 3: International Publication No. 2018 / 186402 Summary of the invention
[0012] If CS, which is the compressive stress value at a depth of 90 μm, is increased 90 , for example, a stress distribution diagram in which a large compressive stress is formed near a depth of 90 μm can prevent fracture caused by collision with a large protrusion. Figure 1 As shown, CS 90 It shows a high correlation with directional drop strength. Therefore, in order to develop glass with higher directional drop strength, it is necessary to improve CS 90 The value of .
[0013] For example, the specification of U.S. Patent No. 10730791 discloses that by diffusing Na ions as deeply as possible near the center of the plate thickness, the CT can be increased, thereby increasing the deep stress. However, if the CT is increased, the number of crushings during the spontaneous destruction of the glass will increase sharply, so there is a limit to the CT limit. Therefore, the directional drop strength in the prior art is not sufficient, and in order to further improve the directional drop strength, a higher CS is required. 90 Chemically strengthened glass.
[0014] Therefore, one object of the present invention is to provide a method for maximizing CS 90 , chemically strengthened glass that achieves excellent directional drop strength, its manufacturing method, and glass.
[0015] When two or more stages of ion exchange treatment are performed in the manufacturing process of chemically strengthened glass, the glass is brought into contact with the first molten salt composition for ion exchange in the first stage of ion exchange (hereinafter, also referred to as "first ion exchange"), thereby exchanging the "first alkali metal ions" in the glass with the "second alkali metal ions having an ionic radius larger than the first alkali metal ions" in the first molten salt composition, and the second alkali metal ions in the first molten salt composition are introduced into the glass. Furthermore, in the second stage of ion exchange (hereinafter, also referred to as "second ion exchange") after the first ion exchange, the chemically strengthened glass after the first ion exchange is brought into contact with the second molten salt composition for ion exchange.
[0016] After the second ion exchange, the ions in the second molten salt composition (for example, the third alkali metal ions having an ionic radius larger than the second alkali metal ions) are exchanged with the ions in the glass (for example, the second alkali metal ions), and the second alkali metal ions introduced into the glass from the first molten salt composition in the first ion exchange diffuse into the glass.
[0017] The present inventors have found that by using a composition containing a first alkali metal ion (e.g., Li ion, etc.) as the first molten salt composition in the first ion exchange, ion exchange of a second alkali metal ion (e.g., Na ion, etc.) in the glass with the first alkali metal ion in the first molten salt composition (hereinafter also referred to as reverse ion exchange) and the exchange of the first alkali metal ion in the glass with the second alkali metal ion in the first molten salt composition are carried out in parallel, thereby making it possible to make CS 90 The present invention has been completed based on the above findings.
[0018] The present invention provides chemically strengthened glass having the following structures, a method for producing the same, and glass.
[0019] 1. A chemically strengthened glass having a plate thickness of t (mm) and a compressive stress layer depth DOC of 180×t (μm) or more,
[0020] The integrated value CS of the compressive stress at a depth of 30 to 50 μm from the surface 30-50 is less than 12000Pa·m, and
[0021] Compressive stress value CS at a depth of 90 μm from the surface 90 It is above 175×t-88 (MPa).
[0022] 2. The chemically strengthened glass according to item 1 above, wherein the Young's modulus is 80 GPa or more.
[0023] 3. The chemically strengthened glass according to 1 or 2 above, wherein the stress value CS at a depth x [μm] from the glass surface measured by a scattered light photoelastic stress meter is x [MPa] distribution diagram, the above stress value CS x The value of the second-order differential CS x In CS x The range of ≥0 satisfies the following formula.
[0024] -0.03≤CS x ”≤0.013
[0025] 4. The chemically strengthened glass according to any one of 1 to 3 above, wherein the surface compressive stress value FSM-CS0 is 800 MPa or more.
[0026] 5. A chemically strengthened glass having a surface resistivity of 10 logΩ / sq or less and a Young's modulus of 80 GPa or more.
[0027] 6. A chemically strengthened glass, wherein a value obtained by dividing a Na2O concentration at a depth of 30 μm from the surface by a Na2O concentration at a depth of 90 μm from the surface is 1.30 or less.
[0028] 7. The chemically strengthened glass according to item 6 above, wherein a value obtained by dividing a Na2O concentration at a depth of 50 μm from the surface by a Na2O concentration at a center of the plate thickness is 2 to 4.
[0029] 8. The chemically strengthened glass according to 6 or 7 above, wherein a value obtained by dividing a Na2O concentration at a depth of 90 μm from the surface by a Na2O concentration at a center of the plate thickness is 2.4 or more.
[0030] 9. The chemically strengthened glass according to any one of 1 to 8 above, wherein the matrix composition, expressed in mol % based on oxides, contains 55 to 75% of SiO2, 3 to 15% of Li2O, and 8 to 25% of Al2O3.
[0031] 10. A method for producing a chemically strengthened glass, comprising: a first ion exchange treatment in which the chemically strengthened glass is brought into contact with a first molten salt composition, and a second ion exchange treatment in which the chemically strengthened glass is brought into contact with a second molten salt composition after the first ion exchange treatment.
[0032] In the first ion exchange treatment, the chemically strengthened glass is brought into contact with the first molten salt composition at 350 to 450° C. for 150 minutes or more.
[0033] The chemically strengthened glass contains, expressed in mol % based on oxides, 55 to 75% of SiO2, 3 to 15% of Li2O, and 8 to 25% of Al2O3.
[0034] 11. The method for producing a chemically strengthened glass according to 10 above, wherein the first molten salt composition contains 0.01 to 1 mass % of lithium ions.
[0035] 12. A method for producing a chemically strengthened glass, comprising: a first ion exchange treatment of bringing the chemically strengthened glass into contact with a first molten salt composition, and a second ion exchange treatment of bringing the chemically strengthened glass into contact with a second molten salt composition after the first ion exchange treatment,
[0036] The first ion exchange treatment is performed at 350 to 450° C. for 150 minutes or longer, the first molten salt composition contains lithium ions,
[0037] The chemically strengthened glass contains, expressed in mol % based on oxides, 55 to 75% of SiO2, 3 to 15% of Li2O, and 8 to 25% of Al2O3.
[0038] 13. The method for producing a chemically strengthened glass according to 12 above, wherein the second molten salt composition contains 0 to 5% by mass of lithium nitrate.
[0039] 14. The method for producing a chemically strengthened glass according to 12 or 13, further comprising: a third ion exchange treatment of bringing the chemically strengthened glass into contact with a third molten salt composition after the second ion exchange treatment;
[0040] The third molten salt composition contains 98 mass % or more of potassium nitrate.
[0041] 15. The method for producing a chemically strengthened glass according to any one of 11 to 13 above, wherein the CTave of the chemically strengthened glass is made smaller than CTA by the ion exchange treatment after the second ion exchange treatment. Here, CTA is obtained by the following formula (1), and CTave is obtained by the following formula (2).
[0042]
[0043] t: Plate thickness (μm)
[0044] K1c: Fracture toughness value (MPa·m 1 / 2 )
[0045] CTave=ICT / LCT…Formula (2)
[0046] ICT: Integrated value of tensile stress (Pa·m)
[0047] LCT: Length of the tensile stress region in the plate thickness direction (μm)
[0048] 16. A glass comprising, expressed in mole % based on oxides, 55-75% SiO2, 8-25% Al2O3, 3-15% Li2O, 1-5% Na2O, 0-3% K2O, 0-10% MgO, 0-10% CaO, 0-5% SrO, 0-5% ZnO, 0-3% TiO2, 0-3% ZrO2, 0-1% SnO2, 0-1% P2O5, 0-10% B2O3, 0-3% Y2O3, 0-0.1% Fe2O3,
[0049] The ratio of Li2O content to the total content of Li2O, Na2O and K2O, i.e. Li2O / [Li2O+Na2O+K2O], is 0.5 to 0.9.
[0050] The ratio of the content of Li2O to the content of Na2O, that is, Li2O / Na2O, is 1.5 to 10, and the Young's modulus is 80 GPa or more.
[0051] 17. The glass according to 16 above, wherein the ratio of the content of B2O3 to the content of P2O5, i.e. B2O3 / P2O5, is 2.5 to 500.
[0052] 18. The glass according to 16 or 17, wherein when a compressive stress layer is formed by ion exchange treatment using a molten salt composed of sodium nitrate at 380° C. for 4 hours, the compressive stress value CS of the compressive stress layer at a depth of 30 μm from the surface is 30 It is above 150MPa.
[0053] The chemically strengthened glass according to the first embodiment of the present invention has stress characteristics within a specific range. In the chemically strengthened glass according to the present invention, in particular, the integral value CS of the compressive stress at a depth of 30 to 50 μm from the surface 30-50 12000Pa·m or less to reduce the surface compressive stress, which can suppress the internal tensile stress, and when the plate thickness is t (mm), CS 90 When it is 175×t-88 (MPa) or above, it has high deep compressive stress. This avoids the CT limit and achieves excellent directional drop strength that cannot be achieved with previous technologies.
[0054] The chemically strengthened glass according to the second embodiment of the present invention has a surface resistivity and a Young's modulus within a specific range, thereby suppressing peeling of the coating layer and achieving a higher deep compressive stress than before while maintaining a high surface compressive stress.
[0055] The chemically strengthened glass according to the third embodiment of the present invention has a value obtained by dividing the Na2O concentration at a depth of 30 μm from the surface by the Na2O concentration at a depth of 90 μm from the surface, which is 1.30 or less. The Na2O concentration of a general chemically strengthened glass increases from the center of the glass to the surface of the glass, but by making the above value 1.30 or less, the distribution diagram of the sodium concentration in the glass becomes flat, the surface compressive stress can be reduced and the internal tensile stress can be suppressed, and a high deep compressive stress can be achieved. In addition, compared with the past, the increase in surface resistivity can be effectively suppressed, and the peeling of the coating can be suppressed.
[0056] The method for producing chemically strengthened glass according to the fourth embodiment of the present invention includes at least: a first ion exchange treatment in which a chemically strengthened glass having a composition in a specific range is brought into contact with a first molten salt composition at 350 to 450° C. for 150 minutes or more, and a second ion exchange treatment in which the chemically strengthened glass is brought into contact with a second molten salt composition after the first ion exchange treatment. Thus, the CS is maximized in the first ion exchange treatment. 90 , it is possible to produce chemically strengthened glass that exhibits excellent directional drop strength that was not achievable with previous technologies.
[0057] The manufacturing method of the chemically strengthened glass of the fifth embodiment of the present invention includes at least: a first ion exchange treatment of bringing the chemically strengthened glass having a composition in a specific range into contact with a first molten salt composition containing lithium ions at 350 to 450°C for more than 150 minutes, and a second ion exchange treatment of bringing the chemically strengthened glass into contact with a second molten salt composition after the first ion exchange treatment. Thus, in the first ion exchange, the surface compressive stress is reduced and the internal tensile stress is reduced by processes such as structural relaxation caused by heat and reverse ion exchange in the surface layer, so that the CS can be maximized while avoiding the CT limit. 90 , chemically strengthened glass that exhibits excellent directional drop strength that could not be achieved with previous technologies.
[0058] The glass according to the sixth embodiment of the present invention has a composition and a Young's modulus within specific ranges, and is obtained by chemically strengthening to have a higher deep compressive stress than ever while maintaining a high surface compressive stress. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 It shows CS 90 Plot of correlation with directional drop strength on #80 sandpaper.
[0060] Figure 2 (a) and (b) are schematic diagrams for explaining ion exchange in one embodiment of the present invention. Figure 2 (a) represents the first ion exchange treatment, Figure 2 (b) represents the second ion exchange treatment.
[0061] Figure 3 This is a diagram showing stress characteristics of glass after one-step chemical strengthening.
[0062] Figure 4 This is a diagram showing the results of measuring CS on chemically strengthened glass.
[0063] Figure 5 The CTave and CS values of chemically strengthened glass are shown in Figure 1. 90 A graph of the correlation.
[0064] Figure 6 (a) and (b) are diagrams showing stress distribution diagrams of chemically strengthened glass. DETAILED DESCRIPTION
[0065] In this specification, "chemically strengthened glass" refers to glass subjected to a chemical strengthening treatment, and "glass for chemical strengthening" refers to glass before subjected to a chemical strengthening treatment.
[0066] In this specification, unless otherwise specified, the glass composition is expressed in mol % based on oxides, and mol % is abbreviated as "%".
[0067] In addition, the term "substantially free of" in this specification means that the content is less than the level of impurities contained in raw materials, etc., that is, it is not intentionally added. Specifically, for example, it is less than 0.1%.
[0068] In this specification, "stress distribution diagram" refers to a diagram that represents the compressive stress value with the depth from the glass surface as a variable. In the stress distribution diagram, tensile stress is sometimes represented as negative compressive stress. In this specification, tensile stress is represented by absolute value.
[0069] The "compressive stress value (CS)" can be measured by thinning the cross section of the glass and analyzing the thinned sample using a birefringence imaging system. The birefringence imaging system stress meter is a device that uses a polarizing microscope and a liquid crystal compensator to measure the magnitude of the delay caused by stress, such as the birefringence imaging system Abrio-IM manufactured by CRi.
[0070] In addition, scattered light photoelasticity can sometimes be used for measurement. In this method, light is incident from the surface of the glass, and the polarized light of the scattered light is analyzed to measure CS. As a stress measuring instrument using scattered light photoelasticity, for example, there is a scattered light photoelasticity stress meter SLP-2000 manufactured by Orihara Manufacturing Co., Ltd.
[0071] In this specification, the "compression stress layer depth (DOC)" is the depth at which the compression stress value is zero. In the following, the surface compression stress value measured by the scattered light photoelastic stress meter is sometimes referred to as CS0, and the compression stress value at a depth of 50 μm from the surface is sometimes referred to as CS 50 , the compressive stress value at a depth of 90 μm from the surface is recorded as CS 90 In addition, "internal tensile stress (CT)" refers to the absolute value of the tensile stress at a depth of 1 / 2 of the plate thickness t. In this specification, it is the same as "CS t / 2 "Equal.
[0072] In this specification, "Young's modulus" is measured by an ultrasonic method.
[0073] In this specification, the "fracture toughness value K1c" is a value obtained according to the IF method specified in JIS R1607: 2015. The value of K1c is a value dependent on the glass composition and can be adjusted according to the glass composition.
[0074] In this specification, "surface resistivity" is measured using a contact conductivity meter. Surface resistivity has a positive correlation with volume resistivity.
[0075] <Directional drop strength>
[0076] In this specification, "#80 drop strength" is measured by the following method.
[0077] A glass sample of 120mm×60mm×0.7mm was embedded in a structure with mass and rigidity adjusted to the size of a smartphone commonly used today, and a smartphone was prepared to be dropped freely onto #80SiC sandpaper. As for the drop height, if it did not break after falling from a height of 5cm, the operation of raising the height by 5cm and dropping it again was repeated until it broke, and the height at the first break was taken as the drop height. The average crack height when 20 sheets of each glass sample were dropped was taken as the "#80 sandpaper average directional drop strength".
[0078] <4PB strength (4-point bending strength)>
[0079] In this specification, the 4PB strength is measured by the following method.
[0080] The chemically strengthened glass was processed into a strip of 120 mm × 60 mm, and a 4-point bending test was performed under the conditions of 30 mm between the outer fulcrums of the support, 10 mm between the inner fulcrums, and 5.0 mm / min of the crosshead speed to measure the 4-point bending strength. The number of test pieces was 10. It should be noted that after the chemically strengthened glass was processed into a strip, automatic chamfering (C chamfering) was performed using a No. 1000 grindstone (manufactured by Tokyo Diamond Tool Manufacturing Co., Ltd.), and the end surface was mirror-finished using a nylon brush with a diameter of 0.1 mm and SHOROX NZ abrasives (manufactured by Showa Denko K.K.) to obtain a glass plate with a thickness of 120 × 60 × 0.7 mm, and the glass plate was measured.
[0081] <Na concentration>
[0082] In this specification, the Na2O concentration at the depth x (μm) is measured by using EPMA (Electron Probe MicroAnalyzer) on the cross section in the plate thickness direction. The EPMA measurement is specifically performed as follows.
[0083] First, the glass sample is embedded with epoxy resin, and mechanically polished in a direction perpendicular to the first main surface and the second main surface opposite to the first main surface to prepare a cross-sectional sample. The polished cross section is carbon-coated and measured using EPMA (JEOL: JXA-8500F). The acceleration voltage is 15 kV, the probe current is 30 nA, the accumulation time is 1000 msec. / point, and the linear distribution diagram of the X-ray intensity of Na is obtained at 1 μm intervals. For the obtained Na2O concentration distribution diagram, the average count of the central part of the plate thickness (0.5×t) ± 25 μm (the plate thickness is set to t μm) is taken as the main composition, and the count of the entire plate thickness is converted into mole % in proportion.
[0084] <Stress measurement method>
[0085] In recent years, cover glass for smartphones and the like has become mainstream when it is obtained by chemically strengthening the glass in two or more stages, namely, exchanging lithium ions inside the glass with sodium ions (Li-Na exchange) and then further exchanging sodium ions inside the glass with potassium ions in the surface layer of the glass (Na-K exchange).
[0086] In order to obtain the stress distribution diagram of such a two-step chemically strengthened glass in a non-destructive manner, for example, a scattered light photoelastic stress meter (SLP), a film stress meter (FSM), etc. may be used in combination.
[0087] In the method using a scattered light photoelastic stress meter (SLP), the compressive stress from Li-Na exchange can be measured inside the glass at a distance of tens of μm or more from the glass surface. On the other hand, in the method using a glass surface stress meter (FSM), the compressive stress from Na-K exchange can be measured on the glass surface at a distance of tens of μm or less from the glass surface (for example, International Publication No. 2018 / 056121, International Publication No. 2017 / 115811). Therefore, as a stress distribution diagram of the glass surface and interior of a two-stage chemically strengthened glass, a stress distribution diagram synthesized from the information of SLP and FSM is sometimes used.
[0088] In the present invention, the stress distribution diagram measured by a scattered light photoelastic stress meter (SLP) is mainly used. It should be noted that when the compressive stress CS, tensile stress CT, compressive stress layer depth DOC, etc. are mentioned in this specification, it means the value in the SLP stress distribution diagram.
[0089] The scattered light photoelastic stress gauge is a stress measuring device having the following structure: a polarization phase difference variable member that changes the polarization phase difference of laser light by one wavelength or more relative to the wavelength of the laser light, an imaging element that captures scattered light generated by incident laser light with the changed polarization phase difference on tempered glass a plurality of times at predetermined time intervals to obtain a plurality of images, and a computing unit that measures periodic brightness changes of the scattered light using the plurality of images to calculate a phase change of the brightness change and calculates stress distribution in a depth direction from the surface of the tempered glass based on the phase change.
[0090] As a method for measuring the stress distribution map using a scattered light photoelastic stress meter, the method described in International Publication No. 2018 / 056121 can be cited. As scattered light photoelastic stress meters, for example, SLP-1000 and SLP-2000 manufactured by Orihara Seisakusho can be cited. If the attached software SlpIV_up3 (Ver.2019.01.10.001) is combined with these scattered light photoelastic stress meters, high-precision stress measurement can be performed.
[0091] <CTA>
[0092] The CT limit corresponds to CTA obtained by the following formula (1), and is a value determined by the composition of the chemically strengthened glass.
[0093]
[0094] t: Plate thickness (mm)
[0095] K1c: Fracture toughness value (MPa·m 1 / 2 )
[0096] <CTave>
[0097] "CTave" in this specification is calculated by the following formula (2): CTave is a value corresponding to the average value of the tensile stress, and is a value obtained by integrating the stress value of the tensile stress region in the plate thickness direction of the tensile stress region and dividing the result by the length of the tensile stress region.
[0098] CTave=ICT / LCT…Formula (2)
[0099] ICT: Integrated value of tensile stress (Pa·m)
[0100] LCT: Length of the tensile stress region in the plate thickness direction (μm)
[0101] <Chemically strengthened glass: first to third embodiments>
[0102] Hereinafter, as embodiments of the chemically strengthened glass according to the present invention, first to third embodiments will be described. In this specification, the chemically strengthened glass according to the present invention including the first to third embodiments is also abbreviated as "the present chemically strengthened glass".
[0103] [Chemically Strengthened Glass of First Embodiment]
[0104] The chemically strengthened glass according to the first embodiment is characterized in that the thickness is t (mm), the depth of the compressive stress layer DOC is 180×t (μm) or more, and the integrated value CS of the compressive stress at a depth of 30 to 50 μm from the surface is 30-50 The compressive stress value CS at a depth of 90 μm from the surface is less than 12000 Pa·m. 90 It is above 175×t-88 (MPa).
[0105] The compressive stress layer depth DOC of the chemically strengthened glass involved in the first embodiment is 180×t (μm) or more, preferably 182.5×t (μm) or more, more preferably 185×t (μm) or more, further preferably 187.5×t (μm) or more, and particularly preferably 190×t (μm) or more. When DOC is 190×t (μm) or more, the compressive stress layer is formed to a deeper part of the glass, thereby obtaining an effect that it is not easy to break even when subjected to a large impact. There is no particular upper limit on the DOC. In order to suppress the cumulative value of the compressive stress value to a low level, for example, it is 300×t (μm) or less, preferably 280×t (μm) or less, further preferably 260×t (μm) or less, and particularly preferably 250×t (μm) or less.
[0106] The integrated value CS of the compressive stress at a depth of 30 to 50 μm from the surface of the chemically strengthened glass according to the first embodiment 30-50 Below 12000Pa·m. 30-50 12000Pa·m or less can reduce surface compressive stress and suppress internal tensile stress. 30-50 The lower limit of is not particularly limited, but is usually 7500 Pa·m or more, preferably 8000 Pa·m or more, more preferably 8250 Pa·m or more, and further preferably 8500 Pa·m or more.
[0107] The compressive stress value CS at a depth of 90 μm from the surface of the chemically strengthened glass according to the first embodiment 90It is 175×t-88 (MPa) or more, preferably 175×t-86 (MPa) or more, more preferably 175×t-83 (MPa) or more, further preferably 175×t-81 (MPa) or more, and particularly preferably 175×t-78 (MPa) or more. 90 175×t-88 (MPa) or more, which can improve the directional drop strength (for example, the directional drop strength of #80 sandpaper) compared with the past. 90 There is no particular upper limit on the value. In order to suppress the cumulative value of the compressive stress value to a lower level, it is, for example, 175×t-40 (MPa) or less, preferably 175×t-42.5 (MPa) or less, further preferably 175×t-45 (MPa) or less, and particularly preferably 175×t-50 (MPa) or less.
[0108] The Young's modulus of the chemically strengthened glass according to the first embodiment is preferably 80 GPa or more, more preferably 82 GPa or more, further preferably 84 GPa or more, and particularly preferably 85 GPa or more. When the Young's modulus is 80 GPa or more, a higher CTA can be achieved, and deep stress can be increased.
[0109] There is correlation between the diffusivity of Young's modulus and sodium ions, and the higher the Young's modulus, the more difficult the trend of Na ions to diffuse. If Young's modulus is more than 80GPa, Na ions are difficult to diffuse, and high surface compressive stress is easily introduced by ion exchange, even if the surface compressive stress is reduced due to reverse ion exchange, higher deep compressive stress can be maintained while maintaining high surface compressive stress. The upper limit of Young's modulus is not particularly limited, and from the viewpoint of bending process technology, it is usually less than 100GPa, preferably less than 95GPa, more preferably less than 90GPa.
[0110] As described above, the stress value CS of the chemically strengthened glass of the first embodiment measured by the scattered light photoelastic stress meter at a depth x [μm] from the glass surface is x In the distribution diagram of [MPa], the preferred stress value CS x The value of the second-order differential CS x In CS x ≥0, satisfying -0.03≤CS x ”≤0.013. Here, if CS x "It is more preferably 0.010 or less, further preferably 0.008 or less, and particularly preferably 0.006 or less, which further becomes a linear shape and can effectively increase the stress value CS at a depth of 90 μm. 90 In addition, CS x " is more preferably -0.028 or more, and even more preferably -0.024 or more.
[0111] CS x Stress value CS in the range ≥0 x The value of the first-order differential CS x ' is preferably -3.0 or more, more preferably -2.8 or more, and even more preferably -2.6 or more. If the first-order differential value CS x ' is within the above range, then CS x ' changes smaller, stress value CS x The distribution graph of becomes a straight line. In addition, for the same CS0, through CS x 'Large and get to maintain high CS 90 CS x 'Typically below -0.8.
[0112] It should be noted that, as a differentiation method of the stress distribution diagram, in the present invention, as shown in the following formula, in CS x In the distribution diagram, the CS value when the change of x is 0.5 μm is used. x The rate of change of CS x ', using the CS when the change in x is 0.5 μm x The rate of change of CS x ” value.
[0113] CS x '=(CS x+0.5 -CS x ) / 0.5
[0114] CS x = (CS x+0.5 '-CS x ') / 0.5
[0115] The chemically strengthened glass of the first embodiment is preferably such that the surface compressive stress value FSM-CS0 measured by FSM is 800 MPa or more, because the directional drop strength is further improved and it is not easy to break due to deformation such as bending. FSM-CS0 is more preferably 900 MPa or more, more preferably 950 MPa or more, and particularly preferably 1000 MPa or more. There is no particular upper limit on FSM-CS0, but it is usually preferably 1500 MPa or less from the viewpoint of suppressing the cumulative value of the compressive stress value to a lower value.
[0116] FSM-CS0: Compressive stress value at a depth of 0 μm measured by FSM
[0117] CS x : Compressive stress value at depth x [μm] measured by SLP
[0118] The depth DOL-tail of the surface compressive stress layer of the chemically strengthened glass of the first embodiment is preferably 2.8 μm or more, more preferably 2.9 μm or more, further preferably 3.0 μm or more, and particularly preferably 3.3 μm or more. By having a DOL-tail of 2.8 μm or more, the 4-point bending strength can be improved. There is no particular restriction on the upper limit of DOL-tail. From the perspective of balance with deep stress, it is preferably 8.0 μm or less, and more preferably 7.0 μm or less. In this specification, the depth DOL-tail of the surface compressive stress layer refers to the maximum depth of the compressive stress layer that can be measured by FSM.
[0119] The surface resistivity of the chemically strengthened glass according to the first embodiment is preferably 10 logΩ / sq or less, more preferably 9.5 logΩ / sq or less, further preferably 9.0 logΩ / sq or less, and particularly preferably 8.5 logΩ / sq or less. By making the surface resistivity 10 logΩ / sq or less, peeling of the coating layer can be suppressed. The lower limit of the surface resistivity is not particularly limited, but is generally preferably 7.0 logΩ / sq or more.
[0120] From the perspective of improving strength, the thickness t (mm) of the chemically strengthened glass in the first embodiment is preferably 0.8 mm or less, more preferably 0.7 mm or less, further preferably 0.65 mm or less, and particularly preferably 0.6 mm or less. The smaller t is, the more the effect of improving strength can be obtained by the present invention. t is typically 0.02 mm or more.
[0121] The stress characteristics and ion distribution diagram of the chemically strengthened glass of the first embodiment can be adjusted according to its parent composition and the conditions of the ion exchange treatment. The glass composition of the chemically strengthened glass of the first embodiment will be described later in the section "Parent Composition of Chemically Strengthened Glass".
[0122] [Chemically strengthened glass according to the second embodiment]
[0123] The chemically strengthened glass according to the second embodiment has a surface resistivity of 10 logΩ / sq or less and a Young's modulus of 80 GPa or more.
[0124] The surface resistivity of the chemically strengthened glass according to the second embodiment is 10 logΩ / sq or less, preferably 9.5 logΩ / sq or less, more preferably 9.0 logΩ / sq or less, further preferably 8.5 logΩ / sq or less, and particularly preferably 8.0 logΩ / sq or less.
[0125] The greater the surface resistivity of chemically strengthened glass, the easier it is for the coating to peel off (International Publication No. 2021 / 010376). In addition, the content ratio of alkali metal oxides affects the surface resistivity (International Publication No. 2021 / 010376). For example, a glass containing three alkali metal oxides, Li2O, Na2O, and K2O, has a larger surface resistivity than a glass containing only one or two alkali metal oxides although containing the same amount of alkali metal oxides due to the so-called mixed alkali effect.
[0126] Therefore, when the glass is chemically strengthened by ion exchange in two or more stages, a chemically strengthened glass containing three alkali metal oxides, namely Li2O, Na2O and K2O, is obtained, and there is a tendency that peeling of the coating layer becomes easy to occur. On the other hand, if the glass composition before strengthening and the chemical strengthening treatment conditions are adjusted in order to suppress peeling of the coating layer after chemical strengthening, it will be difficult to obtain sufficient strength by chemical strengthening.
[0127] The chemically strengthened glass of the second embodiment can suppress the charge between the coating surface and the glass surface and suppress the peeling of the coating layer by making the surface resistivity 10 logΩ / sq or less. The lower limit of the surface resistivity is not particularly limited, but is usually preferably 7.0 logΩ / sq or more.
[0128] The Young's modulus of the chemically strengthened glass according to the second embodiment is 80 GPa or more, preferably 82 GPa or more, more preferably 84 GPa or more, further preferably 85 GPa or more, and particularly preferably 85.5 GPa or more. If the Young's modulus is 80 GPa or more, Na ions are not easily diffused, and high surface compressive stress can be easily introduced by ion exchange. Even if the surface compressive stress is reduced by reverse ion exchange, a higher deep compressive stress can be maintained while maintaining a high surface compressive stress.
[0129] The chemically strengthened glass of the second embodiment preferably has the same properties as those of the chemically strengthened glass of the first embodiment with respect to properties other than surface resistivity and Young's modulus.
[0130] [Chemically strengthened glass according to the third embodiment]
[0131] The chemically strengthened glass of the third embodiment is characterized in that the value obtained by dividing the Na2O concentration at a depth of 30 μm from the surface by the Na2O concentration at a depth of 90 μm from the surface is 1.30 or less. The value obtained by dividing the Na2O concentration at a depth of 30 μm from the surface of the chemically strengthened glass of the third embodiment by the Na2O concentration at a depth of 90 μm from the surface is preferably 1.25 or less, more preferably 1.2 or less, further preferably 1.15 or less, further preferably 1.1 or less, and particularly preferably 1 or less. By making this value 1.30 or less, the distribution diagram of the sodium concentration in the glass becomes flat, the surface compressive stress can be reduced and the internal tensile stress can be suppressed, and a high deep compressive stress can be achieved. In addition, compared with the past, the increase in surface resistivity can be effectively suppressed, and the peeling of the coating can be suppressed.
[0132] The lower limit of the value obtained by dividing the Na 2 O concentration at a depth of 30 μm from the surface of the chemically strengthened glass according to the third embodiment by the Na 2 O concentration at a depth of 90 μm from the surface is not particularly limited.
[0133] The value obtained by dividing the Na2O concentration at a depth of 50 μm from the surface of the chemically strengthened glass of the third embodiment by the Na2O concentration at the center of the plate thickness is preferably 2 to 4. By setting this value to 2 to 4, the surface compressive stress can be further reduced, the internal tensile stress can be suppressed, and the deep compressive stress can be further increased.
[0134] The value obtained by dividing the Na2O concentration at a depth of 50 μm from the surface of the chemically strengthened glass of the third embodiment by the Na2O concentration in the center of the plate thickness is preferably 2 or more, more preferably 2.5 or more, further preferably 2.7 or more, further preferably 2.8 or more, and particularly preferably 2.9 or more. In addition, the value is preferably 4 or less, more preferably 3.5 or less, further preferably 3.3 or less, further preferably 3.2 or less, and particularly preferably 3.1 or less.
[0135] The value obtained by dividing the Na2O concentration at a depth of 90 μm from the surface of the chemically strengthened glass of the third embodiment by the Na2O concentration in the center of the plate thickness is preferably 2.4 or more. It is more preferably 2.5 or more, further preferably 2.7 or more, and particularly preferably 3.0 or more. By making this value 2.4 or more, the deep stress effective for the drop strength of #80 sandpaper can be efficiently increased, and a high deep compressive stress can be achieved.
[0136] The upper limit of the value obtained by dividing the Na 2 O concentration at a depth of 90 μm from the surface of the chemically strengthened glass of the third embodiment by the Na 2 O concentration at the center of the plate thickness is not particularly limited, but is usually preferably 6.0 or less.
[0137] The chemically strengthened glass of the third embodiment preferably has the same characteristics as those of the chemically strengthened glass of the first embodiment except for the Na 2 O concentration profile.
[0138] <<Applications of chemically strengthened glass>>
[0139] The chemically strengthened glass is also useful as a cover glass used in electronic devices such as mobile phones, portable devices such as smart phones. Furthermore, it is also useful for cover glass of electronic devices such as televisions, personal computers, touch panels, etc. that are not for carrying, elevator walls, houses, buildings and other buildings (full-screen displays). In addition, as building materials such as window glass, interiors of desktops, cars or airplanes, etc. or their cover glasses, in addition, it is also useful for frames with curved shapes.
[0140] <<Main composition of chemically strengthened glass>>
[0141] In this specification, "the mother composition of chemically strengthened glass" refers to the composition of glass before chemical strengthening. This composition will be described later. The composition of the chemically strengthened glass has a composition similar to that of the glass before strengthening as a whole, except when an extreme ion exchange treatment is performed. Usually, the composition of the glass before strengthening is equivalent to the composition of the center of the plate thickness of the chemically strengthened glass. In particular, the composition of the deepest part from the glass surface is the same as the composition of the glass before strengthening, except when an extreme ion exchange treatment is performed.
[0142] The mother composition of the present chemically strengthened glass preferably contains SiO2, Li2O, and Al2O3.
[0143] As one embodiment of the mother composition of the present chemically strengthened glass, it is preferred to contain 52 to 75% SiO2, 3 to 15% Li2O, and 8 to 25% Al2O3, expressed in terms of mole % based on oxides. Hereinafter, the glass of the above composition is referred to as glass X1 .
[0144] As glass X1 , more preferably it contains 55-75% SiO2, 3-15% Li2O, 8-25% Al2O3, 1-5% Na2O, 0-3% K2O, 0-10% MgO, 0-10% CaO, 0-5% SrO, 0-5% ZnO, 0-3% TiO2, 0-3% ZrO2, 0-1% SnO2, 0-1% P2O5, 0-10% B2O3, 0-3% Y2O3, and 0-0.1% Fe2O3.
[0145] As another embodiment of the mother composition of the present chemically strengthened glass, it is preferred to contain 40 to 70% SiO2, 10 to 35% Li2O, and 1 to 15% Al2O3, expressed in terms of mole % based on oxides. Hereinafter, the glass of the above composition is referred to as glass X2 When the chemically strengthened glass is a crystallized glass, the mother composition is preferably glass X2 composition.
[0146] As glass X2 One embodiment, expressed as molar % based on oxides, preferably contains 40-70% SiO2, 10-35% Li2O, 1-15% Al2O3, 0.5-5% P2O5, 0.5-5% ZrO2, 0-10% B2O3, 0-3% Na2O, 0-1% K2O, and 0-4% SnO2.
[0147] As glass X2 Another embodiment, expressed in molar % based on oxides, preferably contains 50-70% SiO2, 15-30% Li2O, 1-10% Al2O3, 0.5-5% P2O5, 0.5-8% ZrO2, 0.1-10% MgO, 0-5% Y2O3, 0-10% B2O3, 0-3% Na2O, 0-1% K2O, and 0-2% SnO2.
[0148] Next, the glass composition will be described.
[0149] SiO2 is a component that constitutes the glass skeleton. It is also a component that improves chemical durability and reduces the occurrence of cracks when the glass surface is scratched.
[0150] Glass X1 In the present invention, the content of SiO2 is 55% or more, preferably 60% or more, more preferably 61% or more, further preferably 62% or more, and particularly preferably 65% or more. On the other hand, from the viewpoint of making the meltability good, the content of SiO2 is 75% or less, preferably 72% or less, more preferably 70% or less, further preferably 67% or less, and particularly preferably 66.5% or less.
[0151] Glass X2 In the embodiment of the present invention, the content of SiO2 is preferably 45% or more. The content of SiO2 is more preferably 48% or more, further preferably 50% or more, particularly preferably 52% or more, and extremely preferably 54% or more. On the other hand, in order to make the meltability good, the content of SiO2 is preferably 70% or less, more preferably 68% or less, further preferably 66% or less, and particularly preferably 64% or less.
[0152] Al2O3 is an effective component from the viewpoint of improving ion exchange performance during chemical strengthening and increasing surface compressive stress after strengthening.
[0153] Glass X1 In the embodiment of the present invention, the content of Al2O3 is 8% or more, preferably 9% or more, more preferably 10% or more, further preferably 11% or more, and particularly preferably 12% or more. On the other hand, if the content of Al2O3 is too much, crystals are easy to grow during melting, and the yield is easily reduced due to devitrification defects. In addition, the viscosity of the glass increases and the solubility decreases. The content of Al2O3 is 25% or less, preferably 22% or less, more preferably 20% or less, further preferably 18% or less, and particularly preferably 16% or less.
[0154] Glass X2 In the embodiment of the present invention, the content of Al2O3 is preferably 1% or more, more preferably 2% or more, further preferably 3% or more, 5% or more, 5.5% or more, 6% or more, particularly preferably 6.5% or more, and most preferably 7% or more. On the other hand, in order to avoid excessively high devitrification temperature of the glass, the content of Al2O3 is preferably 15% or less, more preferably 12% or less, further preferably 10% or less, particularly preferably 9% or less, and most preferably 8% or less.
[0155] Glass X1 In the glass, SiO 2 and Al 2 O 3 are both components that stabilize the glass structure. In order to reduce brittleness, the total content is preferably 65% or more, more preferably 70% or more, and further preferably 75% or more.
[0156] Li2O is a component that forms surface compressive stress by ion exchange and is a component that improves the meltability of glass. By chemically strengthening glass containing Li2O, a stress distribution diagram with large surface compressive stress and compressive stress layer is obtained by exchanging lithium ions on the glass surface with sodium ions and then exchanging sodium ions with potassium ions.
[0157] Glass X1 In view of the ease of obtaining an ideal stress distribution diagram, the content of Li2O is 3% or more, preferably 5% or more, more preferably 7% or more, further preferably 9% or more, particularly preferably 10% or more, and most preferably 11% or more. On the other hand, if the content of Li2O is too much, the crystal growth rate during glass molding increases, and the problem of reduced yield due to devitrification defects increases. The content of Li2O is 15% or less, preferably 14% or less, more preferably 13% or less, and particularly preferably 12% or less.
[0158] Glass X2In the present invention, the content of Li2O is preferably 10% or more, more preferably 14% or more, more preferably 15% or more, further preferably 18% or more, particularly preferably 20% or more, and most preferably 22% or more. On the other hand, in order to stabilize the glass, the content of Li2O is preferably 35% or less, more preferably 32% or less, further preferably 30% or less, particularly preferably 28% or less, and most preferably 26% or less.
[0159] Na2O and K2O are both optional components that improve the solubility of glass and reduce the crystal growth rate of glass. X1 In order to improve the ion exchange performance, the total content of Na2O and K2O, Na2O+K2O, is preferably 2% or more. In addition, Na2O+K2O is preferably 10% or less, preferably 9% or less, more preferably 8% or less, further preferably 7% or less, and particularly preferably 5% or less.
[0160] Na2O is a component that forms a surface compressive stress layer in a chemical strengthening treatment using potassium salt, and is also a component that can improve the solubility of glass.
[0161] Glass X1 In order to obtain this effect, the content of Na2O is 1% or more, preferably 2% or more, more preferably 3% or more, and further preferably 4% or more. On the other hand, from the perspective of avoiding the reduction of surface compressive stress (FSM-CS0) in the strengthening treatment based on sodium salt and achieving CS 90 From the viewpoint of a high profile, it is 5% or less, preferably 4% or less, more preferably 3.5% or less, and further preferably 3% or less.
[0162] Glass composition X2 In the present invention, Na2O is not essential, but when contained, it is preferably 0.5% or more, more preferably 1% or more, and particularly preferably 2% or more. If Na2O is too much, crystals such as Li3PO4 as the main crystal become difficult to precipitate, or the chemical strengthening characteristics are reduced, so the content of Na2O is preferably 10% or less, more preferably 9% or less, further preferably 8% or less, and particularly preferably 7% or less.
[0163] K2O may be contained for the purpose of improving ion exchange performance, etc.
[0164] Glass X1When K2O is contained, the content is preferably 0.1% or more, more preferably 0.15% or more, and particularly preferably 0.2% or more. In order to further prevent devitrification, it is preferably 0.5% or more, more preferably 1.2% or more. On the other hand, since a large amount of K is contained, it becomes an important factor for brittleness and reduction of surface stress due to reverse exchange during strengthening, so it is 3% or less, preferably 2% or less, and more preferably 1% or less.
[0165] Glass composition X2 When K2O is contained, the content is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, and particularly preferably 2% or more. If K2O is too much, the chemical strengthening characteristics are reduced or the chemical durability is reduced, so it is preferably 5% or less, more preferably 4% or less, further preferably 3% or less, particularly preferably 2% or less, and most preferably 1% or less.
[0166] Here, the balance of Li2O, Na2O, and K2O affects the ion exchange performance. X1 In the composition, the value obtained by dividing the content of Li2O by the total content of Li2O, Na2O and K2O, i.e., Li2O / [Li2O+Na2O+K2O], is 0.5 to 0.9. If the value is 0.5 or more, the Li ions in the glass are efficiently exchanged with the Na ions in the molten salt composition. If the value is 0.9 or less, the resistance of the glass can be reduced. Li2O / [Li2O+Na2O+K2O] is preferably 0.55 or more, more preferably 0.60 or more, further preferably 0.65 or more, preferably 0.85 or less, more preferably 0.80 or less, and further preferably 0.75 or less.
[0167] Glass X1 In the embodiment of the present invention, the ratio of the content of Li2O to the content of Na2O, i.e., Li2O / Na2O, is 1.5 to 10. If Li2O / Na2O is 1.5 or more, the Li ions in the glass are efficiently exchanged with the Na ions in the molten salt composition. If Li2O / Na2O is 10 or less, the resistance of the glass can be reduced. Li2O / Na2O is preferably 2 or more, more preferably 4 or more, further preferably 6 or more, preferably 9 or less, more preferably 8 or less, and further preferably 7 or less.
[0168] Glass X2 In order to improve the melting property of glass raw materials, the total content of Na2O and K2O (Na2O+K2O) is preferably 1% or more, more preferably 2% or more. X2In the embodiment, if the ratio K2O / R2O of the K2O content to the total content of Li2O, Na2O and K2O (hereinafter referred to as R2O) is 0.2 or less, the chemical strengthening characteristics can be improved and the chemical durability can be improved, so it is preferred. K2O / R2O is more preferably 0.15 or less, and further preferably 0.10 or less. It should be noted that R2O is preferably 10% or more, more preferably 15% or more, and further preferably 20% or more. In addition, R2O is preferably 29% or less, and more preferably 26% or less.
[0169] MgO may be contained to reduce viscosity during dissolution. When MgO is contained, its content is preferably 1% or more, more preferably 2% or more, and further preferably 3% or more. On the other hand, if the content of MgO is too high, it is difficult to increase the compressive stress layer during chemical strengthening treatment, and the resistance of the glass increases. The content of MgO is 10% or less, preferably 9% or less, more preferably 8% or less, further preferably 7% or less, and particularly preferably 6% or less.
[0170] CaO may be contained in order to reduce viscosity when dissolved. When CaO is contained, its content is preferably 1% or more, more preferably 2% or more, and further preferably 3% or more. On the other hand, if the content of CaO is too much, the resistance of the glass becomes large. The content of CaO is 10% or less, preferably 9% or less, more preferably 8% or less, further preferably 7% or less, and particularly preferably 6% or less.
[0171] SrO may be contained in order to reduce the viscosity when dissolved. When SrO is contained, its content is preferably 0.5% or more, more preferably 1% or more, and further preferably 2% or more. On the other hand, if the content of SrO is too much, the resistance of the glass increases. The content of SrO is 5% or less, preferably 4.5% or less, more preferably 4% or less, further preferably 3.5% or less, and particularly preferably 3% or less.
[0172] When ZnO is contained, its content is preferably 0.5% or more, more preferably 1% or more, and further preferably 2% or more. On the other hand, if the content of ZnO is too much, the thermal expansion coefficient becomes small. The content of ZnO is 5% or less, preferably 4.5% or less, more preferably 4% or less, further preferably 3.5% or less, and particularly preferably 3% or less.
[0173] When TiO2 is contained, its content is preferably 0.05% or more, more preferably 0.1% or more, and further preferably 0.2% or more. On the other hand, if the content of TiO2 is too much, devitrification occurs when the glass is melted. The content of TiO2 is 3% or less, preferably 2.5% or less, more preferably 2% or less, further preferably 1.7% or less, and particularly preferably 1.4% or less.
[0174] Although ZrO2 may not be contained, it is preferably contained from the viewpoint of increasing the surface compressive stress of chemically strengthened glass. When ZrO2 is contained, its content is preferably 0.1% or more, more preferably 0.15% or more, further preferably 0.2% or more, particularly preferably 0.25% or more, and typically 0.3% or more. On the other hand, if the content of ZrO2 is too high, devitrification defects are likely to occur, and it is not easy to increase the compressive stress value during chemical strengthening treatment. The content of ZrO2 is 3% or less, preferably 2% or less, more preferably 1.5% or less, further preferably 1% or less, and particularly preferably 0.8% or less.
[0175] SnO2 can be contained as a clarifier during glass manufacturing. When SnO2 is contained, its content is preferably 0.02% or more, more preferably 0.05% or more, and further preferably 0.1% or more. On the other hand, if the content of SnO2 is too much, the color tone may be affected. The content of SnO2 is 1% or less, preferably 0.5% or less, more preferably 0.3% or less, further preferably 0.2% or less, and particularly preferably 0.1% or less.
[0176] Glass X1 In order to increase the compressive stress layer based on chemical strengthening, P2O5 may be contained. When P2O5 is contained, its content is preferably 0.1% or more, more preferably 0.2% or more, and further preferably 0.3% or more. On the other hand, if the content of P2O5 is too much, the durability to acid and alkali is reduced. The content of P2O5 is 1% or less, preferably 0.8% or less, more preferably 0.7% or less, further preferably 0.6% or less, and particularly preferably 0.5% or less.
[0177] Glass X2 In the embodiment of the present invention, P2O5 is a constituent component of Li3PO4 crystals and is essential. In order to promote crystallization, the content of P2O5 is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, particularly preferably 2% or more, and extremely preferably 2.5% or more. On the other hand, if the content of P2O5 is too high, phase separation is easy during melting, and the acid resistance is significantly reduced. Therefore, the content of P2O5 is preferably 5% or less, more preferably 4.8% or less, further preferably 4.5% or less, and particularly preferably 4.2% or less.
[0178] Glass X2 Among them, SiO2, Al2O3, P2O5 and B2O3 are the network forming components of glass (hereinafter also abbreviated as NWF). The strength of crystallized glass is increased by the large total amount of NWF. This increases the fracture toughness value of crystallized glass. From the above point of view, glass X2The total amount of NWF is preferably 60% or more, more preferably 63% or more, and particularly preferably 65% or more. However, since too much NWF increases the melting temperature of the glass and makes it difficult to manufacture, it is preferably 85% or less, more preferably 80% or less, and more preferably 75% or less.
[0179] Glass X2 In the present invention, the ratio of the total amount of Li2O, Na2O and K2O to the total amount of NWF, i.e., SiO2, Al2O3, P2O5 and B2O3, is preferably 0.20 to 0.60. Li2O, Na2O and K2O are mesh modification components, and reducing the ratio relative to NWF will increase the gaps in the network, thereby improving impact resistance. Therefore, the ratio of the total amount of Li2O, Na2O and K2O to NWF is preferably 0.60 or less, more preferably 0.55 or less, and particularly preferably 0.50 or less. On the other hand, these are the components required for chemical strengthening, so in order to improve the chemical strengthening properties, the ratio of the total amount of Li2O, Na2O and K2O to NWF is preferably 0.20 or more, more preferably 0.25 or more, and particularly preferably 0.30 or more.
[0180] B2O3 may be contained in order to improve the scratch resistance of the glass. When B2O3 is contained, its content is preferably 1% or more, more preferably 3% or more, and further preferably 5% or more. On the other hand, if the content of B2O3 is too much, ribs will be generated during melting, or phase separation will be easy to cause the quality of the chemically strengthened glass to be easily reduced. The content of B2O3 is 10% or less, preferably 9.5% or less, more preferably 9% or less, further preferably 8.5% or less, and particularly preferably 8% or less.
[0181] Glass X1 The preferred B2O3 / P2O5 ratio is 2.5 to 500. When B2O3 / P2O5 is 2.5 or more, the glass is prevented from generating ribs when it is melted, and stable production is possible. B2O3 / P2O5 is more preferably 5 or more, further preferably 10 or more, and particularly preferably 50 or more. When B2O3 / P2O5 is 500 or less, ion exchange is easy to carry out, and the glass is not easy to be scratched. B2O3 / P2O5 is more preferably 450 or less, further preferably 400 or less, particularly preferably 300 or less, and most preferably 250 or less.
[0182] Y2O3 may be contained in order to improve the fracture toughness value of the glass. When Y2O3 is contained, its content is preferably 0.1% or more, more preferably 0.2% or more, further preferably 0.5% or more, and particularly preferably 1% or more. On the other hand, if it is too much, it is not easy to increase the compressive stress layer during chemical strengthening treatment. The content of Y2O3 is 3% or less, preferably 2.5% or less, more preferably 2% or less, and further preferably 1.5% or less.
[0183] Fe2O3 may be contained in order to reduce the resistance of the glass. When Fe2O3 is contained, its content is preferably 0.01% or more, more preferably 0.02% or more, and further preferably 0.04% or more. On the other hand, if the content of Fe2O3 is too much, the glass will become colored, which will damage the commercial value of the cover glass for electronic devices. The content of Fe2O3 is 0.1% or less, preferably 0.09% or less, more preferably 0.08% or less, further preferably 0.07% or less, and particularly preferably 0.06% or less.
[0184] BaO, SrO, MgO, CaO, and ZnO are components that improve the solubility of glass and may be contained.
[0185] Among them, BaO, SrO, and ZnO can be contained in the glass in order to increase the refractive index of the residual glass and make it close to the precipitated crystal phase, thereby increasing the light transmittance of the crystallized glass and reducing the haze value. X2 In this case, the total content of BaO, SrO and ZnO (hereinafter referred to as BaO+SrO+ZnO) is preferably 0.3% or more, more preferably 0.5% or more, further preferably 0.7% or more, and particularly preferably 1% or more. On the other hand, these components sometimes reduce the ion exchange rate. In order to make the chemical strengthening characteristics good, BaO+SrO+ZnO is preferably 2.5% or less, more preferably 2% or less, further preferably 1.7% or less, and particularly preferably 1.5% or less.
[0186] La2O3, Nb2O5 and Ta2O5 are all components that make it difficult for fragments to fly when chemically strengthened glass breaks, and they can be contained to increase the refractive index. When these components are contained, the total content of La2O3, Nb2O5 and Ta2O5 (hereinafter referred to as La2O3+Nb2O5+Ta2O5) is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, and particularly preferably 2% or more. In addition, in order to make the glass less likely to lose clarity during melting, La2O3+Nb2O5+Ta2O5 is preferably 4% or less, more preferably 3% or less, further preferably 2% or less, and particularly preferably 1% or less.
[0187] In addition, CeO2 may be contained. CeO2 sometimes suppresses coloration by oxidizing the glass. When CeO2 is contained, the content is preferably 0.03% or more, more preferably 0.05% or more, and further preferably 0.07% or more. In order to improve transparency, the content of CeO2 is preferably 1.5% or less, and more preferably 1.0% or less.
[0188] When chemically strengthened glass is colored for use, a coloring component may be added within a range that does not hinder the realization of the desired chemically strengthened properties. Examples of coloring components include Co3O4, MnO2, Fe2O3, NiO, CuO, Cr2O3, V2O5, Bi2O3, SeO2, Er2O3, and Nd2O3.
[0189] The content of the coloring components is preferably within a range of 1% or less in total. In order to further increase the visible light transmittance of the glass, it is preferred that these components are substantially not contained.
[0190] In order to improve the weather resistance to ultraviolet light, HfO2, Nb2O5, and Ti2O3 can be added. When added for the purpose of improving the weather resistance to ultraviolet light, in order to suppress the influence on other properties, the total content of HfO2, Nb2O5, and Ti2O3 is preferably 1% or less, more preferably 0.5% or less, and more preferably 0.1% or less.
[0191] In addition, as a clarifier during glass melting, SO3, chloride, and fluoride may be appropriately contained. If added in excess, the strengthening characteristics and crystallization behavior are affected, so the total content of the components that function as clarifiers is preferably 2% or less, more preferably 1% or less, and further preferably 0.5% or less, expressed in mass % based on oxides. The lower limit is not particularly limited, but typically, it is preferably 0.05% or more in total, expressed in mass % based on oxides.
[0192] When SO3 is used as a clarifier, if the content of SO3 is too small, no effect can be seen, so it is preferably 0.01% or more, more preferably 0.05% or more, and further preferably 0.1% or more, expressed as mass % based on oxides. In addition, when SO3 is used as a clarifier, the content of SO3 is preferably 1% or less, more preferably 0.8% or less, and further preferably 0.6% or less, expressed as mass % based on oxides.
[0193] If added in excessive amount, physical properties such as strengthening characteristics are affected, so when Cl is used as a clarifier, the Cl content is preferably 1% or less, more preferably 0.8% or less, and further preferably 0.6% or less, expressed in mass % based on oxides. On the other hand, if it is too little, no effect is observed, so when Cl is used as a clarifier, the Cl content is preferably 0.05% or more, more preferably 0.1% or more, and further preferably 0.2% or more, expressed in mass % based on oxides.
[0194] If added in excess, the crystallization behavior is affected, so when SnO2 is used as a clarifier, the content of SnO2 is preferably 1% or less, more preferably 0.5% or less, and further preferably 0.3% or less, expressed in mass % based on the oxide. In addition, if it is too little, no effect can be seen, so when SnO2 is used as a clarifier, the content of SnO2 is preferably 0.02% or more, more preferably 0.05% or more, and further preferably 0.1% or more, expressed in mass % based on the oxide.
[0195] It is preferred that As2O3 is not contained. It may contain impurities such as Sb2O3 as a trace component. When Sb2O3 is contained, it is preferably 0.3% or less, more preferably 0.1% or less, and most preferably not contained.
[0196] As the mother composition of the present chemically strengthened glass, specifically, for example, a glass having the following compositions (i) to (iii) is preferable.
[0197] (i) Glass containing 66% SiO2, 11% Li2O, 11% Al2O3, 5.5% Na2O, 1.5% K2O, 1.3% ZrO2, 3% MgO, 0.5% Y2O3, and 0.3% of other components.
[0198] (ii) Glass containing 68% SiO2, 11% Li2O, 12% Al2O3, 1.6% Na2O, 1.6% K2O, 0.6% ZrO2, 1.4% Y2O3, 3.5% MgO, and 0.3% of other components.
[0199] (iii) Glass containing 57% SiO2, 11% Li2O, 18% Al2O3, 3% Na2O, 0.5% K2O, 0.5% P2O5, 6% B2O3, and 4.5% MgO.
[0200] The mother composition of the chemically strengthened glass of the present invention including the first to third embodiments is more preferably the same as the composition described later in the section <Glass: Sixth Embodiment>.
[0201] <<Directional drop strength>>
[0202] The #80 drop strength of the chemically strengthened glass of the present embodiment is preferably 40 cm or more, more preferably 42 cm or more, further preferably 43 cm or more, and particularly preferably 45 cm or more.
[0203] <<4-point bending strength>>
[0204] The four-point bending strength of the chemically strengthened glass of the present embodiment is preferably 550 MPa or more, more preferably 600 MPa or more, further preferably 700 MPa or more, particularly preferably 750 MPa or more.
[0205] <Method for producing chemically strengthened glass: Fourth and fifth embodiments>
[0206] Hereinafter, as specific embodiments of the method for producing chemically strengthened glass according to the present invention, the fourth embodiment and the fifth embodiment are described. In this specification, the method for producing chemically strengthened glass according to the present invention including the fourth embodiment and the fifth embodiment is also abbreviated as "this production method".
[0207] [Method for producing chemically strengthened glass according to fourth embodiment]
[0208] A method for producing a chemically strengthened glass according to a fourth embodiment of the present invention is characterized in that the method comprises at least a first ion exchange treatment of bringing a chemically strengthened glass into contact with a first molten salt composition, and a second ion exchange treatment of bringing the chemically strengthened glass into contact with a second molten salt composition after the first ion exchange treatment, wherein in the first ion exchange treatment, the chemically strengthened glass is brought into contact with the first molten salt composition at 350 to 450° C. for 150 minutes or more, and the chemically strengthened glass contains, in terms of mol % based on oxides, 55 to 75% of SiO 2 , 3 to 15% of Li 2 O, and 8 to 25% of Al 2 O 3 .
[0209] [Method for producing chemically strengthened glass according to the fifth embodiment]
[0210] The method for producing a chemically strengthened glass according to a fifth embodiment of the present invention is characterized in that it includes at least a first ion exchange treatment of bringing a chemically strengthened glass into contact with a first molten salt composition, and a second ion exchange treatment of bringing the chemically strengthened glass into contact with a second molten salt composition after the first ion exchange treatment, wherein the first ion exchange treatment is performed at 350 to 450° C. for 150 minutes or more, the first molten salt composition contains Li ions, and the chemically strengthened glass contains 55 to 75% of SiO 2 , 3 to 15% of Li 2 O, and 8 to 25% of Al 2 O 3 in terms of mol % based on oxides.
[0211] <<Chemically strengthened glass>>
[0212] As one embodiment of the chemically strengthened glass of the present embodiment, 55 to 75% of SiO2, 3 to 15% of Li2O, and 8 to 25% of Al2O3 are contained in terms of mole % based on oxides. As another embodiment of the chemically strengthened glass of the present embodiment, 40 to 70% of SiO2, 10 to 35% of Li2O, and 1 to 15% of Al2O3 are contained in terms of mole % based on oxides. The chemically strengthened glass preferably has the composition described in the item <<Mother composition of chemically strengthened glass>>, and more preferably has the composition described later in the item <Glass: 6th embodiment>. Glass raw materials are appropriately blended in such a manner as to obtain glass of the composition, and are heated and melted in a glass melting furnace. Then, the glass is homogenized by bubbling, stirring, adding a clarifier, etc., and is formed into a glass plate of a specified thickness and slowly cooled. Alternatively, it can be formed into a plate by forming it into a block and cutting it after slowly cooling.
[0213] As a method for forming into a plate, for example, a float process, a press process, a fusion process and a down-draw process can be cited. In particular, when manufacturing a large glass plate, the float process is preferred. In addition, continuous forming methods other than the float process, such as a fusion process and a down-draw process, are also preferred.
[0214] The chemically strengthened glass may also be a crystallized glass. In the case of a crystallized glass, a crystallized glass containing one or more crystals selected from lithium silicate crystals, lithium aluminosilicate crystals, and lithium phosphate crystals is preferred. As lithium silicate crystals, lithium metasilicate crystals, lithium disilicate crystals, etc. are preferred. As lithium phosphate crystals, lithium orthophosphate crystals, etc. are preferred. As lithium aluminosilicate crystals, β-spodumene crystals, petalite crystals, etc. are preferred.
[0215] In order to improve mechanical strength, the crystallization rate of crystallized glass is preferably more than 10%, more preferably more than 15%, further preferably more than 20%, and particularly preferably more than 25%. In addition, in order to improve transparency, it is preferably less than 70%, more preferably less than 60%, and particularly preferably less than 50%. The low crystallization rate is also excellent from the aspects of heating and easy bending molding. The crystallization rate can be calculated using the Rietveld method according to the X-ray diffraction intensity. The Rietveld method is recorded in the "Crystallization Analysis Handbook" Editorial Committee of the Japanese Society of Crystallization, "Crystallization Analysis Handbook" (Kyori Publishing 1999 Annual, p492~499).
[0216] In order to improve transparency, the average particle size of the precipitated crystals of sintered glass is preferably below 300nm, more preferably below 200nm, further preferably below 150nm, and particularly preferably below 100nm. The average particle size of the precipitated crystals can be obtained according to transmission electron microscope (TEM) image. In addition, it can be inferred according to scanning electron microscope (SEM) image.
[0217] <<Chemical strengthening treatment>>
[0218] Chemical strengthening treatment is a treatment in which the glass is brought into contact with a metal salt by immersing the glass in a melt of a metal salt (e.g., potassium nitrate) containing metal ions with a large ionic radius (typically Na ions or K ions), thereby replacing the metal ions with a small ionic radius (typically Na ions or K ions relative to Li ions, and K ions relative to Na ions) in the glass.
[0219] As the molten salt for chemical strengthening treatment, for example, nitrates, sulfates, carbonates, chlorides, etc. can be mentioned. As nitrates therein, for example, lithium nitrate, sodium nitrate, potassium nitrate, cesium nitrate, silver nitrate, etc. can be mentioned. As sulfates, for example, lithium sulfate, sodium sulfate, potassium sulfate, cesium sulfate, silver sulfate, etc. can be mentioned. As carbonates, for example, lithium carbonate, sodium carbonate, potassium carbonate, etc. can be mentioned. As chlorides, for example, lithium chloride, sodium chloride, potassium chloride, cesium chloride, silver chloride, etc. can be mentioned. These molten salts can be used alone or in combination.
[0220] The molten salt composition preferably contains nitrate as a main component, and more preferably contains sodium nitrate or potassium nitrate as a main component. Here, "as a main component" means that the content in the molten salt composition is 80% by mass or more.
[0221] The present production method is characterized by sequentially including the following first ion exchange treatment and second ion exchange treatment.
[0222] (First ion exchange treatment) A step of bringing the chemically strengthened glass into contact with a first molten salt composition.
[0223] (Second ion exchange treatment) A step of bringing the chemically strengthened glass into contact with a second molten salt composition after the first ion exchange treatment.
[0224] In one embodiment of the present manufacturing method, in the first ion exchange treatment, the chemically strengthened glass preferably contains a first alkali metal ion, and the first molten salt composition preferably contains a second alkali metal ion having an ionic radius larger than that of the first alkali metal ion. In addition, in the second ion exchange treatment, the second molten salt composition preferably contains a third alkali metal ion having an ionic radius larger than that of the second alkali metal ion. The second molten salt composition more preferably further contains the first alkali metal ion.
[0225] In this embodiment, the first alkali metal ions in the chemically strengthened glass are exchanged with the second alkali metal ions in the first molten salt composition by the first ion exchange treatment. In addition, in the second ion exchange treatment, the second alkali metal ions in the chemically strengthened glass are exchanged with the third alkali metal ions in the second molten salt composition.
[0226] Figure 2 Schematic diagrams for explaining ion exchange in this embodiment are shown in (a) and (b). In this embodiment, the first alkali metal ion is a lithium (Li) ion, the second alkali metal ion is a sodium (Na) ion, and the third alkali metal ion is a potassium (K) ion.
[0227] Figure 2 (a) represents the first ion exchange treatment, Figure 2 (b) represents the second ion exchange treatment.
[0228] The following ion movement occurs in the first ion exchange treatment.
[0229] 1-1) The second alkali metal ions are introduced into the glass by ion exchange between the first alkali metal ions in the chemically strengthened glass and the second alkali metal ions in the first molten salt composition.
[0230] 1-2) Ion exchange of the second alkali metal ions introduced into the chemically strengthened glass by the ion exchange of 1-1) above with the first alkali metal ions in the first molten salt composition [reverse ion exchange, Figure 2 A in (a)] causes the second alkali metal ion to be separated from the glass.
[0231] Thus, the excess second alkali metal ions in the glass surface layer are reduced, and the tensile stress can be controlled to be less than the CT limit value.
[0232] 1-3) The second alkali metal ions diffuse from the glass surface to a depth of about 18% of the preferred plate thickness. Figure 2 Thus, the CS can be increased in the first ion exchange treatment stage. 90 .
[0233] The following ion movement occurs in the second ion exchange treatment.
[0234] 2-1) The third alkali metal ions in the second molten salt composition are introduced into the surface layer of the glass by exchanging the third alkali metal ions in the second molten salt composition with the second alkali metal ions in the chemically strengthened glass. Thus, the surface compressive stress of the glass can be increased. Figure 2 (b) in C].
[0235] 2-2) The second alkali metal ions diffused into the glass in 1-3) above diffuse into the deep layer of the glass. This can improve CS 90 .
[0236] Through the above ion movement, Figure 2 As shown in (b), for example, the second alkali metal ions are reduced in the region from a depth of about 3.3 μm from the surface to a depth of about 80 to 90 μm from the surface to reduce the compressive stress, and the CS of the region deeper than 90 μm from the surface is kept higher, thereby forming a stress distribution diagram with high surface compressive stress.
[0237] Hereinafter, each ion exchange treatment in the present production method will be described in detail.
[0238] <<First ion exchange treatment>>
[0239] The first ion exchange treatment is a process of contacting the chemically strengthened glass with the first molten salt composition. In this embodiment, the temperature and time in the first ion exchange treatment are preferably set by observing the saturation behavior of the compressive stress layer depth DOC accompanying the progress of the first ion exchange time. Specifically, for example, in the first ion exchange treatment, when the plate thickness is set to t (mm), the temperature and time are preferably set in a manner that the compressive stress layer depth DOC exceeds 180×t (μm). By making DOC exceed 180×t, CS can be further improved. 90 .
[0240] In one embodiment, the temperature at which the first molten salt composition is brought into contact with the chemically strengthened glass in the first ion exchange treatment is preferably 350° C. or higher, more preferably 360° C. or higher, and even more preferably 380° C. or higher. If the temperature of the first molten salt composition is 350° C. or higher, reverse ion exchange occurs sufficiently, the stress in the glass surface layer is weakened, and the compressive stress layer is easily introduced to a depth of about 18% of the plate thickness, which makes it easy to increase the CS 90 In addition, from the viewpoint of danger due to evaporation and composition change of the molten salt, the temperature of the first molten salt composition is usually 450° C. or lower.
[0241] In the first ion exchange treatment, when the first molten salt composition is in contact with the chemically strengthened glass for 150 minutes or more, reverse ion exchange occurs sufficiently, the stress in the glass surface layer is weakened, and a compressive stress layer is easily introduced to a depth of about 18% of the plate thickness, thereby easily improving CS. 90 The time is more preferably 180 minutes or longer, and even more preferably 210 minutes or longer.
[0242] Specifically, for example, when the temperature of the first molten salt composition in contact with the chemically strengthened glass is 420° C., the contact time is preferably 360 to 660 minutes. When the temperature of the first molten salt composition in contact with the chemically strengthened glass exceeds 420° C., the contact time is preferably 600 minutes or less.
[0243] In one embodiment, in the first ion exchange treatment, the time t1 (minutes) for immersing the chemically strengthened glass in the first molten salt composition at the temperature T (°C) of the first molten salt composition preferably satisfies the following formula. 90 maximize.
[0244] -7.5T+3400<t1<-7.5T+3850
[0245] t1 (minutes) is preferably greater than (-7.5T+3400), more preferably greater than (-7.5T+3500), and even more preferably greater than (-7.5T+3550). In addition, t1 (minutes) is preferably less than (-7.5T+3850), more preferably less than (-7.5T+3800), and even more preferably less than (-7.5T+3700).
[0246] In the fourth embodiment, the first molten salt composition preferably contains lithium ions. In the fifth embodiment, the first molten salt composition contains lithium ions. The content of lithium ions in the first molten salt composition can be set, for example, as follows. When the temperature and time are determined according to the saturation behavior of the DOC accompanying the progress of the first ion exchange, the simulation can make the concentration of lithium ions that makes the number of fragments when damaged below the CT limit. The lithium ion concentration contained in the first molten salt composition can be set according to this concentration.
[0247] In one embodiment, the content of lithium ions in the first molten salt composition is preferably 0.010% by mass or more, more preferably 0.060% by mass or more, and further preferably 0.15% by mass or more. If the content of lithium ions in the first molten salt composition is 0.010% by mass or more, reverse ion exchange is fully promoted, surface compressive stress can be reduced, internal tensile stress can be further suppressed, and the number of fractures when damaged is easily made to be below the CT limit. The lithium ions in the molten salt composition are combined with SiO2 in the glass component, and it is possible to produce a poor appearance of crystallinity, so the content of lithium in the first molten salt composition is preferably 1.0% by mass or less, more preferably 0.80% by mass or less, and further preferably 0.60% by mass or less.
[0248] In one embodiment, the content of sodium nitrate in the first molten salt composition is preferably 92% by mass or more, more preferably 92.5% by mass or more, 93.0% by mass or more, 93.5% by mass or more, and further preferably 94% by mass or more. If the content of sodium nitrate is within the above range, the amount of sodium introduced into the deep part of the glass can be increased, and the CS can be further improved. 90 .
[0249] In one embodiment, when potassium nitrate is added to the first molten salt composition, its content is preferably 35% by mass or less, and more preferably 25% by mass or less, 15% by mass or less, and 5% by mass or less in the following order. If the content of potassium nitrate is within the above range, it is easy to fully introduce sodium ions into the deep layer of the glass.
[0250] <<Second ion exchange treatment>>
[0251] This is a step of bringing the chemically strengthened glass into contact with the second molten salt composition after the first ion exchange treatment. In this embodiment, it is preferred to measure the surface ion concentration of the chemically strengthened glass after the first ion exchange treatment to obtain the Na / Li ratio, and determine the Na / Li ratio in the second molten salt composition based on the Na / Li ratio.
[0252] In one embodiment, the temperature and time of the second ion exchange treatment are preferably set so that the value of the surface compressive stress layer depth DOL-tail is 3.3 μm or more. When DOL-tail is 3.3 μm or more, the bending strength can be further improved, and mass production is facilitated.
[0253] In one embodiment, the chemically strengthened glass is preferably immersed in a second molten salt composition preferably at a temperature of 420° C. or higher. The temperature of the second molten salt composition is more preferably 422° C. or higher, and further preferably 425° C. or higher. In addition, from the viewpoint of the danger caused by evaporation and the composition change of the molten salt, the temperature of the second molten salt composition is usually 450° C. or lower, and from the viewpoint of preventing excessive reduction of stress, it is more preferably 435° C. or lower.
[0254] In one embodiment, the time for which the second molten salt composition is in contact with the chemically strengthened glass is preferably 0.5 hours or more, more preferably 0.75 hours or more, and even more preferably 1 hour or more. By making the time 0.5 hours or more, the compressive stress is further reduced in the region up to a depth of about 80 to 90 μm from the surface, and the CS in the region deeper than 90 μm from the surface can be kept higher. On the other hand, if the contact time is too long, the CS 50 Therefore, it is usually preferably 4 hours or less.
[0255] Specifically, for example, when the temperature of the second molten salt composition in contact with the chemically strengthened glass is 420° C., the contact time is preferably 0.5 to 2 hours, more preferably 0.5 to 1.75 hours, and even more preferably 0.5 to 1.5 hours.
[0256] In one embodiment, in the second ion exchange treatment, the time t2 (minutes) for immersing the chemically strengthened glass in the second molten salt composition at the temperature T (° C.) of the second molten salt composition preferably satisfies the following formula: Thus, the value of the surface compressive stress layer depth DOL-tail is easily 3.3 μm or more.
[0257] -1×T+450<t2<-4×T+1740
[0258] t2 (minutes) is preferably greater than (-1×T+450), more preferably greater than (-1×T+455), and even more preferably greater than (-1×T+460). In addition, t2 (minutes) is preferably less than (-4×T+1740), more preferably less than (-4×T+1735), and even more preferably less than (-4×T+1730).
[0259] In this embodiment, the second molten salt composition preferably contains 0% to 5% by mass of lithium nitrate. By making the content of lithium nitrate in the second molten salt composition 0% to 5% by mass, potassium can be used to fully introduce stress into the surface layer, increase the surface compressive stress, and further improve the bending strength.
[0260] In one embodiment, the content of potassium nitrate in the second molten salt composition is preferably 90% by mass or more, more preferably 92% by mass or more, and further preferably 95% by mass or more. The upper limit is not particularly limited, but is usually 99.9% by mass or less.
[0261] The second molten salt composition may contain sodium nitrate. When the second molten salt composition contains sodium nitrate, its content is preferably 0.1 mass % or more, and more preferably 0.3 mass % or more. If the content of sodium nitrate is within the above range, the CS 90 The effect is improved.
[0262] The second molten salt composition may further contain additives other than nitrates. As additives, for example, silicic acid, specific inorganic salts, etc. can be cited. By having the additives in the second molten salt composition, FSM-CS0 can be increased.
[0263] The second molten salt composition may contain silicic acid as an additive. Silicic acid refers to a compound composed of silicon, hydrogen, and oxygen represented by the chemical formula nSiO2·xH2O. Here, n and x are natural numbers. As one of such silicic acids, for example, metasilicic acid (SiO2·H2O), disiliic acid (2SiO2·H2O), orthosilicic acid (SiO2·2H2O), pyrosiliconic acid (2SiO2·3H2O), silica gel [SiO2·mH2O (m is a real number of 0.1 to 1)] and the like can be cited.
[0264] By including silicate, the silicate adsorbs lithium ions, and potassium ions easily enter the glass. For this reason, the stress of the surface layer of several μm can be increased while suppressing CT. The amount of silicate added is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, and most preferably 0.5 mass% or more. In addition, the amount of silicate added is preferably 3 mass% or less, more preferably 2 mass% or less, and most preferably 1 mass% or less.
[0265] Silicic acid is preferably silica gel [SiO2·mH2O (m is a real number of 0.1 to 1)]. Silica gel has the advantage of being easy to settle in the molten salt and easy to put in or recover because the secondary particles are large. In addition, there is no concern about flying dust, and the safety of the operator can be ensured. Furthermore, since it is a porous body, it is easy to supply molten salt to the surface of the primary particles, so it has excellent reactivity and a large effect of adsorbing lithium ions.
[0266] The second molten salt composition may also contain a specific inorganic salt (hereinafter referred to as flux) as an additive. As the flux, carbonate, bicarbonate, phosphate, sulfate, hydroxide, chloride are preferred, preferably containing at least one salt selected from K2CO3, Na2CO3, KHCO3, NaHCO3, K3PO4, Na3PO4, K2SO4, Na2SO4, KOH, NaOH, KCl, NaCl, more preferably containing at least one salt selected from K2CO3, Na2CO3, and further preferably K2CO3.
[0267] The chemical strengthening treatment may be an ion exchange treatment of more than two stages. In the present embodiment, when the ion exchange treatment is performed in three stages, the conditions of the ion exchange treatment (eg, the composition, temperature and time of the molten salt composition) are preferably set in a manner such that the surface compressive stress is 1000 MPa or more in the third ion exchange treatment.
[0268] When the third ion exchange treatment is performed after the second ion exchange treatment in which the chemically strengthened glass is brought into contact with the third molten salt composition, the third molten salt composition preferably contains 98% by mass or more of potassium nitrate, more preferably 98.5% by mass or more, and even more preferably 99% by mass or more. By making the content of potassium nitrate in the third molten salt composition 98% by mass or more, the CS 90 .
[0269] In the present embodiment, when two or more stages of ion exchange are performed, it is preferred that CTave of the chemically strengthened glass after the first ion exchange treatment is larger than CTA, and CTave is made smaller than CTA by the second and subsequent ion exchange treatments.
[0270] The CT limit is obtained by the following formula (1). CTA is equivalent to the CT limit and is a value determined by the composition of the chemically strengthened glass. In addition, CTave is a value equivalent to the average value of the tensile stress, and CTave is obtained by the following formula (2). If CTave<CTA, it is lower than the CT limit, and the rapid increase in the number of fractures when damaged can be suppressed.
[0271]
[0272] t: Plate thickness (mm)
[0273] K1c: Fracture toughness value (MPa·m 1 / 2 )
[0274] CTave=ICT / LCT…Formula (2)
[0275] ICT: Integrated value of tensile stress (Pa·m)
[0276] LCT: Length of the tensile stress region in the plate thickness direction (μm)
[0277] If a compressive stress layer is formed on the surface of a glass article by chemical strengthening treatment, a tensile stress corresponding to the total amount of compressive stress on the surface will inevitably be generated in the center of the glass article. If the tensile stress value becomes too large, the glass article will break violently and cause fragments to fly. If the CT exceeds the CT limit, which is its threshold, the number of fractures when damaged increases sharply. In the present embodiment, when two or more stages of ion exchange are performed, the maximum tensile stress value of the stress distribution diagram formed inside the glass by the initial ion exchange treatment (the first ion exchange treatment) is preferably greater than the CT limit. The maximum tensile stress value after the first ion exchange treatment is greater than the CT limit, so that the compressive stress is fully introduced by the first ion exchange treatment, and in the subsequent second ion exchange treatment, the stress value of the surface layer of the glass is reduced and the CS can be maintained. 90 Higher.
[0278] <Glass: Sixth Embodiment>
[0279] The glass according to the sixth embodiment of the present invention is characterized in that, expressed in terms of mol % based on oxides, it contains 55 to 75% of SiO2, 8 to 25% of Al2O3, 3 to 15% of Li2O, 1 to 5% of Na2O, 0 to 3% of K2O, 0 to 10% of MgO, 0 to 10% of CaO, 0 to 5% of SrO, 0 to 5% of ZnO, 0 to 3% of TiO2, 0 to 3% of ZrO2, 0 to 1% of S nO2, 0-1% P2O5, 0-10% B2O3, 0-3% Y2O3, 0-0.1% Fe2O3, the ratio of Li2O content to the total content of Li2O, Na2O and K2O, i.e. Li2O / [Li2O+Na2O+K2O] is 0.5-0.9, the ratio of Li2O content to Na2O content, i.e. Li2O / Na2O is 1.5-10, and the Young's modulus is above 80 GPa.
[0280] Each composition is the same as that described in the section "Main composition of chemically strengthened glass" in the third embodiment.
[0281] The glass of this embodiment has the above composition. Glass raw materials are appropriately prepared in a manner to obtain the glass of the above composition, and heated and melted in a glass melting furnace. Then, the glass is homogenized by bubbling, stirring, adding a clarifier, etc., and formed into a glass plate of a specified thickness, and slowly cooled. Alternatively, it can be formed into a plate by forming it into a block and cutting it after slowly cooling.
[0282] As a method for forming into a plate, for example, a float process, a press process, a fusion process and a down-draw process can be cited. In particular, when manufacturing a large glass plate, the float process is preferred. In addition, continuous forming methods other than the float process, such as a fusion process and a down-draw process, are also preferred.
[0283] The glass of the present embodiment may be crystallized glass. The crystallized glass is the same as the crystallized glass described in the section "Chemically Strengthened Glass".
[0284] The Young's modulus of the glass of the present embodiment is preferably 80 GPa or more, more preferably 82 GPa or more, further preferably 84 GPa or more, and particularly preferably 85 GPa or more. When the Young's modulus is 80 GPa or more, a higher CTA can be achieved during chemical strengthening, and deep stress can be increased. The upper limit of the Young's modulus is not particularly limited, but from the viewpoint of the processability of the glass, it is usually 100 GPa or less, preferably 95 GPa or less, and more preferably 90 GPa or less.
[0285] When the glass of the present embodiment is subjected to an ion exchange treatment using a molten salt composed of sodium nitrate at 380° C. for 4 hours to form a compressive stress layer, the compressive stress value CS at a depth of 30 μm from the surface of the compressive stress layer is 30 It is preferably 150MPa or more. 30 The CS value is 150 MPa or more, which makes it easy to increase the CTA by ion exchange treatment, and the deep compressive stress can be further increased by reducing the surface compressive stress and suppressing the internal tensile stress. 30 It is preferably 160 MPa or more, more preferably 170 MPa or more, and further preferably 180 MPa or more.
[0286] Example
[0287] Hereinafter, the present invention will be described based on examples, but the present invention is not limited thereto.
[0288] <Evaluation of amorphous glass>
[0289] (Young's modulus E)
[0290] The measurement was carried out by ultrasonic method.
[0291] (Fracture toughness value K1c)
[0292] Fracture toughness value K1c (unit: MPa·m 1 / 2 ) was measured by IF method according to JIS R1607:2015.
[0293] [CTA value]
[0294] The CTA value is calculated by the following formula (1).
[0295]
[0296] t: Plate thickness (mm)
[0297] Table 1 shows the composition and evaluation results of the glass used in the test examples described below.
[0298] [Table 1]
[0299]
[0300] <Evaluation of chemically strengthened glass>
[0301] The evaluation method of chemically strengthened glass is described below.
[0302] (EPMA)
[0303] The measurement was performed by EPMA as follows. First, the glass sample was embedded with epoxy resin and mechanically ground in a direction perpendicular to the first main surface and the second main surface opposite to the first main surface to prepare a cross-sectional sample. The ground cross-section was carbon coated and measured using EPMA (manufactured by JEOL: JXA-8500F). The acceleration voltage was 15 kV, the probe current was 30 nA, the accumulation time was 1000 msec. / point, and a linear distribution diagram of the X-ray intensity of Na was obtained at 1 μm intervals.
[0304] (Stress distribution diagram)
[0305] The stress distribution diagram was measured using a scattered light photoelastic stress meter SLP-2000 and a glass surface stress meter FSM manufactured by Orihara Corporation.
[0306] (Surface resistivity)
[0307] (1) Sample preparation and film formation process
[0308] The glass sample used was a glass sample of 120×60×0.7 mm. Film formation was performed according to the following procedure before the surface resistivity measurement. A sputtering device was used to form a film on a glass sample of 120×60×0.7 mm. Platinum was formed on the glass surface. During film formation, patterning was performed in accordance with JISR3256:1998.
[0309] (2) Surface resistivity measurement
[0310] The surface resistivity is measured by the following method.
[0311] As the measuring device, an ultra-micro ammeter 5450 was used.
[0312] As the glass sample, a glass sample of 120×60×0.7 mm was used.
[0313] The measurement was performed by a three-terminal method in accordance with JIS C2141:1992 and JIS R3256:1998.
[0314] The applied voltage was 100 V, and the value was measured 180 seconds after the voltage was applied. The discharge time was 3 seconds.
[0315] (Drop test)
[0316] For the drop strength test, the obtained 120×60×0.7mm glass sample was embedded in a structure with adjusted mass and rigidity to the size of a smartphone commonly used today, and a simulated smartphone was prepared, on which it was freely dropped onto #80SiC sandpaper. The drop height is to make it fall from a height of 5cm and if it does not break, the operation of raising the height by 5cm and dropping it again is repeated until it breaks, and the height at the first break is taken as the drop height. The average fracture height when 20 sheets of the drop test are implemented in each case is taken as the "#80 sandpaper average directional drop strength".
[0317] (4PB strength)
[0318] The chemically strengthened glass was processed into a strip of 120 mm × 60 mm, and a 4-point bending test was performed under the conditions of 30 mm between the outer fulcrums of the support, 10 mm between the inner fulcrums, and 5.0 mm / min of the crosshead speed to measure the 4-point bending strength. The number of test pieces was 10. It should be noted that after the chemically strengthened glass was processed into a strip, automatic chamfering (C chamfering) was performed using a No. 1000 grindstone (manufactured by Tokyo Diamond Tool Manufacturing Co., Ltd.), and the end surface was mirror-finished using a nylon brush with a diameter of 0.1 mm and SHOROX NZ abrasives (manufactured by Showa Denko K.K.) to obtain a glass plate with a thickness of 120 × 60 × 0.7 mm, and the glass plate was measured.
[0319] [Test Example 1]
[0320] Glass raw materials were prepared to obtain the composition of Glass A shown in Table 1 as mol% of oxides, and weighed to obtain 800 g of glass. The mixed glass raw materials were then placed in a platinum crucible and placed in an electric furnace at 1600° C. to be melted for about 5 hours, degassed, and homogenized.
[0321] The obtained molten glass was poured into a mold, kept at a temperature of the glass transition point for 1 hour, and then cooled to room temperature at a rate of 0.5°C / min to obtain a glass block. The obtained glass block was cut, ground, and finally both sides were mirror-polished to obtain a glass plate of 120 mm×60 mm and a thickness of 0.7 mm.
[0322] The glass plate prepared according to the above steps was subjected to ion exchange under the conditions shown in Table 2 to obtain chemically strengthened glass. 90 The results are shown in Figure 3 .exist Figure 3 In the figure, the results of each of Groups 1 to 3 as shown in Table 1, in which the ion exchange time was changed at the same temperature using the molten salt composition with the same components in the same group.
[0323] [Table 2]
[0324]
[0325] like Figure 3 As shown in the figure, when the ion exchange treatment is performed using a molten salt composition with a high sodium ion content, CT becomes higher and CTave exceeds the CT limit. On the other hand, if CT is to be reduced in the ion exchange treatment using the same molten salt composition, there is a tendency for the deep stress to be lowered. From this result, it can be seen that in the method for producing chemically strengthened glass of this embodiment, CTave is made lower than the CT limit by increasing the amount of lithium ions contained in the molten salt composition, and high deep stress can be achieved.
[0326] [Test Example 2]
[0327] According to the same procedure as in Test Example 1, a glass plate made of glass A was prepared, and the glass plate was ion exchanged under the conditions shown in Table 3 to obtain chemically strengthened glass. The results of measuring CS for the obtained chemically strengthened glass are shown in FIG. Figure 4 .
[0328] [Table 3]
[0329]
[0330] like Figure 4 As shown, it can be seen that by making the molten salt composition contain lithium ions, the compressive stress at the surface layer 0-80μm is reduced, and the more the lithium ion content increases, the more the compressive stress of the surface layer decreases. As a result, the internal tensile stress of the deep layer is reduced and is lower than the CT limit, so the compressive stress of the deep layer can be increased while avoiding the CT limit.
[0331] [Test Example 3]
[0332] A glass plate composed of the glass A, glass B and glass C having the glass compositions represented by mol% based on oxides in Table 1 were prepared in the same manner as in Test Example 1. Each of the obtained glass plates was ion exchanged under the conditions shown in Table 4 to obtain chemically strengthened glass. For the obtained chemically strengthened glass, the amount of sodium ions and the amount of lithium ions in the molten salt composition, as well as the temperature and time of the ion exchange treatment were changed as shown in Table 4, and CS was plotted. 90 and CTave, and the results are shown in Figure 5 .
[0333] [Table 4]
[0334]
[0335] like Figure 5 As shown in the figure, the CTave value of glass C is lower, so the CS value is 90 In contrast, glass A is a glass material that has a higher CTave by ion exchange treatment than glass C. Therefore, it can be seen that the method for manufacturing chemically strengthened glass of the present embodiment can further increase the deep compressive stress by reducing the surface compressive stress and suppressing the internal tensile stress in a glass material that has a high CTave by ion exchange treatment such as glass A.
[0336] [Test Example 4]
[0337] A glass plate made of glass A was prepared in the same manner as in Test Example 1, and the glass plate was subjected to ion exchange under the conditions shown in Table 5 to obtain chemically strengthened glass. The results of the evaluation of the glass plate and the chemically strengthened glass are shown in Table 5. Examples 1 to 7 in Table 5 are examples, and Examples 8 to 10 are comparative examples. A blank column (horizontal line) indicates that no evaluation was performed. In addition, the stress distribution diagram of Example 1 is shown in Figure 6 (a), and the stress distribution diagram of Example 8 is shown in Figure 6 (b).
[0338] In Table 5, each symbol represents the following meaning.
[0339] Na2O@center: Na2O concentration at the center of the plate thickness expressed as a molar percentage based on oxides (%)
[0340] Na2O@30μm / Na2O@90μm: The value obtained by dividing the Na2O concentration (%) at a depth of 30μm from the surface by the Na2O concentration (%) at a depth of 90μm from the surface, expressed as a molar percentage based on oxides.
[0341] Na2O@50μm / Na2O@center: The value obtained by dividing the Na2O concentration (%) at a depth of 50μm from the surface by the Na2O concentration (%) at the center of the plate thickness, expressed as a molar percentage based on oxides.
[0342] FSM-CS0: Compressive stress value of glass surface measured by FSM (MPa)
[0343] CS 30 : Compressive stress value at a depth of 30 μm from the glass surface (MPa)
[0344] CS 50 : Compressive stress value at a depth of 50 μm from the glass surface (MPa)
[0345] CS 30-50 : Integrated value of compressive stress CS at a depth of 30 to 50 μm from the surface (Pa·m)
[0346] CS 90 : Compressive stress value at a depth of 90 μm from the glass surface (MPa)
[0347] DOC: Depth of compressive stress layer (μm)
[0348] CTave=ICT / LCT
[0349] ICT: Integrated value of tensile stress (Pa·m)
[0350] LCT: Length of the tensile stress region in the plate thickness direction (μm)
[0351] K1c: Fracture toughness value (MPa·m 1 / 2 )
[0352] DOL-tail: Depth of surface compressive stress layer (μm)
[0353] CS x ”: The second-order differential value of the compressive stress value measured by SLP
[0354] [Table 5]
[0355]
[0356] As shown in Table 5, when Examples 1 to 4 as the embodiment are compared with Examples 8 and 9 as the comparative examples, and when Examples 5 and 6 as the embodiment are compared with Examples 10 and 11 as the comparative examples, it can be seen that CS which contributes to the #80 directional drop strength 90The directional drop strength is improved. The bending strength of Examples 1 to 4 as the embodiment is higher than that of Examples 8 and 9 as the comparative examples, and the bending strength of Examples 5 to 7 as the embodiment is higher than that of Examples 10 and 11 as the comparative examples. In addition, the surface resistivity of Examples 1 to 7 as the embodiment is lower than that of Examples 8 to 11 as the comparative examples, and is less than 10 logΩ / sq.
[0357] Although the present invention has been described in detail with reference to specific embodiments, it is clear to those skilled in the art that various modifications or changes can be made without departing from the spirit and scope of the present invention. This application is based on Japanese patent application No. 2023-083281 filed on May 19, 2023, and its contents are incorporated herein by reference.
Claims
1. A chemically strengthened glass having a plate thickness of t and a compressive stress layer depth DOC of 180×t or more, The integrated value CS of the compressive stress at a depth of 30 μm to 50 μm from the surface 30-50 is less than 12000Pa·m, and Compressive stress value CS at a depth of 90 μm from the surface 90 175×t-88 or above, The unit of t is mm, the unit of DOC is μm, and the unit of CS 90 The unit is MPa.
2. The chemically strengthened glass according to claim 1, in, The Young's modulus is 80 GPa or more.
3. The chemically strengthened glass according to claim 1, in, Stress value CS at depth x from the glass surface measured by a scattered light photoelastic stress meter x In the distribution diagram, the stress value CS x The value of the second-order differential CS x In CS x The range of ≥0 satisfies the following formula, -0.03≤CS x ”≤0.013, The unit of x is μm, the CS x The unit is MPa.
4. The chemically strengthened glass according to claim 1, in, Surface compressive stress value FSM-CS 0 It is above 800MPa.
5. A chemically strengthened glass having a surface resistivity of 10 logΩ / sq or less and a Young's modulus of 80 GPa or more.
6. A chemically strengthened glass having a Na content of 30 μm at a depth of 30 μm from the surface 2 O concentration divided by the Na concentration at a depth of 90 μm from the surface 2 The value obtained by the O concentration is 1.30 or less.
7. The chemically strengthened glass according to claim 6, in, Na at a depth of 50 μm from the surface 2 O concentration divided by Na in the center of the plate thickness 2 The value obtained by adjusting the O concentration is 2 to 4.
8. The chemically strengthened glass according to claim 6, in, Na at a depth of 90 μm from the surface 2 O concentration divided by Na in the center of the plate thickness 2 The value obtained by the O concentration is 2.4 or more.
9. The chemically strengthened glass according to claim 1, 5 or 6, in, The parent composition is expressed as mol% based on oxides and contains 55-75% SiO 2 3~15%Li 2 O, 8~25% Al 2 O 3 .
10. A method for producing chemically strengthened glass, comprising: include: a first ion exchange treatment in which the chemically strengthened glass is brought into contact with a first molten salt composition, and a second ion exchange treatment in which, after the first ion exchange treatment, the chemically strengthened glass is brought into contact with a second molten salt composition, In the first ion exchange treatment, the chemically strengthened glass is brought into contact with the first molten salt composition at 350 to 450° C. for 150 minutes or more. The chemically strengthened glass contains 55 to 75% SiO in terms of mol% based on oxides. 2 3~15%Li 2 O, 8~25% Al 2 O 3 .
11. The method for producing chemically strengthened glass according to claim 10, in, The first molten salt composition contains 0.01 to 1 mass % of lithium ions.
12. A method for producing chemically strengthened glass, comprising: include: a first ion exchange treatment in which the chemically strengthened glass is brought into contact with a first molten salt composition, and a second ion exchange treatment in which, after the first ion exchange treatment, the chemically strengthened glass is brought into contact with a second molten salt composition, The first ion exchange treatment is performed at 350 to 450° C. for 150 minutes or longer, the first molten salt composition contains lithium ions, The chemically strengthened glass contains 55 to 75% SiO in terms of mol% based on oxides. 2 3~15%Li 2 O, 8~25% Al 2 O 3 .
13. The method for producing chemically strengthened glass according to claim 12, in, The second molten salt composition contains 0 to 5 mass % of lithium nitrate.
14. The method for producing chemically strengthened glass according to claim 12, in, include: a third ion exchange treatment of bringing the chemically strengthened glass into contact with a third molten salt composition after the second ion exchange treatment, The third molten salt composition contains 98 mass % or more of potassium nitrate.
15. The method for producing chemically strengthened glass according to any one of claims 10 to 14, in, The ion exchange treatment after the second ion exchange treatment makes CTave of the chemically strengthened glass smaller than CTA, where CTA is obtained by the following formula (1) and CTave is obtained by the following formula (2): t: plate thickness, in μm, K1c: fracture toughness value, unit: MPa·m 1 / 2 , CTave=ICT / LCT…Formula (2) ICT: integrated value of tensile stress, in Pa·m, LCT: The length of the tensile stress region in the thickness direction of the plate, in μm.
16. A glass comprising, expressed in mole percent based on oxides, 55 to 75% SiO 2 , 8~25%Al 2 O 3 3~15%Li 2 O, 1~5% Na 2 O, 0-3% K 2 O, 0-10% MgO, 0-10% CaO, 0-5% SrO, 0-5% ZnO, 0-3% TiO 2 , 0~3% ZrO 2 , 0~1% SnO 2 , 0~1%P 2 O 5 , 0~10% B 2 O 3 , 0~3% Y 2 O 3 , 0~0.1%Fe 2 O 3 , Li 2 O content and Li 2 O、Na 2 O and K 2 The total content ratio of O is Li 2 O / [Li 2 O+Na 2 O+K 2 O] is 0.5 to 0.9, Li 2 O content and Na 2 The ratio of O content to Li 2 O / Na 2 O is 1.5 to 10, and the Young's modulus is 80 GPa or more.
17. The glass according to claim 16, in, B 2 O 3 The content of P 2 O 5 The ratio of B 2 O 3 / P 2 O 5 2.5~500.
18. Glass according to claim 16 or 17, in, When a compressive stress layer is formed by ion exchange treatment using a molten salt composed of sodium nitrate at 380°C for 4 hours, the compressive stress value CS of the compressive stress layer at a depth of 30 μm from the surface is 30 It is above 150MPa.
Citation Information
Cited By
Composition for anti-crack glass, anti-crack glass as well as preparation method and application of anti-crack glass
CN119797755A
Lithium-aluminum-silicon glass with high ball falling resistance and processing technology of lithium-aluminum-silicon glass
CN121494326A
Lithium-aluminum-silicon glass with high impact resistance and process for its production
CN121494326B