RPC tunnel cover plate suitable for high-altitude areas and preparation method of RPC tunnel cover plate

By using resin-coated steel fibers, modified silica hollow tubes and polyethylene glycol in the RPC tunnel cover plate, combined with specific preparation and maintenance processes, the problem of reduced mechanical properties of RPC tunnel cover plates in high altitude areas is solved. High bending strength and weather resistance in harsh environments are achieved.

CN118993627APending Publication Date: 2024-11-22QUJING HUANJU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078161.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The variable climate and complex environments in high altitude areas lead to a reduction in the mechanical properties of RPC tunnel covers, affecting their safety and service life.

Method used

Resin-coated steel fibers, modified silica hollow tubes and polyethylene glycol are used as raw material components, and an RPC tunnel cover with high bending strength and weather resistance is formed through specific preparation methods and curing processes.

Benefits of technology

This method significantly improves the bending strength of RPC tunnel covers, reduces the bending strength loss rate after freezing and blisters, enhances its ability to withstand harsh weather environments, and ensures long-term use stability in high altitude areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993627A_ABST
    Figure CN118993627A_ABST
Patent Text Reader

Abstract

The invention provides an RPC tunnel cover plate suitable for a high altitude area and a preparation method of the RPC tunnel cover plate, and belongs to the technical field of concrete materials. Comprising the following raw material components: 102 parts of cement, 230-270 parts of quartz sand, 35-40 parts of resin coated steel fibers, 4-7 parts of silicon dioxide hollow tubes, 2-3 parts of polyethylene glycol, 1-3 parts of a composite water reducer and 32-38 parts of water. The resin coated steel fiber is prepared by coating steel fiber with polyvinyl chloride. According to the invention, the prepared RPC tunnel cover plate can still maintain excellent mechanical properties after being soaked and frozen, and can resist changeable severe weather in high altitude areas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete materials, and in particular relates to an RPC tunnel cover suitable for high altitude areas and a preparation method thereof. Background Art

[0002] Tunnel covers are key components used in tunnels in the fields of railways, highways, urban rail transit, etc., which play a protective and shielding role. This type of cover plays an indispensable role in the construction of modern transportation infrastructure, especially in improving safety, reliability and meeting the growing transportation needs. RPC, or reactive powder concrete, is a cement-based material with ultra-high strength, high durability, high toughness and good volume stability developed in the mid-1990s by using conventional cement and other materials after high-strength and high-performance concrete. Plates made of RPC materials are now widely used as tunnel covers because of their excellent mechanical strength, stable performance and relatively long service life.

[0003] The changeable climate in high-altitude areas is often accompanied by rainfall and humidity, and the temperature fluctuates greatly, especially in winter, when low temperatures and freezing weather occur frequently. These complex external environmental factors will directly lead to a decrease in the mechanical properties of the RPC tunnel cover, affecting the safety and service life of the RPC tunnel cover. Summary of the invention

[0004] In order to solve the problems existing in the background technology, the present invention provides an RPC tunnel cover suitable for high-altitude areas and a preparation method thereof, which ensures that the prepared RPC tunnel cover still maintains excellent mechanical properties after being soaked in water and frozen, and can withstand the changeable and severe weather in high-altitude areas.

[0005] In order to achieve the above-mentioned purpose, in a first aspect, the present invention provides an RPC tunnel cover suitable for high-altitude areas, which comprises the following raw material components by weight: 102 parts of cement, 230-270 parts of quartz sand, 35-40 parts of resin-coated steel fibers, 4-7 parts of silica hollow tubes, 2-3 parts of polyethylene glycol, 1-3 parts of composite water reducer and 32-38 parts of water; the resin-coated steel fibers are made of polyvinyl chloride-coated steel fibers.

[0006] Furthermore, the preparation method of the resin-coated steel fiber is as follows:

[0007] A1. Weigh polyvinyl chloride powder, add it to 1,2-dichloroethane solvent, heat it to 80°C, stir to completely dissolve the polyvinyl chloride, and cool it to room temperature to obtain a resin solution with a mass concentration of 1-2%;

[0008] A2. Immerse the steel fiber in the resin solution obtained in A1. After 10-15 minutes, take it out and place it in an oven for drying at 80-85℃ for 2 hours to obtain the resin-coated steel fiber.

[0009] Furthermore, the steel fiber is a corrugated steel fiber.

[0010] Furthermore, the preparation method of the silicon dioxide hollow tube is as follows:

[0011] B1, dispersing 2 g of multi-walled carbon nanotubes in 500-550 mL of polyvinyl pyrrolidone-ethanol solution, stirring for 10-12 h, and centrifuging to obtain modified multi-walled carbon nanotubes;

[0012] B2, disperse 2 g of the modified multi-walled carbon nanotubes obtained in B1 in 850-920 mL of ethanol-ammonia solution, ultrasonicate for 35-45 min, then add 6.2 g of hexadecyltrimethylammonium bromide, ultrasonicate for 20-25 min, stir for 2-2.5 h, then add 11 mL of tetraethyl orthosilicate, stir for 7-8 h to obtain a mixed solution;

[0013] B3. The mixed solution obtained in B2 is centrifugally washed with ethanol solution, dried, and calcined in a muffle furnace at 520-550° C. for 6-7 hours to obtain a hollow silica tube.

[0014] Furthermore, in B1, the concentration of polyvinyl pyrrolidone in the polyvinyl pyrrolidone-ethanol solution is 1.6-1.8 g / 100 mL.

[0015] Furthermore, in B2, the molar ratio of NH3, ethanol and water in the ethanol-ammonia aqueous solution is 1:(35-38):(240-250).

[0016] Furthermore, the composite water reducer includes a naphthalene water reducer and a polycarboxylate water reducer.

[0017] Furthermore, the particle size of the quartz sand is 40-80 mesh.

[0018] In a second aspect, the present invention provides a method for preparing the above-mentioned RPC tunnel cover suitable for high altitude areas, comprising the following steps:

[0019] S1. Add cement, quartz sand, resin-coated steel fiber, silica hollow tube, polyethylene glycol, composite water reducer and water into a mixer, stir and mix to obtain slurry;

[0020] S2, place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and forms, demould to obtain a green body;

[0021] S3. The green body obtained in S2 is placed in a curing room for steam curing to obtain an RPC tunnel cover suitable for high altitude areas.

[0022] Furthermore, in S3, the temperature of steam curing is 77-82° C., and the curing time is 2-3 days.

[0023] This application has the following beneficial effects:

[0024] 1. The resin-coated steel fiber, the hollow silica tube and the polyethylene glycol of the present invention are added together to work synergistically, which can not only synergistically improve the flexural strength of the product, but also synergistically reduce the flexural strength loss rate of the product after (water blisters +) freezing, and can also reduce the difference between the flexural strength loss rate before and after freezing and the flexural strength loss rate before and after water blisters + freezing, thereby synergistically enhancing the ability of the product to resist adverse weather environments.

[0025] 2. The surface of the resin-coated steel fiber is wrapped with PVC resin, which not only provides good bonding strength, but also promotes chemical and physical interactions with the concrete matrix. This effect allows the stress to be more evenly transferred from the matrix to the steel fiber when subjected to force, thereby improving the bending strength of the material; the silica hollow tube, due to its high specific surface area and porous structure, can form a stable anchoring effect in the concrete matrix, further improving the interfacial bonding strength with the resin-coated steel fiber and improving the bending strength; polyethylene glycol can form a polymer film in concrete, which helps to fill tiny pores and reduce the formation of cracks, thereby showing better bending resistance on a macro scale.

[0026] 3. The PVC coating can protect the internal steel fibers from corrosion, maintain its performance and structural integrity even in a humid or freeze-thaw environment, and maintain long-term flexural strength; the silica hollow tube can regulate the humidity inside the concrete and reduce the internal stress caused by moisture migration and freezing. This buffering effect helps to maintain a high flexural strength under freezing conditions and reduce strength loss; polyethylene glycol can help concrete maintain a certain plasticity and flexibility in low temperature or humid environments, and reduce cracking and performance degradation caused by temperature or humidity changes; experiments have verified that there is a synergistic effect between the three and they work synergistically. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 , comparative trend diagram of the bending strength of the products obtained in Examples 1-7 of the present invention and Comparative Examples 1-9 before and after freezing and before and after blistering + freezing;

[0028] Figure 2 , comparative trend diagram of the bending strength loss rate of the products obtained in Examples 1-7 of the present invention and Comparative Examples 1-9 before and after freezing and before and after blistering + freezing. DETAILED DESCRIPTION

[0029] The present application is further described in detail below with reference to the embodiments.

[0030] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.

[0031] Example 1: First, prepare resin-coated steel fiber, the steps are as follows:

[0032] A1. Weigh polyvinyl chloride powder, add it to 1,2-dichloroethane solvent, heat it to 80°C, stir to completely dissolve the polyvinyl chloride, cool it to room temperature, and obtain a resin solution with a mass concentration of 1.5%.

[0033] A2. Immerse the corrugated steel fiber in the resin solution obtained in A1. After 12 minutes, take it out and place it in an oven. Dry it at about 83°C for 2 hours to obtain the resin-coated steel fiber.

[0034] Polyvinyl chloride powder (xm-001) was purchased from Dongguan Xinmiao New Materials Co., Ltd.

[0035] 1,2-Dichloroethane (99%) was purchased from Jinan Heshun Chemical Co., Ltd.

[0036] Corrugated steel fiber (>2850MPa) was purchased from Hebei Yiziyuan Engineering Rubber Co., Ltd.

[0037] Then, prepare the silica hollow tube, the steps are as follows:

[0038] B1. Disperse 2 g of multi-walled carbon nanotubes in 520 mL of polyvinyl pyrrolidone-ethanol solution (the concentration of polyvinyl pyrrolidone is 1.7 g / 100 mL), stir for 11 h, and centrifuge to obtain modified multi-walled carbon nanotubes.

[0039] B2, 2 g of modified multi-walled carbon nanotubes obtained in B1 were dispersed in 890 mL of ethanol-ammonia solution (NH 3 , ethanol and water in a molar ratio of 1:36:244), ultrasonicate for 40 min, then add 6.2 g of hexadecyltrimethylammonium bromide, ultrasonicate for 22 min, stir for 2.2 h, then add 11 mL of tetraethyl orthosilicate, stir for 7.5 h to obtain a mixed solution.

[0040] B3. The mixed solution obtained in B2 was centrifugally washed three times with ethanol solution, dried, and calcined in a muffle furnace at 530° C. for 6.5 h to obtain a hollow silica tube.

[0041] Multi-walled carbon nanotubes (HWP-C930) were purchased from Guangzhou Hongwu Material Technology Co., Ltd.

[0042] Polyvinyl pyrrolidone (K30) was purchased from Jinan Xichuan Chemical Technology Co., Ltd.

[0043] Hexadecyltrimethylammonium bromide (SY-Q1) was purchased from Shandong Senya New Materials Co., Ltd.

[0044] Tetraethyl orthosilicate was purchased from Jinan Shuangying Chemical Co., Ltd.

[0045] Finally, the RPC tunnel cover suitable for high altitude areas is prepared as follows:

[0046] S1. Add 102 parts of cement, 245 parts of quartz sand (40-80 mesh), 38 parts of resin-coated steel fiber, 5 parts of silica hollow tube, 2.5 parts of polyethylene glycol, 2 parts of composite water reducer and 35 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. Among them, the composite water reducer includes naphthalene water reducer and polycarboxylic acid water reducer, and the mass ratio of the two is 1:1.

[0047] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0048] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 80° C. and the curing time is 2.5 days (60 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0049] The cement is 42.5R grade ordinary Portland cement (China Resources Cement).

[0050] Polyethylene glycol (PEG600) was purchased from Shandong Jubang Chemical Co., Ltd.

[0051] Naphthalene water reducer (superior grade) and polycarboxylate water reducer (superior grade) were purchased from Shandong Hongquan Chemical Technology Co., Ltd.

[0052] Example 2: The difference between this example and example 1 is that the steps for preparing the resin-coated steel fiber are as follows:

[0053] A1. Weigh polyvinyl chloride powder, add it to 1,2-dichloroethane solvent, heat it to 80°C, stir to completely dissolve the polyvinyl chloride, cool it to room temperature, and obtain a resin solution with a mass concentration of 1%.

[0054] A2. Immerse the corrugated steel fiber in the resin solution obtained in A1. After 10 minutes, take it out and place it in an oven. Dry it at about 80°C for 2 hours to obtain the resin-coated steel fiber.

[0055] Example 3: The difference between this example and Example 1 is that the steps for preparing the resin-coated steel fiber are as follows:

[0056] A1. Weigh polyvinyl chloride powder, add it to 1,2-dichloroethane solvent, heat it to 80°C, stir to completely dissolve the polyvinyl chloride, cool it to room temperature, and obtain a resin solution with a mass concentration of 2%.

[0057] A2. Immerse the corrugated steel fiber in the resin solution obtained in A1. After 15 minutes, take it out and place it in an oven. Dry it at about 85°C for 2 hours to obtain the resin-coated steel fiber.

[0058] Example 4: The difference between this example and Example 1 is that the steps for preparing a hollow silicon dioxide tube are as follows:

[0059] B1. Disperse 2 g of multi-walled carbon nanotubes in 500 mL of polyvinyl pyrrolidone-ethanol solution (the concentration of polyvinyl pyrrolidone is 1.6 g / 100 mL), stir for 10 h, and centrifuge to obtain modified multi-walled carbon nanotubes.

[0060] B2, 2 g of modified multi-walled carbon nanotubes obtained in B1 were dispersed in 850 mL of ethanol-ammonia solution (NH 3 , ethanol and water in a molar ratio of 1:35:240), ultrasonicate for 35 min, then add 6.2 g of hexadecyltrimethylammonium bromide, ultrasonicate for 20 min, stir for 2 h, then add 11 mL of tetraethyl orthosilicate, stir for 7 h to obtain a mixed solution.

[0061] B3. The mixed solution obtained in B2 was centrifugally washed three times with ethanol solution, dried, and calcined in a muffle furnace at 520° C. for 6 h to obtain a hollow silica tube.

[0062] Example 5: The difference between this example and Example 1 is that the steps for preparing a hollow silicon dioxide tube are as follows:

[0063] B1. Disperse 2 g of multi-walled carbon nanotubes in 550 mL of polyvinyl pyrrolidone-ethanol solution (the concentration of polyvinyl pyrrolidone is 1.8 g / 100 mL), stir for 12 h, and centrifuge to obtain modified multi-walled carbon nanotubes.

[0064] B2, 2 g of modified multi-walled carbon nanotubes obtained in B1 were dispersed in 920 mL of ethanol-ammonia solution (NH 3 , ethanol and water in a molar ratio of 1:38:250), ultrasonicate for 45 min, then add 6.2 g of hexadecyltrimethylammonium bromide, ultrasonicate for 25 min, stir for 2.5 h, then add 11 mL of tetraethyl orthosilicate, stir for 8 h to obtain a mixed solution.

[0065] B3. The mixed solution obtained in B2 was centrifugally washed three times with ethanol solution, dried, and calcined in a muffle furnace at 550° C. for 7 h to obtain a hollow silica tube.

[0066] Example 6: The difference between this example and Example 1 is that the steps for preparing an RPC tunnel cover suitable for high altitude areas are as follows:

[0067] S1. Add 102 parts of cement, 230 parts of quartz sand (40-80 mesh), 35 parts of resin-coated steel fiber, 4 parts of silica hollow tube, 2 parts of polyethylene glycol, 1 part of composite water reducer and 32 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. Among them, the composite water reducer includes naphthalene water reducer and polycarboxylate water reducer, and the mass ratio of the two is 1:1.

[0068] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0069] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 77° C. and the curing time is 2 days (48 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0070] Example 7: The difference between this example and Example 1 is that the steps for preparing an RPC tunnel cover suitable for high altitude areas are as follows:

[0071] S1. Add 102 parts of cement, 270 parts of quartz sand (40-80 mesh), 40 parts of resin-coated steel fiber, 7 parts of silica hollow tube, 3 parts of polyethylene glycol, 3 parts of composite water reducer and 38 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. Among them, the composite water reducer includes naphthalene water reducer and polycarboxylate water reducer, and the mass ratio of the two is 1:1.

[0072] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0073] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 82° C. and the curing time is 3 days (72 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0074] Comparative Example 1: The difference between this comparative example and Example 1 is that in the preparation of the resin-coated steel fiber, the corrugated steel fiber is replaced by the end-hook steel fiber.

[0075] Specifically, the steps for preparing the resin-coated steel fiber are as follows:

[0076] A1. Weigh polyvinyl chloride powder, add it to 1,2-dichloroethane solvent, heat it to 80°C, stir to completely dissolve the polyvinyl chloride, cool it to room temperature, and obtain a resin solution with a mass concentration of 1.5%.

[0077] A2. Immerse the end hook steel fiber in the resin solution obtained in A1. After 12 minutes, take it out and place it in an oven. Dry it at about 83°C for 2 hours to obtain the resin-coated steel fiber.

[0078] Comparative Example 2: The difference between this comparative example and Example 1 is that the resin-coated steel fiber is replaced by corrugated steel fiber.

[0079] Specifically, the steps for preparing the RPC tunnel cover suitable for high altitude areas are as follows:

[0080] S1. Add 102 parts of cement, 245 parts of quartz sand (40-80 mesh), 38 parts of corrugated steel fiber, 5 parts of hollow silicon dioxide tube, 2.5 parts of polyethylene glycol, 2 parts of composite water reducer and 35 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. Among them, the composite water reducer includes naphthalene water reducer and polycarboxylic acid water reducer, and the mass ratio of the two is 1:1.

[0081] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0082] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 80° C. and the curing time is 2.5 days (60 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0083] Comparative Example 3: The difference between this comparative example and Example 1 is that the resin-coated steel fiber is replaced by end-hook steel fiber.

[0084] Specifically, the steps for preparing the RPC tunnel cover suitable for high altitude areas are as follows:

[0085] S1. Add 102 parts of cement, 245 parts of quartz sand (40-80 mesh), 38 parts of end hook steel fiber, 5 parts of silica hollow tube, 2.5 parts of polyethylene glycol, 2 parts of composite water reducer and 35 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. Among them, the composite water reducer includes naphthalene water reducer and polycarboxylic acid water reducer, and the mass ratio of the two is 1:1.

[0086] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0087] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 80° C. and the curing time is 2.5 days (60 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0088] Comparative Example 4: The difference between this comparative example and Example 1 is that the resin-coated steel fiber is deleted.

[0089] Specifically, the steps for preparing the RPC tunnel cover suitable for high altitude areas are as follows:

[0090] S1. Add 102 parts of cement, 245 parts of quartz sand (40-80 mesh), 5 parts of hollow silicon dioxide tubes, 2.5 parts of polyethylene glycol, 2 parts of composite water reducer and 35 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. The composite water reducer includes naphthalene water reducer and polycarboxylate water reducer, and the mass ratio of the two is 1:1.

[0091] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0092] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 80° C. and the curing time is 2.5 days (60 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0093] Comparative Example 5: The difference between this comparative example and Example 1 is that the silica hollow tube is replaced with commercially available silica.

[0094] Specifically, the steps for preparing the RPC tunnel cover suitable for high altitude areas are as follows:

[0095] S1. Add 102 parts of cement, 245 parts of quartz sand (40-80 mesh), 38 parts of resin-coated steel fiber, 5 parts of silica, 2.5 parts of polyethylene glycol, 2 parts of composite water reducer and 35 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. Among them, the composite water reducer includes naphthalene water reducer and polycarboxylate water reducer, and the mass ratio of the two is 1:1.

[0096] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0097] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 80° C. and the curing time is 2.5 days (60 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0098] Comparative Example 6: The difference between this comparative example and Example 1 is that the silica hollow tube is deleted.

[0099] Specifically, the steps for preparing the RPC tunnel cover suitable for high altitude areas are as follows:

[0100] S1. Add 102 parts of cement, 245 parts of quartz sand (40-80 mesh), 38 parts of resin-coated steel fiber, 2.5 parts of polyethylene glycol, 2 parts of composite water reducer and 35 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. The composite water reducer includes naphthalene water reducer and polycarboxylate water reducer, and the mass ratio of the two is 1:1.

[0101] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0102] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 80° C. and the curing time is 2.5 days (60 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0103] Comparative Example 7: The difference between this comparative example and Example 1 is that polyethylene glycol is deleted.

[0104] Specifically, the steps for preparing the RPC tunnel cover suitable for high altitude areas are as follows:

[0105] S1. Add 102 parts of cement, 245 parts of quartz sand (40-80 mesh), 38 parts of resin-coated steel fiber, 5 parts of silica hollow tube, 2 parts of composite water reducer and 35 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. Among them, the composite water reducer includes naphthalene water reducer and polycarboxylate water reducer, and the mass ratio of the two is 1:1.

[0106] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0107] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 80° C. and the curing time is 2.5 days (60 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0108] Comparative Example 8: The difference between this comparative example and Example 1 is that the resin-coated steel fiber is replaced by corrugated steel fiber, and the silica hollow tube is replaced by commercially available silica, and polyethylene glycol is deleted.

[0109] Specifically, the steps for preparing the RPC tunnel cover suitable for high altitude areas are as follows:

[0110] S1. Add 102 parts of cement, 245 parts of quartz sand (40-80 mesh), 38 parts of corrugated steel fiber, 5 parts of silicon dioxide, 2 parts of composite water reducer and 35 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. The composite water reducer includes naphthalene water reducer and polycarboxylate water reducer, and the mass ratio of the two is 1:1.

[0111] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0112] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 80° C. and the curing time is 2.5 days (60 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0113] Comparative Example 9: The difference between this comparative example and Example 1 is that the resin-coated steel fiber is deleted, the silica hollow tube is deleted, and the polyethylene glycol is deleted.

[0114] Specifically, the steps for preparing the RPC tunnel cover suitable for high altitude areas are as follows:

[0115] S1. Add 102 parts of cement, 245 parts of quartz sand (40-80 mesh), 2 parts of composite water reducer and 35 parts of water into a mixer, stir at a stirring speed of 40r / min for 10 minutes, mix well, and obtain slurry. The composite water reducer includes naphthalene water reducer and polycarboxylate water reducer, and the mass ratio of the two is 1:1.

[0116] S2. Place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and takes shape, demould to obtain a green body.

[0117] S3. Put the green body obtained in S2 into a curing room for steam curing. The steam curing temperature is about 80° C. and the curing time is 2.5 days (60 hours). Thus, an RPC tunnel cover suitable for high altitude areas is obtained.

[0118] Test example 1: Test item: Mechanical properties (bending strength) before and after freezing treatment.

[0119] Test subjects: products obtained from Examples 1-7 and Comparative Examples 1-9.

[0120] Test method and basis: The freezing treatment condition is -30℃ for 72h, and the flexural strength is tested according to GB / T50081-2019; loss rate = (flexural strength before freezing treatment - flexural strength after freezing treatment) / flexural strength before freezing treatment * 100%.

[0121] Test results: See Table 1.

[0122] Test example 2: Test item: Mechanical properties (bending strength) before and after water blister + freezing treatment.

[0123] Test subjects: products obtained from Examples 1-7 and Comparative Examples 1-9.

[0124] Test method and basis: Soak in water first and then freeze immediately. The soaking condition is to soak in water at room temperature for 7 days. After being fished out, freeze immediately. The freezing condition is to place at -30℃ for 72h. The flexural strength is tested according to GB / T50081-2019; Loss rate = (flexural strength before blister freezing treatment - flexural strength after blister freezing treatment) / flexural strength before blister freezing treatment * 100%.

[0125] Difference = loss rate of test example 2 - loss rate of test example 1. The smaller the difference, the stronger the ability to resist severe weather (heavy rainfall + cooling and freezing).

[0126] Test results: See Table 1.

[0127] Table 1. Test data of Experimental Example 1 and Comparative Example 1

[0128]

[0129] Result analysis: Analyze Examples 1-7 and combine the data in Table 1 and Figure 1-2 It can be seen that the product of the present invention has excellent mechanical properties, and the bending strength is as high as 76.3MPa or more; and the product of the present invention can still maintain excellent mechanical properties after freezing and soaking + freezing, and can withstand the changeable and severe weather in high-altitude areas; among them, after freezing, the bending strength loss rate is 3.13-4.40%; after soaking + freezing, the bending strength loss rate is 4.82-5.60%.

[0130] Analyze Example 1 and Comparative Examples 1-4 and combine the data in Table 1 and Figure 1-2 It can be seen that compared with the end hook steel fiber, the use of corrugated steel fiber is more conducive to improving the bending strength of the product; the use of steel fiber into resin-coated steel fiber through the coating process can further improve the bending strength of the product. In addition, the addition of resin-coated steel fiber can reduce the bending strength loss rate of the product after (water blister +) freezing, and improve the ability of the product to withstand harsh weather environments.

[0131] Analyze Example 1 and Comparative Examples 5-6 and combine the data in Table 1 and Figure 1-2It can be seen that the addition of silicon dioxide can improve the flexural strength of the product; compared with silicon dioxide, the addition of the same amount of the silicon dioxide hollow tube of the present invention is more conducive to improving the flexural strength of the product. In addition, the addition of the silicon dioxide hollow tube can reduce the flexural strength loss rate of the product after (water blister +) freezing, and improve the ability of the product to resist adverse weather environments.

[0132] Analyze Example 1 and Comparative Examples 4, 6, 7 and 9 and combine the data in Table 1 and Figure 1-2 It can be seen that the joint addition of resin-coated steel fiber, silica hollow tube and polyethylene glycol can work synergistically, which can not only synergistically improve the flexural strength of the product, but also synergistically reduce the flexural strength loss rate of the product after (blistering +) freezing, and can also reduce the difference between the flexural strength loss rate before and after freezing and the flexural strength loss rate before and after blistering + freezing, thereby synergistically enhancing the product's ability to withstand adverse weather environments.

[0133] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0134] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. An RPC tunnel cover suitable for high altitude areas, characterized in that: The raw material components include the following by weight: 102 parts of cement, 230-270 parts of quartz sand, 35-40 parts of resin-coated steel fiber, 4-7 parts of silicon dioxide hollow tube, 2-3 parts of polyethylene glycol, 1-3 parts of composite water reducing agent and 32-38 parts of water; the resin-coated steel fiber is made of polyvinyl chloride-coated steel fiber.

2. The RPC tunnel cover suitable for high altitude areas according to claim 1, characterized in that: The preparation method of the resin coated steel fiber is as follows: A1. Weigh polyvinyl chloride powder, add it to 1,2-dichloroethane solvent, heat it to 80°C, stir to completely dissolve the polyvinyl chloride, and cool it to room temperature to obtain a resin solution with a mass concentration of 1-2%; A2. Immerse the steel fiber in the resin solution obtained in A1. After 10-15 minutes, take it out and place it in an oven for drying at 80-85℃ for 2 hours to obtain the resin-coated steel fiber.

3. The RPC tunnel cover suitable for high altitude areas according to claim 2, characterized in that: The steel fibers are corrugated steel fibers.

4. The RPC tunnel cover suitable for high altitude areas according to claim 1, characterized in that: The preparation method of the silicon dioxide hollow tube is as follows: B1, dispersing 2 g of multi-walled carbon nanotubes in 500-550 mL of polyvinyl pyrrolidone-ethanol solution, stirring for 10-12 h, and centrifuging to obtain modified multi-walled carbon nanotubes; B2, disperse 2 g of the modified multi-walled carbon nanotubes obtained in B1 in 850-920 mL of ethanol-ammonia solution, ultrasonicate for 35-45 min, then add 6.2 g of hexadecyltrimethylammonium bromide, ultrasonicate for 20-25 min, stir for 2-2.5 h, then add 11 mL of tetraethyl orthosilicate, stir for 7-8 h to obtain a mixed solution; B3. The mixed solution obtained in B2 is centrifugally washed with ethanol solution, dried, and calcined in a muffle furnace at 520-550° C. for 6-7 hours to obtain a hollow silica tube.

5. The RPC tunnel cover suitable for high altitude areas according to claim 4 is characterized in that: In B1, the concentration of polyvinyl pyrrolidone in the polyvinyl pyrrolidone-ethanol solution is 1.6-1.8 g / 100 mL.

6. The RPC tunnel cover suitable for high altitude areas according to claim 4, characterized in that: In B2, the molar ratio of NH3, ethanol and water in the ethanol-ammonia water solution is 1:(35-38):(240-250).

7. The RPC tunnel cover suitable for high altitude areas according to claim 1, characterized in that: The composite water reducer comprises a naphthalene water reducer and a polycarboxylate water reducer.

8. The RPC tunnel cover suitable for high altitude areas according to claim 1, characterized in that: The particle size of the quartz sand is 40-80 meshes.

9. A method for preparing an RPC tunnel cover suitable for high altitude areas according to any one of claims 1 to 8, characterized in that: The steps include: S1. Add cement, quartz sand, resin-coated steel fiber, silica hollow tube, polyethylene glycol, composite water reducer and water into a mixer, stir and mix to obtain slurry; S2, place the prepared mold on a vibration table, turn on the vibration table, pour the slurry obtained in S1 into the mold, and after the slurry solidifies and forms, demould to obtain a green body; S3. The green body obtained in S2 is placed in a curing room for steam curing to obtain an RPC tunnel cover suitable for high altitude areas.

10. The method for preparing the RPC tunnel cover suitable for high altitude areas according to claim 9, characterized in that: In S3, the steam curing temperature is 77-82°C and the curing time is 2-3 days.