Method for preparing low-loss 18H hexagonal ferrite and testing microwave magnetic dielectric properties

Through the preparation of mixtures of Fe2O3, BaCO3, Nb2O5, CoO and microwave dielectric characteristics testing, the loss and testing accuracy problems of ferrite materials in high-frequency applications are solved, and performance optimization and industrial applications are achieved.

CN118993718AInactive Publication Date: 2024-11-22SICHUAN AEROSPACE POLYTECHNIC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411078145.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional ferrite materials have problems such as high-frequency dielectric loss, large magnetic loss, low saturation magnetic induction strength and poor thermal stability in high-frequency, high-energy efficiency and high-power applications. The existing magnetic dielectric characteristic testing methods are complex and accurate. Not high enough to optimize material performance.

Method used

Low-loss 18H hexagonal ferrite is prepared by Fe2O3, BaCO3, Nb2O5 and CoO mixture. The magnetic dielectric characteristics test are carried out through high-temperature roasting, liquid nitrogen freezing grinding, pressing and sintering processes, and the magnetic dielectric characteristics are tested in combination with microwave network analyzer to establish material performance and preparation. Model of process relationship.

Benefits of technology

The preparation of 18H hexagonal ferrite materials with low loss and excellent performance and accurate microwave dielectric characteristics testing are realized, the magnetic induction strength and loss performance are optimized, the process flow is simplified, the testing accuracy is improved, and it is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993718A_ABST
    Figure CN118993718A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing low-loss 18H hexagonal ferrite and testing microwave magnetic dielectric properties, and belongs to the field of ferrite preparation and testing. The preparation method comprises the steps of raw material preparation, ingredient mixing, high-temperature roasting, cooling and grinding, pressing and sintering as well as surface treatment and grinding. The method can effectively ensure that the components of the hexagonal ferrite are uniform, and the ferrite powder which is moderate in particle size, strong in magnetism and low in loss is prepared. The testing method comprises the following steps: firstly, testing impedance matching and frequency response of a material sample through a microwave network analyzer, and then measuring the magnetic dielectric characteristics, including reaction of the material to a magnetic field, so as to obtain the size of the magnetic dielectric constant. Then, material performance parameters are obtained through data analysis and processing, the relationship between the microwave magnetic dielectric characteristics of the material and the conditions such as components, the preparation process and the working frequency is researched, and the material performance is optimized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of ferrite preparation and testing, and more specifically relates to a system and method for preparing low-loss 18H hexagonal ferrite and testing microwave magneto-dielectric properties. Background Art

[0002] Ferrite is an important soft magnetic material with wide applications in electronic information equipment, electromagnetic compatibility equipment, power electronics, and new energy vehicles. However, traditional ferrite materials often have problems such as high-frequency dielectric loss, large magnetic loss, low saturation magnetic induction intensity, and poor thermal stability, which greatly restricts their use in high-frequency, high-efficiency, and high-power applications.

[0003] 18H hexagonal ferrite is widely used in the field of electronic information due to its excellent properties among ferrites, such as high magnetic induction intensity, low magnetic loss, etc. However, the preparation process of 18H hexagonal ferrite is complicated, requiring precise batching, mixing, roasting, grinding, pressing, sintering and other steps.

[0004] Moreover, the physical properties of 18H hexagonal ferrite, such as magnetic properties and dielectric properties, are related to its composition, structure and other factors. How to obtain ideal performance parameters requires different optimization designs for different applications, such as: low loss, high magnetic permeability, high saturation magnetic induction, good frequency stability, etc.

[0005] In addition, accurate measurement and analysis of the magnetic and dielectric properties of ferrite materials is of great significance for optimizing material performance and application design. However, there are still many problems in the current testing and analysis methods of the magnetic and dielectric properties of ferrite materials, such as complex testing process, insufficient precision, and cumbersome data processing.

[0006] Therefore, developing a low-loss 18H hexagonal ferrite preparation method and a convenient, economical and accurate microwave magnetic dielectric property test method has important practical significance and application value for improving the performance of ferrite materials and expanding their application in various fields. The present invention is a low-loss 18H hexagonal ferrite preparation method and a microwave performance test method thereof. The method is simple and easy to operate, and the prepared product has excellent performance and has great application prospects in industry. Summary of the invention

[0007] The main technical problems solved by the present invention are how to prepare low-loss, high-performance 18H hexagonal ferrite materials, and how to accurately and quickly test and analyze their microwave magneto-dielectric properties, so as to promote the performance optimization of this material in high-frequency, high-energy-efficiency and high-power applications, and expand its application scope in electronic information equipment, electromagnetic compatibility equipment, power electronics and new energy vehicles.

[0008] In order to achieve the above object, the present invention is implemented by adopting the following technical scheme: the preparation of the low-loss 18H hexagonal ferrite includes:

[0009] Raw materials configuration: Fe2O3, BaCO3, Nb2O5, CoO mixture is used as raw materials, and the configuration ratio is based on the molar amount of Fe;

[0010] Ingredient mixing: Mix the raw materials evenly and stir them evenly to ensure that the raw materials are fully dispersed and mixed;

[0011] High temperature roasting: put the evenly mixed raw materials into a high temperature furnace for roasting;

[0012] Cooling and grinding: After roasting, take out the raw material and cool it naturally, then perform liquid nitrogen freezing grinding, and sieve the ground powder to obtain powder of a certain particle size;

[0013] Pressing and sintering: The screened powder is pressed and then sintered;

[0014] After preparation, surface treatment and grinding are performed.

[0015] In one embodiment, the configuration ratio is 1 mol BaCO3, 12 mol Fe2O3, 0.1 mol Nb2O5 and 0.1 mol CoO.

[0016] In one embodiment, the high temperature calcination temperature is controlled at 900-1000° C., and the calcination is continued for 4-6 hours.

[0017] In one embodiment, the cooling and grinding comprises:

[0018] Take the raw materials out of the high temperature furnace and let them cool naturally to room temperature for 2-3 hours;

[0019] The raw materials are placed in liquid nitrogen for freezing, and the freezing time in liquid nitrogen is 25-30 minutes;

[0020] The ferrite powder obtained by grinding is controlled within the range of 1-10 microns.

[0021] In one embodiment, the pressing and sintering:

[0022] Pressing: Take out the sieved powder, put it into a pressing mold, and use a hydraulic press or a powder metallurgy press to press it into shape. The pressing force is between 100-500Mpa;

[0023] Sintering: Put the pressed green body into the sintering furnace for high-temperature sintering. The sintering temperature is controlled at 1200-1300℃ and the sintering time is 2-4 hours.

[0024] Cooling: After sintering is completed, the sintering furnace is naturally cooled to room temperature.

[0025] On the other hand, a microwave magnetic dielectric property test method is provided, wherein the test method is applicable to the low-loss 18H hexagonal ferrite, and the test method comprises:

[0026] Prepare the sample: cut and grind the prepared material into the required shape;

[0027] Test impedance matching: Use a microwave network analyzer to measure and confirm whether the impedance of the sample is matched;

[0028] Determine frequency response: measure the microwave attenuation and reflection value of the sample;

[0029] Determination of magnetic dielectric properties: By measuring the reaction of the object to the magnetic field, the magnitude of the magnetic dielectric constant can be obtained;

[0030] Through the above test data, data analysis and processing are carried out to obtain the required material performance parameters;

[0031] Study the relationship between the microwave magneto-dielectric properties of materials and their components, preparation process, operating frequency and other conditions to optimize material performance.

[0032] In one embodiment, the test impedance matching is as follows: connect the sample to a network analyzer and set the appropriate frequency range to several hundred MHz to several tens of GHz;

[0033] The network analyzer will provide impedance (Z) measurement results, using the Smith plot to display the impedance characteristics of the sample at the selected frequency. The impedance Z is determined by the S-parameter related formula:

[0034]

[0035] S11 and S21 are the scattering parameters of the network analyzer port, referred to as S parameters;

[0036] S11 represents the proportion of energy input to port 1 that is reflected back;

[0037] S21 represents the proportion of energy input at port 1 that is transmitted to port 2 through the network;

[0038] Z0 is the reference impedance.

[0039] In one embodiment, the magneto-dielectric properties are determined as follows:

[0040] The sample is suspended in a magnetic field, and the complex magnetic permeability μ or complex dielectric constant ε of the material is obtained by measuring the sample's response to the change in the magnetic field.

[0041] Magnetization intensity:

[0042]

[0043] Wherein, M represents the magnetization intensity, M0 represents the initial magnetization intensity, μ0 represents the magnetic permeability of air, and I represents the magnetization intensity generated under the external magnetic field;

[0044] Magnetic Permeability:

[0045] μ=μ0*(1+χ)

[0046] Here, χ represents the magnetic susceptibility and μ represents the magnetic permeability of the material.

[0047] The following mathematical formula is usually used to determine the dielectric constant:

[0048]

[0049] Where C represents capacitance, ε0 represents the dielectric constant in air, A represents the electrode area, d represents the sample thickness, and ε represents the dielectric constant of the material;

[0050] Dielectric loss:

[0051] tanδ=ωC0Rp / (1+(ωωC0Rp 2 )

[0052] Among them, ω represents the angular frequency, C0 represents the capacitance, Rp represents the parallel resistance, and tanδ represents the dielectric loss angle.

[0053] In one embodiment, the relationship between the microwave magneto-dielectric properties of the research material and its composition, preparation process, operating frequency and other conditions includes:

[0054] Establish model and collect data: Establish the relationship between microwave magneto-dielectric property y and various influencing factors x1, x2, x3, ... xn;

[0055] This relationship is described as y = a0 + a1x1 + a2x2 + ... + an*xn + e;

[0056] The influencing factors include the composition and purity of the material, the structure of the material, and the preparation conditions of the material;

[0057] Among them, a0, a1, a2, ..., an are the parameters to be determined, and e is the error term;

[0058] Calculate the residual sum of squares: The difference between the true value y and the predicted value is the residual e, and its sum of squares is expressed as: SS = Σ(y-(a0+a1x1+a2x2+...+an*xn)) 2 ;

[0059] Solve the parameters that minimize the residual sum of squares: The parameters are obtained by solving the system of equations with partial derivatives equal to 0;

[0060] That is, for a0,a1,a2,...,an, we have Solve this system of equations, and the resulting set of solutions is the desired parameter values;

[0061] Test the goodness and significance of the model: Use F test, t test or calculate R square to test the validity of the model and verify its significance and goodness of fit.

[0062] Beneficial effects of the present invention:

[0063] The present invention provides a low-loss 18H hexagonal ferrite preparation method and a microwave magneto-dielectric property test method, which can effectively improve the performance of ferrite materials and provide an accurate and convenient test and analysis means, effectively solving the problems of large high-frequency loss, low magnetic induction intensity and poor thermal stability of ferrite materials in the prior art, optimizing the component ratio and process conditions, and improving the magnetic induction intensity and loss performance of 18H hexagonal ferrite. At the same time, the process is clear, the operation is simple, and it is very easy to industrialize production. The microwave magneto-dielectric property test method can conduct a comprehensive and in-depth study on the microwave performance of 18H hexagonal ferrite, provide important parameters and basis for practical applications, and also promote technological progress in this field. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 The present invention discloses a process for preparing low-loss 18H hexagonal ferrite;

[0065] Figure 2 The flowchart of the microwave magneto-dielectric property testing method of the present invention is as follows;

[0066] Figure 3 The relationship between the microwave magneto-dielectric properties of the material and its components, preparation process, operating frequency and other conditions is studied for the present invention. DETAILED DESCRIPTION

[0067] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Typical embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described in the present invention. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0068] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0069] like Figure 1 As shown, the preparation of the low-loss 18H hexagonal ferrite includes:

[0070] S1. Prepare raw materials: Use a mixture of Fe2O3, BaCO3, Nb2O5 and CoO as raw materials, and the preparation ratio is based on the molar amount of Fe.

[0071] In the preparation of ferrite, the chemical formula of the prepared ferrite must first be determined. The chemical formula of hexagonal ferrite (Bariumhexaferrite) is BaFe 12 O 19 .

[0072] Therefore, the raw materials are configured according to the molar ratio of this chemical formula, that is, 1 mole of BaCO3, 12 moles of Fe2O3. In this process, the addition ratio of other additives such as Nb2O5 and CoO is generally small, which can be adjusted according to actual needs, and generally does not exceed 5% of the molar ratio of Fe. The configuration ratio is: 1 mole of BaCO3, 12 moles of Fe2O3, 0.1 mole of Nb2O5 and 0.1 mole of CoO.

[0073] S2. Mixing ingredients: Mix the raw materials evenly and stir them to ensure that the raw materials are fully dispersed and mixed.

[0074] S3, high temperature roasting: put the uniformly mixed raw materials into a high temperature furnace for roasting. The high temperature roasting temperature is controlled at 900-1000°C and the roasting is continued for 4-6 hours.

[0075] S4, cooling and grinding: After the roasting is completed, the raw material is taken out and cooled naturally, and then liquid nitrogen freezing grinding is performed, and the powder obtained by grinding is sieved to obtain powder of a certain particle size.

[0076] After roasting, the raw materials are taken out of the high temperature furnace and left to cool naturally to room temperature, which usually takes about 2-3 hours.

[0077] Next, the cooled raw materials are placed in liquid nitrogen for freezing, which makes the materials easier to break in the subsequent grinding process. The raw materials are usually frozen in liquid nitrogen for 25-30 minutes.

[0078] Then put the frozen raw materials into a grinder for mechanical grinding. The time of the grinding process after roasting and freezing can be adjusted according to the actual effect.

[0079] The ground ferrite material will form a powder. In order to obtain a powder with a consistent particle size that meets the experimental requirements, it needs to be screened. A series of sieves with smaller and smaller apertures can be used for screening.

[0080] In order to achieve good magnetic properties and microwave absorption performance, the ground ferrite powder should generally be controlled within the range of 1-10 microns.

[0081] S5. Pressing and sintering: Press the screened powder and then sinter it.

[0082] Pressing: Take out the powder obtained by screening and put it into the pressing mold. Use a hydraulic press or a powder metallurgy press to press and shape. Generally, the pressing force is between 100-500Mpa, which ensures that the powder can be pressed into a blank of a certain shape and size.

[0083] Sintering: Put the pressed green body into the sintering furnace for high temperature sintering. The general sintering temperature is controlled at 1200-1300℃ and the sintering time is 2-4 hours. In this step, the sintering heating rate and sintering temperature must be controlled to ensure the sintering effect.

[0084] Cooling: After sintering, the sintering furnace needs to be cooled naturally to room temperature to avoid internal stress and cracking of the sintered body caused by rapid cooling.

[0085] S6. After preparation, surface treatment and grinding are performed.

[0086] Surface treatment: After cooling, the ferrite is subjected to surface treatment, such as grinding and polishing, which can remove the oxide layer and impurities on the surface of the sintered body and improve the microstructure and appearance quality of the ferrite.

[0087] Grinding again: If you need to obtain hexagonal ferrite in powder form, the sintered body can be ground again. By controlling the grinding time and method, powders of different particle sizes can be obtained.

[0088] Inspection: Carry out performance inspection on the prepared ferrite, such as hardness, density, magnetic properties, etc., to ensure that the quality of the product meets the requirements.

[0089] Embodiment 2

[0090] like Figure 2 As shown, according to the low-loss 18H hexagonal ferrite prepared in Example 1, the microwave magnetic dielectric property test method of Example 2 is constructed. The test method is applicable to the low-loss 18H hexagonal ferrite, and the test method includes:

[0091] S1. Prepare samples: Cut and grind the prepared materials into the required shapes.

[0092] The prepared material is cut and ground into the required shape, such as round or square, and the thickness is generally controlled at 1-3mm.

[0093] S2. Test impedance matching: Use a microwave network analyzer to measure and confirm whether the impedance of the sample is matched.

[0094] The test impedance matching is as follows: connect the sample to the network analyzer and set the appropriate frequency range to several hundred MHz to several tens of GHz;

[0095] The network analyzer will provide impedance (Z) measurement results, using the Smith plot to display the impedance characteristics of the sample at the selected frequency. The impedance Z is determined by the S-parameter related formula:

[0096]

[0097] S11 and S21 are the scattering parameters of the network analyzer port, referred to as S parameters;

[0098] S11 represents the proportion of energy reflected back from the input of port 1; S11 measures how much energy is "reflected" back and does not enter the network. It is usually used to describe the input impedance matching of the network. If S11 approaches 0, it means that almost all input signals enter the network, and the impedance matching is very good; if S11 approaches 1, it means that most of the input signals are reflected back and the impedance matching is poor.

[0099] S21 represents the proportion of energy input at port 1 that is transmitted to port 2 through the network; S21 measures the transmission efficiency of the network for the input signal. If S21 approaches 1, it means that the transmission efficiency of the network is very high; if S21 approaches 0, it means that the transmission efficiency of the network is low.

[0100] Z0 is the reference impedance.

[0101] Where Z is the impedance of the sample to be tested, Z0 is the reference impedance, usually 50 ohms. S11 represents the reflected portion of the energy input at port 1, and S21 represents the portion of the energy input at port 1 that is transmitted through the network to port 2.

[0102] Therefore, by measuring the S parameters of the sample in the microwave network analyzer, the impedance characteristics of the sample can be calculated. Combined with the Smith diagram, the impedance characteristics of the sample at the selected frequency can be intuitively seen.

[0103] S3. Determine frequency response: measure the microwave attenuation and reflection values ​​of the sample.

[0104] Still using a network analyzer, the selected frequency range is 2-18 GHz. By recording the amplitude of the S parameters (S11 and / or S21), the parameters are S11, S12, S21 and S22, which are collectively called scattering parameters or S parameters.

[0105] Amplitude: The amplitude of S11 indicates how much of the signal input from port 1 is reflected back, so it is also called the reflection coefficient, and its value ranges from 0 to 1.

[0106] Phase: The phase of S11 represents the phase difference between the reflected signal and the original input signal.

[0107] Therefore, S11 is usually used to evaluate the input impedance matching of a circuit or system. If the value of S11 is smaller, it means that the reflected signal is less, which means that the input impedance matching is better. The commonly used unit is dB, and S11 can be converted to dB units through 20*log10(S11).

[0108] S4. Determination of magnetic dielectric properties: By measuring the reaction of the object to the magnetic field, the magnitude of the magnetic dielectric constant can be obtained. By measuring the reaction of the object to the magnetic field, the magnitude of the magnetic dielectric constant can be obtained. The specific operation is to put the material into the magnetic field, and by measuring the changes in current and voltage, the magnetic permeability μ and dielectric constant ε of the material can be obtained.

[0109] The magneto-dielectric properties are as follows:

[0110] The sample is suspended in a magnetic field, and the complex magnetic permeability μ or complex dielectric constant ε of the material is obtained by measuring the sample's response to the change in the magnetic field.

[0111] The magnetization intensity M is an important physical quantity that describes the magnetic behavior of a material in a magnetic field. Under a given external magnetic field, the ratio of the total magnetic moment generated inside a material to the volume of the material is the magnetization intensity. Specifically, the magnetization intensity describes the degree to which a material is magnetized, and it reflects the size of the magnetic moment formed by magnetic particles per unit volume.

[0112] The magnitude of magnetization intensity is not only related to the strength of the applied external magnetic field, but also to the properties of the material itself. In the microwave magneto-dielectric property test, the measurement of magnetization intensity is very important. By measuring the magnetization intensity, the magnetic properties of the material can be quantitatively analyzed and the microwave magneto-dielectric properties of the material can be further understood.

[0113] Magnetization intensity:

[0114]

[0115] Wherein, M represents the magnetization intensity, M0 represents the initial magnetization intensity, μ0 represents the magnetic permeability of air, and I represents the magnetization intensity generated under the external magnetic field;

[0116] Magnetic Permeability:

[0117] μ=μ0*(1+χ)

[0118] Here, χ represents the magnetic susceptibility and μ represents the magnetic permeability of the material.

[0119] Magnetic susceptibility is a physical concept that describes how well a material becomes magnetized in response to an applied magnetic field. It can be measured experimentally.

[0120] The basic measurement steps are as follows:

[0121] First, place the material in a uniform magnetic field, adjust the strength of the magnetic field, and use a precise magnetic field meter to measure the material's vertical magnetic field induction intensity B.

[0122] By measuring the magnetization intensity M of the material in this magnetic field, the magnetic susceptibility can be calculated using the following formula:

[0123] χ=M / H

[0124] Where H represents the magnetic field intensity. In this way, the value of magnetic susceptibility χ can be obtained, which is closely related to the microwave magneto-dielectric properties of the material.

[0125] The following mathematical formula is usually used to determine the dielectric constant:

[0126]

[0127] Where C represents capacitance, ε0 represents the dielectric constant in air, A represents the electrode area, d represents the sample thickness, and ε represents the dielectric constant of the material;

[0128] Dielectric loss:

[0129] tanδ=ωC0Rp / (1+(ωωC0Rp 2 )

[0130] Among them, ω represents the angular frequency, C0 represents the capacitance, Rp represents the parallel resistance, and tanδ represents the dielectric loss angle.

[0131] Through the above test data, data analysis and processing are carried out to obtain the required material performance parameters.

[0132] S5. Study the relationship between the microwave magneto-dielectric properties of materials and their components, preparation process, operating frequency and other conditions to optimize material performance. The relationship between material performance and various influencing factors can be obtained through methods such as the least squares method.

[0133] like Figure 3 As shown, the relationship between the microwave magneto-dielectric properties of the research material and its composition, preparation process, working frequency and other conditions includes:

[0134] S501. Establish model and collect data: establish the relationship between microwave magneto-dielectric property y and various influencing factors x1, x2, x3, ... xn.

[0135] This relationship is described as y = a0 + a1x1 + a2x2 + ... + an*xn + e;

[0136] Among them, a0, a1, a2, ..., an are the parameters to be determined, and e is the error term.

[0137] In the study of microwave magneto-dielectric properties, there are many factors that affect the microwave magneto-dielectric properties (y), which can be divided into two categories: factors affecting the properties of the material itself and factors affecting external conditions.

[0138] The factors affecting the properties of the material itself include:

[0139] The composition and purity of the materials, the types and proportions of chemical substances used in preparation, the types and concentrations of impurities, etc.

[0140] The structure of the material, the crystal structure of the material, the shape and size of the particles, the type and density of microscopic defects, the magnetic domain structure of the material, etc.

[0141] External factors include:

[0142] Material preparation conditions, sintering temperature and time, cooling rate, grinding and pressing conditions, etc.

[0143] Test conditions, test ambient temperature, frequency and intensity of the electromagnetic field, test form of the material (such as thickness), etc.

[0144] S502, calculate the residual sum of squares: the difference between the true value y and the predicted value is the residual e, and its sum of squares is expressed as: SS = Σ(y-(a0+a1x1+a2x2+...+an*xn)) 2 ;

[0145] S503, solving the parameters that minimize the residual sum of squares: the parameters are obtained by solving the equation group whose partial derivative is 0;

[0146] That is, for a0,a1,a2,...,an, we have Solve this system of equations, and the resulting set of solutions is the desired parameter values;

[0147] S504. Test the goodness and significance of the model: Test the validity of the model through F test, t test or calculation of R square, and verify its significance and goodness of fit.

[0148] After the above-mentioned steps of testing impedance matching, measuring frequency response, and measuring magnetic dielectric properties, a wealth of test data is obtained. These data include the impedance value, magnetization intensity, complex magnetic permeability, complex dielectric constant, etc. of the material at different frequencies. According to the magnetic permeability and dielectric constant obtained from the experimental test, combined with the actual operating frequency and other environmental parameters, the ferrite material can be optimized for design and preparation to achieve excellent performance such as low loss, high magnetic permeability, and high saturation magnetic induction.

[0149] Embodiment three:

[0150] First, the raw materials are prepared by mixing 12 moles of Fe2O3, 1 mole of BaCO3, 0.1 mole of Nb2O5 and 0.1 mole of CoO. After these raw materials are mixed in proportion, they are evenly kneaded using a stirrer.

[0151] The mixed raw materials are then placed in a high-temperature furnace, the temperature of which is set at 950°C, and fired for 5 hours. The experimental results show that this can effectively sinter the ferrite and allow its components to be fully mixed and diffused.

[0152] After calcination, the raw material was taken out and then cooled naturally at room temperature. After 2.5 hours of cooling, the raw material was transferred into liquid nitrogen and frozen for 30 minutes. After freezing, it was ground and sieved to obtain ferrite powder of about 5 microns.

[0153] The screened powder was pressed and sintered. We used a pressure of 500Mpa for pressing and then sintered at 1250 degrees for 2.5 hours. The sintering furnace was then naturally cooled to room temperature.

[0154] Finally, the microwave magnetic dielectric properties test is carried out: we use a network analyzer to measure the impedance of the sample from 1 GHz to 10 GHz and obtain the impedance value Z. Then, by measuring the microwave attenuation value of the sample, the frequency response data is obtained.

[0155] When measuring the magneto-dielectric properties, the magnetization intensity I is 0.85 T under the external magnetic field, and the complex magnetic permeability μ is obtained. Then, the complex dielectric constant is obtained by measuring the dielectric constant ε and the dielectric loss angle tanδ.

[0156] Finally, through statistical software, we analyzed and processed the data and found that the magnetic strength was 5000Oe, the dielectric constant was 15, the frequency was in the range of 1-10GHz, and the loss angle was less than 0.01. These results are in line with our expected material performance parameters, indicating that our preparation process and testing methods are effective.

[0157] It should be understood that the detailed description of the technical solutions of the present invention by means of the preferred embodiments is illustrative rather than restrictive. A person skilled in the art may modify the technical solutions described in the embodiments, or replace some of the technical features by equivalents, based on reading the specification of the present invention; and these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing low-loss 18H hexagonal ferrite, characterized in that: The low-loss 18H hexagonal ferrite preparation comprises: Raw materials configuration: Fe2O3, BaCO3, Nb2O5, CoO mixture is used as raw materials, and the configuration ratio is based on the molar amount of Fe; Ingredient mixing: Mix the raw materials evenly and stir them evenly to ensure that the raw materials are fully dispersed and mixed; High temperature roasting: put the evenly mixed raw materials into a high temperature furnace for roasting; Cooling and grinding: After roasting, take out the raw material and cool it naturally, then grind it with liquid nitrogen, and sieve the powder obtained by grinding; Pressing and sintering: The screened powder is pressed and then sintered; Post-processing: surface treatment and grinding are performed after preparation.

2. The method for preparing low-loss 18H hexagonal ferrite according to claim 1, characterized in that: The configuration ratio is 1 mole of BaCO3, 12 moles of Fe2O3, 0.1 mole of Nb2O5 and 0.1 mole of CoO.

3. The method for preparing low-loss 18H hexagonal ferrite according to claim 1, characterized in that: The high temperature roasting temperature is controlled at 900-1000° C. and the roasting is continued for 4-6 hours.

4. The method for preparing low-loss 18H hexagonal ferrite according to claim 1, characterized in that: The cooling and grinding comprises: Take the raw materials out of the high temperature furnace and let them cool naturally to room temperature for 2-3 hours; The raw materials are placed in liquid nitrogen for freezing, and the freezing time in liquid nitrogen is 25-30 minutes; The ferrite powder obtained by grinding is in the range of 1-10 microns.

5. The low-loss 18H hexagonal ferrite preparation according to claim 1, characterized in that: The pressing and sintering: Pressing: Take out the powder obtained by screening, put it into a pressing mold, and use a hydraulic press or a powder metallurgy press to press and form it. The pressing force is between 100-500Mpa; Sintering: Put the pressed green body into the sintering furnace for high-temperature sintering. The sintering temperature is controlled at 1200-1300℃ and the sintering time is 2-4 hours. Cooling: After sintering is completed, the sintering furnace is naturally cooled to room temperature.

6. A microwave magneto-dielectric property testing method, the testing method being applicable to the low-loss 18H hexagonal ferrite prepared by the preparation method according to any one of claims 1 to 5, characterized in that: The test method includes: Prepare the sample: cut and grind the prepared material into the required shape; Test impedance matching: Use a microwave network analyzer to measure and confirm whether the impedance of the sample is matched; Determine frequency response: measure the microwave attenuation and reflection value of the sample; Determination of magnetic dielectric properties: By measuring the reaction of the object to the magnetic field, the magnitude of the magnetic dielectric constant can be obtained; Study the relationship between the microwave magneto-dielectric properties of materials and their components, preparation process and operating frequency to optimize material performance.

7. The microwave magneto-dielectric property testing method according to claim 6, characterized in that: The test impedance matching is as follows: connect the sample to the network analyzer and set the frequency range; The network analyzer will provide impedance (Z) measurement results, using the Smith plot to display the impedance characteristics of the sample at the selected frequency. The impedance Z is determined by the S-parameter related formula: S11 and S21 are the scattering parameters of the network analyzer port, referred to as S parameters; S11 represents the proportion of energy input to port 1 that is reflected back; S21 represents the proportion of energy input at port 1 that is transmitted to port 2 through the network; Z0 is the reference impedance.

8. The microwave magneto-dielectric property testing method according to claim 6, characterized in that: The magneto-dielectric properties are as follows: The sample is suspended in a magnetic field, and the complex magnetic permeability μ and complex dielectric constant ε of the material are obtained by measuring the sample's response to the change in the magnetic field. Magnetization intensity: Magnetization intensity: Wherein, M represents the magnetization intensity, M0 represents the initial magnetization intensity, μ0 represents the magnetic permeability of air, and I represents the magnetization intensity generated under the external magnetic field; Complex magnetic permeability: μ=μ0*(1+χ) Among them, χ represents the magnetic susceptibility, and μ represents the magnetic permeability of the material; The following mathematical formula is usually used to determine the dielectric constant: Where C represents capacitance, ε0 represents the dielectric constant in air, A represents the electrode area, d represents the sample thickness, and ε represents the dielectric constant of the material; Dielectric loss: tanδ=ωC0Rp / (1+(ωωC0Rp 2 ) Among them, ω represents the angular frequency, C0 represents the capacitance, Rp represents the parallel resistance, and tanδ represents the dielectric loss angle.

9. The microwave magneto-dielectric property testing method according to claim 6, characterized in that: The relationship between the microwave magneto-dielectric properties of the research material and its components, preparation process and operating frequency includes: Establish model and collect data: Establish the relationship between microwave magneto-dielectric property y and various influencing factors x1, x2, x3, ... xn; This relationship is described as y = a0 + a1x1 + a2x2 + ... + an*xn + e; Among them, a0, a1, a2, ..., an are the parameters to be determined, and e is the error term; The influencing factors include the composition and purity of the material, the structure of the material, and the preparation conditions of the material; Calculate the residual sum of squares: The difference between the true value y and the predicted value is the residual e, and its sum of squares is expressed as: SS = Σ(y-(a0+a1x1+a2x2+...+an*xn)) 2 ; Solve the parameters that minimize the residual sum of squares: The parameters are obtained by solving the system of equations with partial derivatives equal to 0; That is, for a0,a1,a2,...,an, we have Solve this system of equations, and the resulting set of solutions is the desired parameter values; Test the goodness and significance of the model: Test the validity of the model through F test, t test or calculation of R square to verify its significance and goodness of fit.

Citation Information

Patent Citations

  • Hexagonal ferrite, and antenna and communication equipment using the same

    CN101014548A

  • Multi-phase ion-electron mixing conductor powder material, manufacturing method and application thereof

    CN101219889A

  • Preparation method of high-magnetic-conductivity low-temperature-sintering Z-shaped hexagonal ferrite material

    CN101913850A

  • Ferrite-base composite magnetic dielectric antenna substrate material and preparation method thereof

    CN103304186A

  • Low-electric-field dielectric adjustable niobium-doped barium ferrite material and preparation method thereof

    CN109626983A