Method for regulating and controlling radial shrinkage of permanent magnetic ferrite

By combining non-ionic and bio-based surfactants and combining ionic liquids, uniformly distributed ferrite slurry is prepared, which solves the problem of radial shrinkage after permanent magnet ferrite sintering, improves magnetic performance and production efficiency, and reduces the cost.

CN118993719AInactive Publication Date: 2024-11-22DONGYANG FIRST MAGNETICS CO LTD

Patent Information

Application Number
CN202411499336.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The permanent magnet ferrite undergoes radial shrinkage after sintering, which affects the magnetic performance and product dimensional accuracy, resulting in large fluctuations in grinding volume, high cost and low economic benefits.

Method used

By preparing compounded non-ionic surfactants and bio-based surfactants, the adsorption behavior of ferrite particles at the oil-water interface is improved, and a mixed solvent of ionic liquid and non-ionic surfactants is combined to prepare a uniformly distributed slurry to reduce sintering During the process, the cavity is formed to control the radial shrinkage rate.

Benefits of technology

The ferrite particles are uniformly distributed, the radial shrinkage rate is reduced, the magnetic performance and production efficiency are improved, and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993719A_ABST
    Figure CN118993719A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of permanent magnetic ferrite materials, in particular to a method for regulating and controlling radial shrinkage of permanent magnetic ferrite. The preparation method comprises the following steps: proportioning and ball-milling; preparing a compound non-ionic surface active agent; preparing a mixed solvent; preparing a bio-based surfactant; preparing slurry; and carrying out compression molding and detection. According to the invention, the lauramide propyl dimethyl amine oxide and the triton are compounded to prepare the compound nonionic surfactant, and the interaction force of molecular long chains of the lauramide nonionic surfactant and the sorbitol nonionic surfactant is relatively strong, so that the adsorption behavior of ferrite particles on an oil-water interface can be improved; the interface activity of ferrite particles in an oily system and an aqueous system is improved, the metal particles of the prepared slurry are uniformly distributed, and agglomeration is reduced, so that cavities possibly formed in the sintering process are reduced, and the purpose of controlling the radial shrinkage rate of the permanent magnetic ferrite is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of permanent magnetic ferrite materials, and in particular to a method for regulating radial contraction of permanent magnetic ferrite. Background Art

[0002] At present, permanent ferrites are usually manufactured using a relatively simple ceramic process in industrial production. Compared with the size of the green sheet after wet pressing, the green sheet after sintering usually shrinks to a certain extent, which also affects the magnetic properties of the permanent ferrite.

[0003] In order to ensure the dimensional accuracy of permanent magnet ferrite products, the cooked blank is ground after sintering. The large fluctuation of shrinkage rate leads to large fluctuation of subsequent grinding amount, which makes it difficult to achieve efficient automated production. In addition, too large shrinkage rate means that the volume of the permanent magnet ferrite finished product is insufficient, and the cost of the permanent magnet ferrite product is too high, thereby reducing the economic benefit. Therefore, the present invention provides a method for regulating the radial shrinkage of permanent magnet ferrite to solve the above technical problems. Summary of the invention

[0004] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for regulating the radial contraction of permanent ferrite.

[0005] A method for regulating radial contraction of a permanent ferrite comprises the following steps: S1: Batching and ball milling The following components are weighed and added according to mass percentage: CaCO3: 0.8%-1%, La2O3: 0.6%-0.8%, CoO: 0.2%-0.4%, SiO2: 0.1%-0.25%, sorbitol: 0.1%-0.25%, HBO3: 0.1%-0.3%, and the rest is strontium ferrite wet pressed powder, and ball milled and dried to obtain a mixed powder; S2: Preparation of compound nonionic surfactant The composite nonionic surfactant is prepared by mixing lauramide propyl dimethylamine oxide and Triton; S3: Preparation of mixed solvent The ionic liquid [BMIM] BF4 is mixed with a compound nonionic surfactant to prepare a mixed solvent; S4: Preparation of bio-based surfactants N-dodecyl succinic anhydride and L-leucine are suspended in acetone and DMAP is added to react to obtain a colorless oily liquid product, the colorless oily liquid product is reacted with 2-(2-butoxyethoxy)ethanol, HATU and DIPEA to prepare a succinic acid derivative surfactant, and the product is compounded with hydroxyethyl cellulose to obtain a bio-based surfactant; S5: Preparation of slurry The mixed powder is immersed in a bio-based surfactant and a mixed solvent is added, urea is added after magnetic stirring to obtain a treatment solution, the treatment solution is allowed to stand for reaction to obtain a dark brown precipitate, and a slurry is obtained after washing; S6: Pressing and testing The slurry obtained in step S5 is pressed and sintered to obtain a blank, which is then ground and then tested for magnetic properties and appearance defects. When the requirements are met, a finished permanent ferrite is obtained.

[0006] Furthermore, step S1 batching and ball milling comprises the following steps: S1.1: Weigh and add the following ingredients according to mass percentage: CaCO3: 0.8%-1%, La2O3: 0.6%-0.8%, CoO: 0.2%-0.4%, SiO2: 0.1%-0.25%, sorbitol: 0.1%-0.25%, HBO3: 0.1%-0.3%, and the rest is strontium ferrite wet pressed powder to obtain wet powder; S1.2: Divide the wet powder into two equal parts and pour them into two ball mills respectively. At the same time, add 50% of the mass of water to mix and crush the materials in the ball mill. After the ball milling is completed, mix the materials in the two ball mills together, ball mill for 2-5 hours, and then dry for 4-6 hours to obtain a mixed powder.

[0007] Furthermore, step S2 prepares a compounded nonionic surfactant, comprising the following steps: S2.1: Add appropriate amounts of methyl laurate and triethylamine to a three-necked flask, stir and heat to 80-90°C, then add N,N-dimethyl-1,3-propylenediamine, raise the temperature to 120-160°C, reflux for 3-5h, and then distill under reduced pressure to obtain lauryl amide propyl tertiary amine; S2.2: Then, 30% of the system mass of the material in the three-necked flask is added dropwise to the three-necked flask with hydrogen peroxide, the temperature is raised to 60-80°C, and the reaction is carried out for 2-4 hours to obtain lauramide propyl dimethyl amine oxide; S2.3: Mix lauramide propyl dimethyl amine oxide and Triton in a mass ratio of 1:3 and stir for 20-25 minutes to obtain a compound nonionic surfactant.

[0008] Furthermore, step S3 of preparing a mixed solvent comprises the following steps: S3.1: First, the ionic liquid [BMIM] BF4 and the compound nonionic surfactant were placed in a vacuum drying oven at 80 °C for 8 h to remove water; S3.2: Then, the ionic liquid [BMIM] BF4 and the compound non-ionic surfactant are mixed in a mass ratio of 1:7, and magnetically stirred at a speed of 600-800r / min for 5-10min, and then benzene accounting for 25% of the total mass of the system of ionic liquid [BMIM] BF4 and the compound non-ionic surfactant is added dropwise at a rate of 1-2mL / s, and stirring is continued for 5-6h to obtain a mixed solvent.

[0009] Furthermore, step S4 prepares a bio-based surfactant, comprising the following steps: S4.1: First, 12 parts by mass of N-dodecylsuccinic anhydride and 10 parts by mass of L-leucine are suspended in 30 parts by mass of acetone, 1 part by mass of DMAP is added under stirring at room temperature, and then the temperature is raised to 40°C and stirred. After the reaction, the solvent is evaporated under reduced pressure, and column chromatography is used for separation to obtain a colorless oily liquid product; S4.2: The colorless oily liquid product was dissolved in dichloromethane, and then 11 parts by mass of 2-(2-butoxyethoxy)ethanol, 11 parts by mass of HATU, and 22 parts by mass of DIPEA were added in sequence, and the mixture was stirred at room temperature for 5-6 hours, and the solvent was removed by distillation under reduced pressure, and separated by column chromatography to obtain a succinic acid derivative surfactant; S4.3: Compound the succinic acid derivative surfactant and hydroxyethyl cellulose in a ratio of 3:1, and magnetically stir at a speed of 500-600 r / min for 10-15 min to obtain a bio-based surfactant.

[0010] Further, step S5 of preparing the slurry comprises the following steps: S5.1: Then soak the mixed powder in a bio-based surfactant, then add the mixed solvent prepared in step S3, the added amount is 80% of the system mass of the mixed powder and the bio-based surfactant, stir magnetically for 2 hours, leave at room temperature for 24 hours, and then add 5% of the system mass of urea of ​​the mixed powder and the bio-based surfactant, stir evenly, and obtain a treated liquid; S5.2: Place the treated liquid in a stainless steel reactor lined with polytetrafluoroethylene, seal it, place the reactor in a rotary oven, and let it react at 80-90°C for 4-5 hours. Filter to obtain a dark brown precipitate. After cooling the dark brown precipitate to room temperature, centrifuge it and wash it with deionized water and anhydrous ethanol respectively until it is neutral. Control the moisture content at 35%-45% to obtain a slurry.

[0011] Furthermore, step S6, compression molding and testing, includes the following steps: S6.1: Pressing the slurry obtained in step S5 to obtain a green compact with a density of 3.4-3.8 g / cm3; S6.2: Sintering the green compact at 500-550°C, with a density of 4.8-5.2 g / cm3 after sintering, to obtain a green compact; S6.3: Grind the blank, and then inspect its magnetic properties and appearance defects. When the requirements are met, the finished permanent ferrite magnet is obtained.

[0012] Furthermore, in step S2.1, the mass ratio of methyl laurate, triethylamine and N,N-dimethyl-1,3-propylenediamine is 3:0.5:2.

[0013] Furthermore, in step S4.2, the mass ratio of the colorless oily liquid product to dichloromethane is 1:6.

[0014] Furthermore, in step S5.1, the material-liquid ratio of the mixed powder and the bio-based surfactant is 1:5.

[0015] Compared with the prior art, the present invention has at least the following beneficial effects: 1. The present invention compounds lauramide propyl dimethyl amine oxide and Triton to prepare a compound nonionic surfactant. In a mixed surfactant system containing two surfactants, it can exhibit interfacial properties different from those of a single component. The chemical name of Triton is polyoxyethylene sorbitan fatty acid ester. The molecular long chains of lauramide nonionic surfactants and sorbitol nonionic surfactants have strong interaction forces, thereby improving the adsorption behavior of ferrite particles on the oil-water interface and enhancing the interfacial activity of ferrite particles in oily and aqueous systems. The prepared slurry metal particles are evenly distributed, reducing agglomeration, thereby reducing cavities that may be formed during sintering, thereby achieving the purpose of controlling the radial shrinkage rate of permanent magnet ferrite.

[0016] 2. The present invention compounds succinic acid derivatives with hydroxyethyl cellulose to prepare a bio-based surfactant. As a type of green biodegradable material derived from natural succinic acid, succinic acid derivative surfactants have good surface activity and environmental protection properties. Hydroxyethyl cellulose is a water-soluble polymer that can effectively improve the viscosity and structural stability of aqueous systems. The succinic acid derivative surfactant is used to prevent ferrite from settling and agglomerating in the aqueous system, and the stability of the suspension containing ferrite particles is maintained by hydroxyethyl cellulose. The distribution of ferrite particles inside the slurry containing water is regulated to make the slurry evenly distributed, thereby reducing the radial shrinkage rate of the permanent magnet ferrite.

[0017] 3. The present invention prepares a mixed solvent by mixing a compounded non-ionic surfactant with an ionic liquid, and uses a microemulsion composed of ionic liquid and non-ionic surfactant as the reaction system. The ionic liquid absorbs heat rapidly and evenly, and has a high heat transfer rate. The mixed solvent prepared with the ionic liquid can increase the reaction rate and make the pressed green body heated evenly, thereby reducing the radial shrinkage deviation and improving the magnetic properties of the ferrite. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.

[0019] Figure 1 The present invention is a flowchart of a method for regulating radial contraction of a permanent ferrite according to an embodiment of the present invention.

[0020] Figure 2 This is a scanning electron microscope (SEM) image of the blank in Example 1 of the present invention.

[0021] Figure 3 This is the X-ray diffraction XRD diagram of the blank in Example 1 of the present invention. DETAILED DESCRIPTION

[0022] The following is a detailed description of a method for regulating radial contraction of a permanent ferrite provided by the present invention in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternatives to implement some known technologies; and the accompanying drawings are only for a more specific description of the embodiments, and are not intended to specifically limit the present invention.

[0023] Embodiment 1:

[0024] A method for regulating radial contraction of permanent ferrite, such as Figure 1 As shown, the following steps are included: S1: Batching and ball milling S1.1: The following ingredients are weighed and added according to mass percentage: CaCO3: 0.8%, La2O3: 0.6%, CoO: 0.2%, SiO2: 0.25%, sorbitol: 0.1%, HBO3: 0.1%, and the rest is strontium ferrite wet pressed powder to obtain wet powder; S1.2: Divide the wet powder into two equal parts and pour them into two ball mills respectively. At the same time, add 50% of the system mass of water in the ball mill for mixing and crushing. After the ball milling is completed, mix the materials in the two ball mills together, ball mill for 5 hours, and then dry for 6 hours to obtain a mixed powder.

[0025] S2: Preparation of compound nonionic surfactant S2.1: Add appropriate amounts of methyl laurate and triethylamine to a three-necked flask, stir and heat to 80°C, then add N,N-dimethyl-1,3-propylenediamine, the mass ratio of methyl laurate, triethylamine and N,N-dimethyl-1,3-propylenediamine is 3:0.5:2, heat to 120°C, reflux for 3h, and distill under reduced pressure to obtain lauryl amide propyl tertiary amine; S2.2: Then, 30% of the system mass of the material in the three-necked flask is added dropwise to the three-necked flask with hydrogen peroxide, the temperature is raised to 80°C, and the reaction is carried out for 4 hours to obtain lauramide propyl dimethyl amine oxide; S2.3: Lauramide propyl dimethyl amine oxide and Triton are mixed in a mass ratio of 1:3 and stirred for 25 minutes to obtain a composite nonionic surfactant.

[0026] S3: Preparation of mixed solvent S3.1: First, the ionic liquid [BMIM] BF4 and the compound nonionic surfactant were placed in a vacuum drying oven at 80 °C for 8 h to remove water; S3.2: The ionic liquid [BMIM]BF4 and the compound non-ionic surfactant were then mixed in a mass ratio of 1:7, and magnetically stirred at a speed of 600r / min for 5 minutes. Then, benzene accounting for 25% of the total mass of the system of ionic liquid [BMIM]BF4 and the compound non-ionic surfactant was added dropwise at a rate of 2mL / s, and stirring was continued for 6h to obtain a mixed solvent.

[0027] S4: Preparation of bio-based surfactants S4.1: First, 12 parts by mass of N-dodecylsuccinic anhydride and 10 parts by mass of L-leucine are suspended in 30 parts by mass of acetone, 1 part by mass of DMAP is added under stirring at room temperature, and then the temperature is raised to 40°C and stirred. After the reaction, the solvent is evaporated under reduced pressure, and column chromatography is used for separation to obtain a colorless oily liquid product; S4.2: The colorless oily liquid product was dissolved in dichloromethane, and then 11 parts by mass of (2-(2-butoxyethoxy)ethanol, 11 parts by mass of HATU, and 22 parts by mass of DIPEA were added in sequence, and the mixture was stirred at room temperature for 5 hours, and the solvent was removed by distillation under reduced pressure, and the mixture was separated by column chromatography to obtain a succinic acid derivative surfactant; S4.3: The succinic acid derivative surfactant and hydroxyethyl cellulose were compounded in a ratio of 3:1, and magnetically stirred at a speed of 600 r / min for 10 min to obtain a bio-based surfactant.

[0028] S5: Preparation of slurry S5.1: Then soak the mixed powder in a bio-based surfactant, the solid-liquid ratio of the mixed powder to the bio-based surfactant is 1:5, and then add the mixed solvent prepared in step S3, the added amount is 80% of the system mass of the mixed powder and the bio-based surfactant, magnetic stirring for 2 hours, and place at room temperature for 24 hours, and then add 5% of the system mass of the mixed powder and the bio-based surfactant urea, stir evenly, and obtain a treated liquid; S5.2: Place the treated liquid in a stainless steel reactor lined with polytetrafluoroethylene, seal it, put the reactor into a rotary oven, and let it react at 80°C for 5 hours. Filter to obtain a dark brown precipitate. After cooling the dark brown precipitate to room temperature, centrifuge it and wash it with deionized water and anhydrous ethanol respectively until it is neutral. Control the moisture content at 35% to obtain a slurry.

[0029] S6: Pressing and testing S6.1: The slurry obtained in step S5 is pressed to obtain a green compact with a density of 3.4 g / cm 3 ; S6.2: The compact is sintered at 550°C, and the density after sintering is 4.8 g / cm 3 , and obtain the blank; S6.3: Grind the blank, and then inspect its magnetic properties and appearance defects. When the requirements are met, the finished permanent ferrite magnet is obtained.

[0030] Embodiment 2:

[0031] A method for regulating radial contraction of permanent ferrite, such as Figure 1 As shown, the following steps are included: S1: Batching and ball milling S1.1: The following ingredients are weighed and added according to mass percentage: CaCO3: 1%, La2O3: 0.8%, CoO: 0.4%, SiO2: 0.1%, sorbitol: 0.25%, HBO3: 0.3%, and the rest is strontium ferrite wet pressed powder to obtain wet powder; S1.2: Divide the wet powder into two equal parts and pour them into two ball mills respectively. At the same time, add 50% of the system mass of water in the ball mill for mixing and crushing. After the ball milling is completed, mix the materials in the two ball mills together, ball mill for 5 hours, and then dry for 6 hours to obtain a mixed powder.

[0032] S2: Preparation of compound nonionic surfactant S2.1: Add appropriate amounts of methyl laurate and triethylamine to a three-necked flask, stir and heat to 80°C, then add N,N-dimethyl-1,3-propylenediamine, the mass ratio of methyl laurate, triethylamine and N,N-dimethyl-1,3-propylenediamine is 3:0.5:2, heat to 120°C, reflux for 3h, and distill under reduced pressure to obtain lauryl amide propyl tertiary amine; S2.2: Then, 30% of the system mass of the material in the three-necked flask is added dropwise to the three-necked flask with hydrogen peroxide, the temperature is raised to 80°C, and the reaction is carried out for 4 hours to obtain lauramide propyl dimethyl amine oxide; S2.3: Lauramide propyl dimethyl amine oxide and Triton are mixed in a mass ratio of 1:3 and stirred for 25 minutes to obtain a composite nonionic surfactant.

[0033] S3: Preparation of mixed solvent S3.1: First, the ionic liquid [BMIM] BF4 and the compound nonionic surfactant were placed in a vacuum drying oven at 80 °C for 8 h to remove water; S3.2: The ionic liquid [BMIM]BF4 and the compound non-ionic surfactant were then mixed in a mass ratio of 1:7, and magnetically stirred at a speed of 600r / min for 5 minutes. Then, benzene accounting for 25% of the total mass of the system of ionic liquid [BMIM]BF4 and the compound non-ionic surfactant was added dropwise at a rate of 2mL / s, and stirring was continued for 6h to obtain a mixed solvent.

[0034] S4: Preparation of bio-based surfactants S4.1: First, 12 parts by mass of N-dodecylsuccinic anhydride and 10 parts by mass of L-leucine are suspended in 30 parts by mass of acetone, 1 part by mass of DMAP is added under stirring at room temperature, and then the temperature is raised to 40°C and stirred. After the reaction, the solvent is evaporated under reduced pressure, and column chromatography is used for separation to obtain a colorless oily liquid product; S4.2: The colorless oily liquid product was dissolved in dichloromethane, and then 11 parts by mass of (2-(2-butoxyethoxy)ethanol, 11 parts by mass of HATU, and 22 parts by mass of DIPEA were added in sequence, and the mixture was stirred at room temperature for 5 hours, and the solvent was removed by distillation under reduced pressure, and the mixture was separated by column chromatography to obtain a succinic acid derivative surfactant; S4.3: The succinic acid derivative surfactant and hydroxyethyl cellulose were compounded in a ratio of 3:1, and magnetically stirred at a speed of 600 r / min for 10 min to obtain a bio-based surfactant.

[0035] S5: Preparation of slurry S5.1: Then soak the mixed powder in a bio-based surfactant, the solid-liquid ratio of the mixed powder to the bio-based surfactant is 1:5, and then add the mixed solvent prepared in step S3, the added amount is 80% of the system mass of the mixed powder and the bio-based surfactant, magnetic stirring for 2 hours, and place at room temperature for 24 hours, and then add 5% of the system mass of the mixed powder and the bio-based surfactant urea, stir evenly, and obtain a treated liquid; S5.2: Place the treated liquid in a stainless steel reactor lined with polytetrafluoroethylene, seal it, put the reactor into a rotary oven, and let it react at 80°C for 5 hours. Filter to obtain a dark brown precipitate. After cooling the dark brown precipitate to room temperature, centrifuge it and wash it with deionized water and anhydrous ethanol respectively until it is neutral. Control the moisture content at 35% to obtain a slurry.

[0036] S6: Pressing and testing S6.1: The slurry obtained in step S5 is pressed to obtain a green compact with a density of 3.8 g / cm 3 ; S6.2: The compact is sintered at 550°C, and the density after sintering is 5.2 g / cm 3 , and obtain the blank; S6.3: Grind the blank, and then inspect its magnetic properties and appearance defects. When the requirements are met, the finished permanent ferrite magnet is obtained.

[0037] Embodiment 3:

[0038] A method for regulating radial contraction of permanent ferrite, such as Figure 1 As shown, the following steps are included: S1: Batching and ball milling S1.1: The following ingredients are weighed and added according to mass percentage: CaCO3: 0.8%, La2O3: 0.6%, CoO: 0.2%, SiO2: 0.25%, sorbitol: 0.1%, HBO3: 0.1, and the rest is strontium ferrite wet pressed powder to obtain wet powder; S1.2: Divide the wet powder into two equal parts and pour them into two ball mills respectively. At the same time, add 50% of the system mass of water in the ball mill to mix and crush. After the ball milling is completed, mix the materials in the two ball mills together, ball mill for 2 hours, and then dry for 4 hours to obtain a mixed powder.

[0039] S2: Preparation of compound nonionic surfactant S2.1: Add appropriate amounts of methyl laurate and triethylamine to a three-necked flask, stir and heat to 80°C, then add N,N-dimethyl-1,3-propylenediamine, the mass ratio of methyl laurate, triethylamine and N,N-dimethyl-1,3-propylenediamine is 3:0.5:2, heat to 160°C, reflux for 5 hours, and distill under reduced pressure to obtain lauryl amide propyl tertiary amine; S2.2: Then, 30% of the system mass of the material in the three-necked flask is added dropwise to the three-necked flask with hydrogen peroxide, the temperature is raised to 60°C, and the reaction is carried out for 2 hours to obtain lauramide propyl dimethyl amine oxide; S2.3: Lauramide propyl dimethyl amine oxide and Triton are mixed in a mass ratio of 1:3 and stirred for 20 minutes to obtain a composite nonionic surfactant.

[0040] S3: Preparation of mixed solvent S3.1: First, the ionic liquid [BMIM] BF4 and the compound nonionic surfactant were placed in a vacuum drying oven at 80 °C for 8 h to remove water; S3.2: Then, the ionic liquid [BMIM]BF4 and the compound non-ionic surfactant were mixed in a mass ratio of 1:7, and magnetically stirred at a speed of 800r / min for 10min. Then, benzene accounting for 25% of the total mass of the system of ionic liquid [BMIM]BF4 and the compound non-ionic surfactant was added dropwise at a rate of 1mL / s, and stirring was continued for 5h to obtain a mixed solvent.

[0041] S4: Preparation of bio-based surfactants S4.1: First, 12 parts by mass of N-dodecylsuccinic anhydride and 10 parts by mass of L-leucine are suspended in 30 parts by mass of acetone, 1 part by mass of DMAP is added under stirring at room temperature, and then the temperature is raised to 40°C and stirred. After the reaction, the solvent is evaporated under reduced pressure, and column chromatography is used for separation to obtain a colorless oily liquid product; S4.2: The colorless oily liquid product was dissolved in dichloromethane, and then 11 parts by mass of (2-(2-butoxyethoxy)ethanol, 11 parts by mass of HATU, and 22 parts by mass of DIPEA were added in sequence, and the mixture was stirred at room temperature for 5 hours, and the solvent was removed by distillation under reduced pressure, and the mixture was separated by column chromatography to obtain a succinic acid derivative surfactant; S4.3: The succinic acid derivative surfactant and hydroxyethyl cellulose were compounded in a ratio of 3:1, and magnetically stirred at a speed of 500 r / min for 15 minutes to obtain a bio-based surfactant.

[0042] S5: Preparation of slurry S5.1: Then soak the mixed powder in a bio-based surfactant, the solid-liquid ratio of the mixed powder to the bio-based surfactant is 1:5, and then add the mixed solvent prepared in step S3, the added amount is 80% of the system mass of the mixed powder and the bio-based surfactant, magnetic stirring for 2 hours, and place at room temperature for 24 hours, and then add 5% of the system mass of the mixed powder and the bio-based surfactant urea, stir evenly, and obtain a treated liquid; S5.2: Place the treated liquid in a stainless steel reactor lined with polytetrafluoroethylene, seal it, put the reactor into a rotary oven, and let it react at 90°C for 4 hours. Filter to obtain a dark brown precipitate. After cooling the dark brown precipitate to room temperature, centrifuge it and wash it with deionized water and anhydrous ethanol respectively until it is neutral. Control the moisture content at 35% to obtain a slurry.

[0043] S6: Pressing and testing S6.1: The slurry obtained in step S5 is pressed to obtain a green compact with a density of 3.5 g / cm 3 ; S6.2: The compact is sintered at 500°C, and the density after sintering is 4.9 g / cm 3 , and obtain the blank; S6.3: Grind the blank, and then inspect its magnetic properties and appearance defects. When the requirements are met, the finished permanent ferrite magnet is obtained.

[0044] Comparative Example 1: Compared with Example 1, the difference of Comparative Example 1 is that in step S3, lauramide propyl dimethyl amine oxide is directly mixed with the ionic liquid, specifically: "S3: preparing a mixed solvent S3.1: First, the ionic liquid [BMIM] BF4 and lauryl amide propyl dimethyl amine oxide were placed in a vacuum drying oven at 80 °C for 8 h to remove water; S3.2: Then, the ionic liquid [BMIM] BF4 and lauryl amide propyl dimethyl amine oxide were mixed in a mass ratio of 1:7, and magnetically stirred at a speed of 600 r / min for 5 min, and then 25% of the total mass of the system of the ionic liquid [BMIM] BF4 and the compounded non-ionic surfactant was added dropwise at a speed of 2 mL / s, and stirring was continued for 6 h to obtain a mixed solvent. The finished permanent ferrite prepared in step S6 was recorded as Comparative Example 1.

[0045] Comparative Example 2: Compared with Example 1, the difference of Comparative Example 2 is that in step S3, Triton is directly mixed with the ionic liquid, specifically: "S3: preparing a mixed solvent S3.1: First, the ionic liquid [BMIM]BF4 and Triton were placed in a vacuum drying oven at 80 °C for 8 h to remove water; S3.2: Then, the ionic liquid [BMIM] BF4 and Triton were mixed in a mass ratio of 1:7, and magnetically stirred at a speed of 600 r / min for 5 min, and then 25% of the total mass of the system of the ionic liquid [BMIM] BF4 and the compounded non-ionic surfactant was added dropwise at a speed of 2 mL / s, and stirring was continued for 6 h to obtain a mixed solvent. The finished permanent ferrite prepared in step S6 was recorded as Comparative Example 2.

[0046] Comparative Example 3: Compared with Example 1, the difference of Comparative Example 3 is that in step S5, a succinic acid derivative surfactant is directly used instead of a bio-based surfactant, specifically: "S5: preparing slurry S5.1: Then soak the mixed powder in a succinic acid derivative surfactant, the solid-liquid ratio of the mixed powder to the succinic acid derivative surfactant is 1:5, and then add the mixed solvent prepared in step S3, the addition amount is 80% of the system mass, magnetic stirring for 2h, let it stand at room temperature for 24h, and then add 5% of the system mass of urea, stir evenly, to obtain a treated liquid; S5.2: Place the treated liquid in a stainless steel reactor lined with polytetrafluoroethylene, seal it, place the reactor in a rotary oven, and let it stand for reaction at 80°C for 5 hours, filter to obtain a dark brown precipitate, cool the dark brown precipitate to room temperature, centrifuge it, and wash it with deionized water and anhydrous ethanol respectively until it is neutral, and control the moisture content to 35% to obtain a slurry. The finished permanent ferrite prepared in step S6 is recorded as Comparative Example 3.

[0047] Comparative Example 4: Compared with Example 1, the difference of Comparative Example 4 is that hydroxyethyl cellulose is directly used in step S5 instead of the bio-based surfactant, specifically: "S5: preparing slurry S5.1: Then soak the mixed powder in hydroxyethyl cellulose, the solid-liquid ratio of the mixed powder to hydroxyethyl cellulose is 1:5, and then add the mixed solvent prepared in step S3, the addition amount is 80% of the system mass, magnetic stirring for 2 hours, and place at room temperature for 24 hours, and then add 5% of the system mass of urea, stir evenly, to obtain a treated liquid; S5.2: Place the treated liquid in a stainless steel reactor lined with polytetrafluoroethylene, seal it, place the reactor in a rotary oven, and let it stand for reaction at 80°C for 5 hours, filter to obtain a dark brown precipitate, cool the dark brown precipitate to room temperature, centrifuge it, and wash it with deionized water and anhydrous ethanol respectively until it is neutral, and control the moisture content to 35% to obtain a slurry. The finished permanent ferrite prepared in step S6 is recorded as Comparative Example 4.

[0048] The SEM and X-ray diffraction (XRD) images of the blank of Example 1 are as follows: Figure 2 and Figure 3As shown, it can be seen from the scanning electron microscope (SEM) image that the grains inside the sintered blank in Example 1 are densely distributed and evenly dispersed, with a good and stable structure. According to the X-ray diffraction (XRD) image characterization, it can be seen that the diffraction peak in the permanent magnet ferrite blank of Example 1 is single, and no other impurities that obviously affect the chemical properties are generated.

[0049] The results of magnetic property tests on Examples 1-3 and Comparative Examples 1-4 are shown in Table 1, wherein the shrinkage ratio is the ratio of the diameter of the green compact and the green blank in step S6.

[0050] In the table, the shrinkage rates of Examples 1-3 are 1.13, 1.12 and 1.13 respectively, the remanence of Example 2 is the highest, which is 4.19 kGs, the magnetic coercivity and intrinsic coercivity of Example 3 are both the highest, which are 3.40 kOe and 3.53 kOe respectively, and the maximum magnetic energy product of Example 1 is the highest, which is 4.19 MGOe. The specific process parameters can be selected according to the needs.

[0051] The shrinkage rates of Comparative Examples 1 and 2 are 1.18 and 1.19, respectively. It can be seen that the ratio of the diameter of the compact and the blank of Comparative Examples 1-2 becomes larger, and the compact shrinks more after sintering. In addition, the remanence, magnetic coercive force and maximum magnetic energy product of Comparative Examples 1-2 are not as good as those of the embodiment. It can be seen that the non-ionic surfactant compounded with lauryl amide propyl dimethyl amine oxide and Triton has a better dispersing effect on the ferrite particles than a single component, thereby reducing the cavities that may be formed during the sintering process, thereby achieving the purpose of controlling the radial shrinkage rate of the permanent magnet ferrite.

[0052] The shrinkage rates of Comparative Examples 3 and 4 are 1.26 and 1.34, respectively. It can be seen that the succinic acid derivatives and hydroxyethyl cellulose have a better anti-settling effect on the ferrite particles, and the combined use effect is better than that of a single component, and can further reduce the shrinkage rate of the permanent magnet ferrite.

[0053] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for regulating radial contraction of permanent ferrite, characterized in that: The steps include: S1: Batching and ball milling The following components are weighed and added according to mass percentage: CaCO3: 0.8%-1%, La2O3: 0.6%-0.8%, CoO: 0.2%-0.4%, SiO2: 0.1%-0.25%, sorbitol: 0.1%-0.25%, HBO3: 0.1%-0.3%, and the rest is strontium ferrite wet pressed powder, and ball milled and dried to obtain a mixed powder; S2: Preparation of compound nonionic surfactant The composite nonionic surfactant is prepared by mixing lauramide propyl dimethylamine oxide and Triton; S3: Preparation of mixed solvent The ionic liquid [BMIM] BF4 is mixed with a compound nonionic surfactant to prepare a mixed solvent; S4: Preparation of bio-based surfactants N-dodecyl succinic anhydride and L-leucine are suspended in acetone and DMAP is added to react to obtain a colorless oily liquid product, the colorless oily liquid product is reacted with 2-(2-butoxyethoxy)ethanol, HATU and DIPEA to prepare a succinic acid derivative surfactant, and the product is compounded with hydroxyethyl cellulose to obtain a bio-based surfactant; S5: Preparation of slurry The mixed powder is immersed in a bio-based surfactant and a mixed solvent is added, urea is added after magnetic stirring to obtain a treatment solution, the treatment solution is allowed to stand for reaction to obtain a dark brown precipitate, and a slurry is obtained after washing; S6: Pressing and testing The slurry obtained in step S5 is pressed and sintered to obtain a blank, which is then ground and then tested for magnetic properties and appearance defects. When the requirements are met, a finished permanent ferrite is obtained.

2. The method for regulating radial contraction of permanent ferrite according to claim 1, characterized in that: Step S1: batching and ball milling, comprising the following steps: S1.1: Weigh and add the following ingredients according to mass percentage: CaCO3: 0.8%-1%, La2O3: 0.6%-0.8%, CoO: 0.2%-0.4%, SiO2: 0.1%-0.25%, sorbitol: 0.1%-0.25%, HBO3: 0.1%-0.3%, and the rest is strontium ferrite wet pressed powder to obtain wet powder; S1.2: Divide the wet powder into two equal parts and pour them into two ball mills respectively. At the same time, add 50% of the mass of water to mix and crush the materials in the ball mill. After the ball milling is completed, mix the materials in the two ball mills together, ball mill for 2-5 hours, and then dry for 4-6 hours to obtain a mixed powder.

3. A method for regulating radial contraction of permanent ferrite according to claim 2, characterized in that: Step S2 prepares a compound nonionic surfactant, comprising the following steps: S2.1: Add appropriate amounts of methyl laurate and triethylamine to a three-necked flask, stir and heat to 80-90°C, then add N,N-dimethyl-1,3-propylenediamine, raise the temperature to 120-160°C, reflux for 3-5h, and then distill under reduced pressure to obtain lauryl amide propyl tertiary amine; S2.2: Then, 30% of the system mass of the material in the three-necked flask is added dropwise to the three-necked flask with hydrogen peroxide, the temperature is raised to 60-80°C, and the reaction is carried out for 2-4 hours to obtain lauramide propyl dimethyl amine oxide; S2.3: Mix lauramide propyl dimethyl amine oxide and Triton in a mass ratio of 1:3 and stir for 20-25 minutes to obtain a compound nonionic surfactant.

4. The method for regulating radial contraction of permanent ferrite according to claim 3, characterized in that: Step S3 prepares a mixed solvent, comprising the following steps: S3.1: First, the ionic liquid [BMIM] BF4 and the compound nonionic surfactant were placed in a vacuum drying oven at 80 °C for 8 h to remove water; S3.2: Then, the ionic liquid [BMIM] BF4 and the compound non-ionic surfactant are mixed in a mass ratio of 1:7, and magnetically stirred at a speed of 600-800r / min for 5-10min, and then benzene accounting for 25% of the total mass of the system of ionic liquid [BMIM] BF4 and the compound non-ionic surfactant is added dropwise at a rate of 1-2mL / s, and stirring is continued for 5-6h to obtain a mixed solvent.

5. The method for regulating radial contraction of permanent ferrite according to claim 4, characterized in that: Step S4 prepares a bio-based surfactant, comprising the following steps: S4.1: First, 12 parts by mass of N-dodecylsuccinic anhydride and 10 parts by mass of L-leucine are suspended in 30 parts by mass of acetone, 1 part by mass of DMAP is added under stirring at room temperature, and then the temperature is raised to 40°C and stirred. After the reaction, the solvent is evaporated under reduced pressure, and column chromatography is used for separation to obtain a colorless oily liquid product; S4.2: The colorless oily liquid product was dissolved in dichloromethane, and then 11 parts by mass of 2-(2-butoxyethoxy)ethanol, 11 parts by mass of HATU, and 22 parts by mass of DIPEA were added in sequence, and the mixture was stirred at room temperature for 5-6 hours, and the solvent was removed by distillation under reduced pressure, and separated by column chromatography to obtain a succinic acid derivative surfactant; S4.3: Compound the succinic acid derivative surfactant and hydroxyethyl cellulose in a ratio of 3:1, and magnetically stir at a speed of 500-600 r / min for 10-15 min to obtain a bio-based surfactant.

6. The method for regulating radial contraction of permanent ferrite according to claim 5, characterized in that: Step S5 is preparing slurry, comprising the following steps: S5.1: Then soak the mixed powder in a bio-based surfactant, then add the mixed solvent prepared in step S3, the added amount is 80% of the system mass of the mixed powder and the bio-based surfactant, stir magnetically for 2 hours, leave at room temperature for 24 hours, and then add 5% of the system mass of urea of ​​the mixed powder and the bio-based surfactant, stir evenly, and obtain a treated liquid; S5.2: Place the treated liquid in a stainless steel reactor lined with polytetrafluoroethylene, seal it, place the reactor in a rotary oven, and let it react at 80-90°C for 4-5 hours. Filter to obtain a dark brown precipitate. After cooling the dark brown precipitate to room temperature, centrifuge it and wash it with deionized water and anhydrous ethanol respectively until it is neutral. Control the moisture content at 35%-45% to obtain a slurry.

7. The method for regulating radial contraction of permanent ferrite according to claim 6, characterized in that: Step S6: pressing and testing, including the following steps: S6.1: Pressing the slurry obtained in step S5 to obtain a green compact with a density of 3.4-3.8 g / cm3; S6.2: Sintering the green compact at 500-550°C, with a density of 4.8-5.2 g / cm3 after sintering, to obtain a green compact; S6.3: Grind the blank, and then inspect its magnetic properties and appearance defects. When the requirements are met, the finished permanent ferrite magnet is obtained.

8. The method for regulating radial contraction of permanent ferrite according to claim 7, characterized in that: In step S2.1, the mass ratio of methyl laurate, triethylamine and N,N-dimethyl-1,3-propylenediamine is 3:0.5:

2.

9. The method for regulating radial contraction of permanent ferrite according to claim 8, characterized in that: The mass ratio of the colorless oily liquid product to dichloromethane in step S4.2 is 1:

6.

10. The method for regulating radial contraction of permanent ferrite according to claim 9, characterized in that: The material-liquid ratio of the mixed powder and the bio-based surfactant in step S5.1 is 1:5.

Citation Information

Patent Citations

  • Preparation method of permanent ferrite material

    CN110372365A

  • Additive for preparing permanent magnetic strontium ferrite material and application of additive

    CN114907130A

  • High-squareness permanent magnetic strontium ferrite magnetic material and preparation method thereof

    CN114956801A

  • Preparation method of microwave auxiliary ion liquid body of nanometer micropowder

    CN1559663A

  • Pourable molding compound containing sinterable powders

    US5190898A

Cited By

  • High-performance ultrathin rare earth permanent magnet sheet and preparation method thereof

    CN119694774A