Moisture-curable polyurethane resin composition, adhesive, and laminate
By using isocyanate-based moisture-hardened polyurethane resin composition, the problem of adhesion hinderment caused by water repellent is solved, excellent adhesion and feel of water repellent blanks are achieved, and manufacturing efficiency and product performance are improved. .
Patent Information
- Application Number
- CN202410306173.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2024-03-18
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing moisture-permeable waterproof functional clothing, the use of a water repellent leads to the adhesion of the adhesion agent, and when the water repellent blank is used, the adhesion agent penetrates into the blank, affecting the feel and manufacturing efficiency.
Using a moisture-hardened polyurethane resin composition with isocyanate groups, a monoester having three hydroxyl groups is added by the reaction product of a polyol and a polyisocyanate as a prepolymer to improve surface energy and adhesion. Also, preferred polyols and polyisocyanates are used to obtain excellent adhesion and feel.
Excellent adhesion and feel of the water-repellent blank is achieved without requiring a large amount of coating, which improves manufacturing efficiency and product performance.
Smart Images

Figure BDA0004745912710000111 
Figure BDA0004745912710000112
Abstract
Description
Technical Field
[0001] The present invention relates to a moisture-curing polyurethane resin composition, an adhesive and a laminate. Background Art
[0002] The moisture-permeable and waterproof functional clothing having both moisture permeability and waterproofness is a structure formed by bonding a moisture-permeable film to a blank through an adhesive, and as the adhesive, a urethane adhesive is generally used in terms of good adhesion to both the moisture-permeable film and the blank. In addition, among the urethane adhesives, the use of solvent-free moisture-curing polyurethane resin compositions is gradually increasing due to recent global restrictions on solvent discharge or residual solvents (for example, refer to Patent Document 1).
[0003] On the other hand, in order to make it water-repellent, a water-repellent blank obtained by impregnating a water-repellent agent in a blank and drying it is used in a moisture-permeable and waterproof functional clothing. In the past, a fluorine-based water-repellent agent was used for the water-repellent agent. However, with the restriction of the use of fluorine in the world, in addition to switching from fluorine called C8 to C6 fluorine, the action of defluorination is also accelerated, and a substance called C0 long-chain alkyl or silicon-based substance is used as a raw material for the water-repellent agent replacing fluorine. These water-repellent agents are materials with low surface energy, so although they show the water-repellent required in the moisture-permeable and waterproof functional clothing, on the other hand, they cause the adhesion of the adhesive to be hindered. In the case of applying the adhesive to the moisture-permeable film and then laminating it with the non-water-repellent blank to form a structure and then performing water-repellent processing, the above-mentioned adhesion will not be caused, but there is a problem in terms of increasing the process. On the other hand, in the case of using a water-repellent blank, when the adhesive is applied to the film, sufficient adhesion is not shown when laminating, so a method of increasing the amount of adhesive is considered, but because it is a clothing use, it will have a bad effect on the feel. In general, there is a manufacturing method in which an adhesive is applied to a water-repellent base material and the base material is bonded to a moisture-permeable film. However, the adhesive is applied to the base material and penetrates into the base material, which adversely affects the hand feel.
[0004] [Prior art literature]
[0005] [Patent Document]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2017-202608 Summary of the invention
[0007] [Problems to be solved by the invention]
[0008] The problem to be solved by the present invention is to provide a moisture-curable polyurethane resin composition having excellent adhesion to a base material (especially a water-repellent base material) and excellent texture.
[0009] [Technical means to solve the problem]
[0010] The present invention provides a moisture-curing polyurethane hot-melt resin composition, which contains a urethane prepolymer (i) having an isocyanate group, wherein the urethane prepolymer (i) having an isocyanate group is a reaction product of a polyol (A) and a polyisocyanate (B), and the moisture-curing polyurethane hot-melt resin composition is characterized in that the polyol (A) contains a monoester (a1) of a compound having three hydroxyl groups as an essential component.
[0011] The present invention also provides an adhesive comprising the moisture-curing polyurethane resin composition. The present invention also provides a laminate comprising at least a raw material (i) and a cured product of the moisture-curing polyurethane resin composition.
[0012] [Effects of the Invention]
[0013] The moisture-curable polyurethane hot-melt resin composition of the present invention not only has an excellent hand feel, but also has excellent adhesion to various blanks and also has excellent adhesion to water-repellent blanks. In addition, the moisture-curable polyurethane hot-melt resin composition can also obtain excellent film strength. DETAILED DESCRIPTION
[0014] The moisture-curable polyurethane hot-melt resin composition used in the present invention contains a urethane prepolymer (i) which is a reaction product of a polyol (A) containing a specific compound and a polyisocyanate (B) and has an isocyanate group.
[0015] In terms of obtaining excellent adhesion to a base material (especially a water-repellent base material) and a good feel, the polyol (A) contains a monoester (a1) of a compound having three hydroxyl groups as an essential component. Since the monoester (a1) having a hydrophobic functional group is grafted onto the urethane prepolymer (i), the polymer itself is further hydrophobized, and thus the difference in surface energy with respect to an adherend having a low surface energy is reduced, thereby exhibiting excellent adhesion to a water-repellent base material in particular. Furthermore, since excellent adhesion can be obtained without applying a large amount of coating, it also contributes to an excellent feel.
[0016] The monoester (a1) of the compound having three hydroxyl groups is a substance in which one hydroxyl group of the compound having three hydroxyl groups is esterified by a monocarboxylic acid. As the compound having three hydroxyl groups, for example, glycerol, trimethylolpropane, a polypropylene polyol having three hydroxyl groups, 1,2,4-butanetriol, etc. can be used. Among these, glycerol, trimethylolpropane, or a polypropylene polyol having three hydroxyl groups is preferred in terms of obtaining better adhesion to water-repellent raw materials. As the monocarboxylic acid, for example, a substance having an alkyl group having 8 to 22 carbon atoms can be used, and in terms of obtaining better adhesion to water-repellent raw materials, the carbon number is preferably 14 to 22.
[0017] The amount of the monoester (a1) used is preferably 0.5 to 15.0% by mass, more preferably 1.0 to 10.0% by mass, in the polyol (A) in order to obtain better adhesion to a water-repellent material.
[0018] In addition to the monoester (a1), the polyol (A) may also use other polyols. As the other polyols, for example, polyether polyols, polyester polyols, polycarbonate polyols, polyacrylic acid polyols, polybutadiene polyols, etc. may be used. These polyols may be used alone or in combination of two or more. Among these, polyether polyols and / or polyester polyols are preferably used in terms of obtaining better flexibility and adhesion.
[0019] As the polyether polyol, for example, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, etc. can be used. These polyols can be used alone or in combination of two or more. In addition, plant-derived polyether polyols can be used as the polyether polyol. As the plant-derived polyether polyol, for example, "Bio PTMG" manufactured by Mitsubishi Chemical Co., Ltd., "Bio (Bio) PTG" manufactured by Hodogaya Chemical Co., Ltd., and biomass polypropylene glycol manufactured by Vithal Castor Polyols can be obtained as commercial products. In terms of obtaining better flexibility and adhesion, the amount used when using the polyether polyol is preferably 20% to 60% by mass in the polyol (A).
[0020] As the polyester polyol, for example, a reaction product of a compound having two or more hydroxyl groups and a polybasic acid can be used. As the compound having two or more hydroxyl groups, for example, ethylene glycol, diethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, pentanediol, 2,4-diethyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, hexanediol, neopentyl glycol, hexamethylene glycol, glycerol, trimethylolpropane, bisphenol A or bisphenol F and its alkylene oxide adducts can be used. In addition, as the polybasic acid, for example, adipic acid, glutaric acid, pimelic acid, suberic acid, dimer acid, sebacic acid, undecanedicarboxylic acid, hexahydroterephthalic acid, phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, etc. can be used. In terms of obtaining better mechanical strength and adhesion, the amount used when using the polyester polyol is preferably 40% to 70% by mass in the polyol (A).
[0021] The number average molecular weight of the other polyol is, for example, 500 to 100,000. The number average molecular weight of the other polyol refers to a value measured by gel permeation chromatography (GPC).
[0022] As the polyisocyanate (B), aromatic polyisocyanates such as polymethylene polyphenyl polyisocyanate, diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, xylene diisocyanate, phenylene diisocyanate, toluene diisocyanate, and naphthalene diisocyanate can be used; aliphatic or alicyclic polyisocyanates such as hexamethylene diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and tetramethylxylene diisocyanate can be used. These polyisocyanates can be used alone or in combination of two or more. Among these, aromatic polyisocyanates are preferred, and diphenylmethane diisocyanate is more preferred in terms of obtaining better reactivity and adhesion to the blank.
[0023] The amount of the polyisocyanate (B) used is preferably 5% by mass to 40% by mass, more preferably 10% by mass to 30% by mass, based on the total mass of the raw materials constituting the urethane prepolymer (i).
[0024] The urethane prepolymer (i) is obtained by reacting the polyol (A) with the polyisocyanate (B), and has an isocyanate group that can react with moisture in the air or in a substrate coated with the moisture-curing polyurethane hot-melt resin composition to form a crosslinked structure.
[0025] The urethane prepolymer (i) can be produced, for example, by placing the polyisocyanate (B) in a reaction vessel containing the polyol (A) and reacting the polyisocyanate (B) under conditions in which the isocyanate group of the polyisocyanate (B) is in excess relative to the hydroxyl group of the polyol (A).
[0026] The equivalent ratio (isocyanate group / hydroxyl group) of the isocyanate group of the polyisocyanate (B) to the hydroxyl group of the polyol (A) when producing the urethane prepolymer (i) is preferably 1.1 to 5, more preferably 1.5 to 3, in order to obtain better adhesion to the blank.
[0027] The isocyanate group content (hereinafter referred to as "NCO%") of the urethane prepolymer (i) obtained by the above method is preferably 1.5 to 10, and more preferably 2 to 6, from the viewpoint of obtaining more excellent adhesiveness. The NCO% of the urethane prepolymer (i) is a value measured by potentiometric titration in accordance with Japanese Industrial Standards (JIS) K1603-1:2007.
[0028] The moisture-curable polyurethane hot-melt resin composition used in the present invention contains the above-mentioned urethane prepolymer (i) as an essential component, but other additives may be used as necessary.
[0029] Examples of the other additives include light stabilizers, curing catalysts, tackifiers, plasticizers, stabilizers, fillers, dyes, pigments, fluorescent brighteners, silane coupling agents, waxes, thermoplastic resins, etc. These additives may be used alone or in combination of two or more.
[0030] Next, the laminated body of the present invention will be described.
[0031] The laminated body of the present invention comprises at least a raw material (i) and a cured product of the moisture-curing polyurethane hot-melt resin composition.
[0032] As the blank (i), for example, the following fiber substrates can be used: polyester fiber, polyethylene fiber, nylon fiber, acrylic fiber, polyurethane fiber, acetate fiber, rayon fiber, polylactic acid fiber, cotton, linen, silk, wool, glass fiber (glassfibre), carbon fiber, and blended fibers thereof, such as nonwoven fabrics, woven fabrics, and braided fabrics; nonwoven fabrics impregnated with resins such as polyurethane resins; nonwoven fabrics having a porous layer further disposed therein; resin substrates, etc.
[0033] In addition, in the present invention, the blank (i) is a blank obtained by subjecting the above-mentioned blank to water repellency treatment (hereinafter referred to as "water repellent blank"), and exhibits excellent adhesion. In addition, in the present invention, the "water repellency" of the water repellent blank is set to be level 4 or above in the water repellency test (spray test) of JIS L 1092:2020.
[0034] In the water repellency test (spray test) of JIS L 1092:2020, after a test piece of about 200 mm × 200 mm is mounted on a test piece holding frame in a wrinkle-free manner, the center of the spray is aligned with the center of the holding frame, and the longitudinal direction of the test piece is aligned in parallel with the flow direction of water, and is inclined at 45 degrees. 250 ml of water adjusted to 20°C ± 3°C is sprayed on the test piece fixed to the holding frame for 25 to 30 seconds. After spraying, excess water drops are dripped off, and after wiping off the water drops remaining on the surface of the test piece, the wet state of the water on the test piece is compared with the wet state of the comparison sample specified in JIS, and a judgment is made on a 1 to 5-level scale.
[0035] 5-level water drop separation, no trace after wiping off
[0036] 4-level water drop separation, no trace after wiping off
[0037] Level 3: No penetration when dripping, but traces after wiping off
[0038] 2nd level dripping and then penetrating
[0039] Level 1 Complete Penetration
[0040] Examples of methods for applying the moisture-curing polyurethane hot-melt resin composition include methods using a roll coater, a knife coater, a spray coater, a gravure roll coater, a notch wheel coater, a T-die coater, an applicator, a dispenser, and the like.
[0041] After the moisture-curable polyurethane hot-melt resin composition is applied, it is dried and cured by a known method.
[0042] The thickness of the cured product of the moisture-curing polyurethane hot-melt resin composition is, for example, in the range of 5 μm to 300 μm.
[0043] In addition, when the moisture-curing polyurethane hot-melt resin composition of the present invention is used as an adhesive for moisture-permeable and waterproof functional clothing, the moisture-curing polyurethane hot-melt resin composition is preferably intermittently coated by a gravure roll coater or a dispenser to bond the blank (i) to a known moisture-permeable film. In the above case, the thickness of the cured product of the moisture-curing polyurethane hot-melt resin composition is, for example, in the range of 5 μm to 50 μm.
[0044] [Example]
[0045] Hereinafter, the present invention will be described in more detail using examples.
[0046] [Example 1]
[0047] In a four-necked flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux cooler, 41 parts by mass of polypropylene glycol (number average molecular weight: 1,000, hereinafter referred to as "PEt-1"), 33 parts by mass of polypropylene glycol (number average molecular weight: 2,000, hereinafter referred to as "PEt-2"), and 55 parts by mass of polyester polyol (reaction product of 1,6-hexanediol and phthalic acid, number average molecular weight: 2,000, hereinafter referred to as "PEs-1") were mixed. ”), 20 parts by mass of polyester polyol (reaction product of neopentyl glycol and phthalic acid, number average molecular weight: 1,000, hereinafter referred to as “PEs-2”), 39 parts by mass of polyester polyol (reaction product of 1,6-hexanediol and sebacic acid, number average molecular weight: 3,500, hereinafter referred to as “PEs-3”), and 16 parts by mass of capric acid monoester of trimethylolpropane, and dehydrated to a water content of 0.05% by mass or less by heating under reduced pressure at 100°C. Then, after cooling to 90°C, 49 parts by mass of diphenylmethane diisocyanate melted at 70°C was added, and the temperature was raised to 110°C, and the reaction was carried out for 3 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer, thereby preparing a moisture-curing polyurethane hot-melt resin composition.
[0048] [Example 2]
[0049] 16 parts by mass of PEt-1, 65 parts by mass of PEt-2, 35 parts by mass of PEs-1, 35 parts by mass of PEs-2, 47 parts by mass of PEs-3, and 6 parts by mass of stearic acid monoester of glycerol were mixed in a four-necked flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux cooler, and dehydrated to a water content of 0.05% by mass or less by heating under reduced pressure at 100° C. Then, after cooling to 90° C., 53 parts by mass of diphenylmethane diisocyanate melted at 70° C. was added, and the temperature was raised to 110° C. and reacted for 3 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer, thereby preparing a moisture-curing polyurethane hot-melt resin composition.
[0050] [Example 3]
[0051] In a four-necked flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux cooler, 65 parts by mass of PEt-2, 31 parts by mass of PEs-1, 49 parts by mass of PEs-2, 49 parts by mass of polyester polyol (reaction product of 1,6-hexanediol and adipic acid, number average molecular weight: 4,500, hereinafter referred to as "PEs-4"), and 10 parts by mass of stearic acid monoester of trimethylolpropane were mixed, and dehydrated to a water content of 0.05% by mass or less by heating under reduced pressure at 100° C. Then, after cooling to 90° C., 57 parts by mass of diphenylmethane diisocyanate melted at 70° C. was added, and the temperature was raised to 110° C., and the reaction was carried out for 3 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer, thereby preparing a moisture-curing polyurethane hot-melt resin composition.
[0052] [Example 4]
[0053] In a four-necked flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux cooler, 53 parts by mass of PEt-1, 53 parts by mass of PEt-2, 55 parts by mass of PEs-1, 20 parts by mass of PEs-2, 39 parts by mass of PEs-3, and 4 parts by mass of stearic acid monoester of glycerol were mixed, and dehydrated to a water content of 0.05% by mass or less by heating under reduced pressure at 100° C. Then, after cooling to 90° C., 68 parts by mass of diphenylmethane diisocyanate melted at 70° C. was added, and the temperature was raised to 110° C. and reacted for 3 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer, thereby preparing a moisture-curing polyurethane hot-melt resin composition.
[0054] [Example 5]
[0055] In a four-necked flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux cooler, 48 parts by mass of PEs-2, 10 parts by mass of PEs-3, 133 parts by mass of polyester polyol (a reaction product of diethylene glycol and sebacic acid, number average molecular weight: 2,000, hereinafter referred to as "PEs-5"), and 13 parts by mass of capric acid monoester of glycerol were mixed, and dehydrated to a water content of 0.05% by mass or less by heating under reduced pressure at 100°C. Then, after cooling to 90°C, 37 parts by mass of diphenylmethane diisocyanate melted at 70°C was added, and the temperature was raised to 110°C, and the reaction was carried out for 3 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer, thereby preparing a moisture-curing polyurethane hot-melt resin composition.
[0056] [Example 6]
[0057] 69 parts by mass of PEt-2, 24 parts by mass of PEs-1, 43 parts by mass of PEs-2, 43 parts by mass of PEs-4, and 24 parts by mass of behenic acid monoester of glycerol were mixed in a four-necked flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux cooler, and dehydrated to a water content of 0.05% by mass or less by heating under reduced pressure at 100° C. Then, after cooling to 90° C., 54 parts by mass of diphenylmethane diisocyanate melted at 70° C. was added, and the temperature was raised to 110° C. and reacted for 3 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer, thereby preparing a moisture-curing polyurethane hot-melt resin composition.
[0058] [Example 7]
[0059] 31 parts by mass of PEt-1, 41 parts by mass of PEt-2, 31 parts by mass of PEs-1, 45 parts by mass of PEs-2, 49 parts by mass of PEs-4, and 8 parts by mass of behenic acid monoester of trimethylolpropane were mixed in a four-necked flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux cooler, and dehydrated to a water content of 0.05% by mass or less by heating under reduced pressure at 100° C. Then, after cooling to 90° C., 64 parts by mass of diphenylmethane diisocyanate melted at 70° C. was added, and the temperature was raised to 110° C., and the reaction was carried out for 3 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer, thereby preparing a moisture-curing polyurethane hot-melt resin composition.
[0060] [Example 8]
[0061] In Example 1, a moisture-curing polyurethane hot-melt resin composition was obtained in the same manner as in Example 1, except that 41 parts by mass of PEt-1 was replaced with a biomass polypropylene glycol (number average molecular weight: 1,000) manufactured by Vithal Castor Polyols, and 33 parts by mass of PEt-2 was replaced with a biomass polypropylene glycol (number average molecular weight: 2,000) manufactured by Vithal Castor Polyols.
[0062] [Comparative Example 1]
[0063] 75 parts by mass of PEt-2, 31 parts by mass of PEs-1, 49 parts by mass of PEs-2, and 49 parts by mass of PEs-4 were mixed in a four-necked flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux cooler, and dehydrated to a water content of 0.05% by mass or less by heating under reduced pressure at 100° C. Then, after cooling to 90° C., 48 parts by mass of diphenylmethane diisocyanate melted at 70° C. was added, and the temperature was raised to 110° C. and reacted for 3 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer, thereby preparing a moisture-curing polyurethane hot-melt resin composition.
[0064] [Method for determining number average molecular weight]
[0065] The number average molecular weight of the polyol used in Examples and Comparative Examples refers to a value measured by gel permeation chromatography (GPC) under the following conditions.
[0066] Measuring device: High-speed GPC device ("HLC-8220GPC" manufactured by Tosoh Corporation)
[0067] Column: The following columns manufactured by Tosoh Corporation were connected in series and used.
[0068] "TSKgel G5000" (7.8mm inner diameter (ID) × 30cm) × 1 piece
[0069] "TSKgel G4000" (7.8mm I.D. × 30cm) × 1 piece
[0070] "TSKgel G3000" (7.8mm I.D. × 30cm) × 1 piece
[0071] "TSKgel G2000" (7.8mm I.D. × 30cm) × 1 piece
[0072] Detector: RI (differential refractometer)
[0073] Column temperature: 40℃
[0074] Eluent: Tetrahydrofuran (THF)
[0075] Flow rate: 1.0mL / min
[0076] Injection volume: 100 μL (sample concentration is 0.4 mass% tetrahydrofuran solution)
[0077] Standard sample: The following standard polystyrene was used to prepare a standard curve.
[0078] (Standard Polystyrene)
[0079] "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation
[0080] "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation
[0081] "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation
[0082] "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation
[0083] "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation
[0084] "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation
[0085] "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation
[0086] "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation
[0087] "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation
[0088] "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation
[0089] "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation
[0090] "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation
[0091] "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation
[0092] "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation
[0093] [Evaluation method of adhesion to blank material]
[0094] The moisture-curable polyurethane hot-melt resin compositions obtained in the examples and comparative examples were melted at 100° C. and coated using a gravure roll coater (coating amount: 17.5 g / m 2 ±5g / m 2 ) was intermittently coated on a moisture permeable film (Crisvon S-517 manufactured by DIC Corporation processed into a 15 μm film) and respectively attached to a water-repellent blank 1 (a polyester blank (manufactured by the Japan Standards Association, warp and weft: 75D / 36f-FDY, unit area weight: 71.8 g / m 2 ) treated with a water repellent (Neoside NR-8800 manufactured by Nichia Chemical Co., Ltd., water repellency level 5; hereinafter referred to as "blank 1") and water repellent blank 2 (a polyester blank (manufactured by the Japan Standards Association, warp and weft: 75D / 36f-FDY, unit area weight: 71.8g / m 2 ) was treated with a water repellent (NEOSEED NR-7080 manufactured by Nichika Chemical Co., Ltd., with a water repellency of level 5; hereinafter referred to as "blank 2"), and placed in an environment of temperature 23°C and humidity 50% for 24 hours to obtain a processed cloth. Each processed cloth obtained was cut into 1 inch width, and the peel strength was measured using Tensilon (Tensilon universal machine "RTC-1210A" manufactured by Orientec Co., Ltd.) at a crosshead speed of 200 mm / min, and evaluated as follows.
[0095] "T": 6N / cm or more.
[0096] "F": less than 6N / cm.
[0097] [Evaluation method of hand feel]
[0098] The processed cloth obtained in the above [Evaluation method for adhesion to blanks] was cut into pieces 1 inch wide and 8 cm long, and the test piece was folded in half using a precision universal testing machine ("Autograph AG-1" manufactured by Shimadzu Corporation), and installed in a manner such that the 5 cm long portion of the folded portion protrudes toward the upper part of the clamping fixture with an arc, and the stress at a displacement of 5 mm when the flat indenter is pressed under a test speed of 10 mm / min was measured, and evaluated in the following manner.
[0099] "T": 100mN or less
[0100] "F": more than 100mN
[0101] [Evaluation method of film properties]
[0102] The moisture-curing polyurethane hot-melt resin composition obtained in the examples and comparative examples was melted at 100°C, and then applied to a flat release paper ("EK-100D" manufactured by Lintec Co., Ltd.) with a thickness of 30 μm using a roll coater, and left to stand for 24 hours in an environment of a temperature of 23°C and a humidity of 50% to obtain a film. The obtained film was cut into a strip of 5 mm in width and 50 mm in length, and stretched using a precision universal testing machine "Autograph AG-NX" (manufactured by Shimadzu Corporation) at a chuck distance of 40 mm, a tensile speed of 10 mm / sec, a temperature of 23°C, and a humidity of 50%, and the stress at 100% elongation was measured and evaluated as follows.
[0103] "T": less than 10MPa.
[0104] "F": 10MPa or above.
[0105] [Table 1]
[0106]
[0107] [Table 2]
[0108]
[0109] It is found that the moisture-curable polyurethane hot-melt resin composition of the present invention has excellent adhesion to a water-repellent base material, texture, and film properties.
[0110] On the other hand, in Comparative Example 1, the monoesterified product (a1) was not used, and the evaluation of the adhesiveness with the blank was poor.
Claims
1. A moisture-curable polyurethane hot-melt resin composition, comprising a urethane prepolymer (i) having an isocyanate group, wherein the urethane prepolymer (i) having an isocyanate group is a reaction product of a polyol (A) and a polyisocyanate (B), wherein the moisture-curable polyurethane hot-melt resin composition is characterized in that: The polyol (A) contains a monoesterified product (a1) of a compound having three hydroxyl groups as an essential component.
2. The moisture-curing polyurethane hot-melt resin composition according to claim 1, in, The monoester (a1) has a structure derived from a monocarboxylic acid having 8 to 22 carbon atoms.
3. The moisture-curing polyurethane hot-melt resin composition according to claim 1, in, The compound having three hydroxyl groups is glycerol, trimethylolpropane, or polypropylene polyol having three hydroxyl groups.
4. The moisture-curing polyurethane hot-melt resin composition according to claim 1, in, The usage-amount of the said monoester (a1) is 0.5 mass % - 15.0 mass % in the said polyol (A).
5. The moisture-curing polyurethane hot-melt resin composition according to claim 1, in, The polyol (A) further contains at least one selected from polyether polyol and polyester polyol.
6. An adhesive, It is characterized in that The moisture-curable polyurethane hot-melt resin composition according to claim 1 is contained.
7. A laminate, It is characterized in that The invention comprises at least a blank (i) and a cured product of the moisture-curing polyurethane hot-melt resin composition according to claim 1.
8. The laminate according to claim 7, in, The blank (i) is a water-repellent blank.