Preparation method and application of water-soluble conductive polyaniline

By using NMP/H2O solvent and sodium bisulfite as sulfonate in polyaniline synthesis, the problems of medium and high cost and dangerous materials for hydrophilic modification of polyaniline are solved, and the high conductivity and water solubility of polyaniline are achieved. Suitable for the preparation of flexible electrochromic films, it has the potential for industrial application.

CN118994571AActive Publication Date: 2024-11-22UNIV OF SCI & TECH OF CHINA

Patent Information

Application Number
CN202411213447.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The existing polyaniline hydrophilic modification methods have problems such as high cost, hazardous material use, complex preparation processes and reduced conductivity, making it difficult to achieve simple, low-cost water-soluble and high conductivity polyaniline preparation.

Method used

Polyaniline is synthesized using NMP/H2O as a mixed solvent, and sodium bisulfite or sodium sulfite is used as a sulfonating agent to make the polyaniline hydrophilic modification. By regulating the reaction conditions, sulfonated polyaniline with both water solubility and conductivity is obtained. , used to prepare flexible electrochromic films.

Benefits of technology

It realizes the hydrophilic modification of polyaniline under simple and mild conditions, with high conductivity and water solubility, and is suitable for the preparation of large-area flexible electrochromic films, and has practical guiding significance for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994571A_ABST
    Figure CN118994571A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of water-soluble conductive polyaniline. The preparation method comprises the following steps: introducing NMP into an aniline polymerization system, synthesizing polyaniline by taking NMP / H2O as a mixed solvent so as to regulate the molecular weight of the polyaniline, and then carrying out hydrophilic modification on the polyaniline by taking sodium hydrogen sulfite or sodium sulfite as a sulfonating agent. The method is simple in preparation, mild in condition and free of a template, and the modified product has water solubility and conductivity, can be used for preparing a large-area flexible electrochromic film, and has practical guiding significance for industrial production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional polymers, and in particular relates to a preparation method of water-soluble conductive polyaniline and application thereof. Background Art

[0002] As one of the three major conductive polymers, polyaniline (PANI) exhibits excellent thermal stability at temperatures up to 250°C and can be easily synthesized by chemical oxidation polymerization and electrochemical methods. In addition, due to its low cost, excellent environmental stability, good conductivity and other advantages, polyaniline has attracted much attention in the fields of electrochromism, electromagnetic interference shielding, solar cells, bio / chemical sensors and anti-corrosion functions. Compared with polypyrrole and polythiophene, it has irreplaceable advantages. However, due to its rigid main chain and the strong π-π stacking and hydrogen bonding between chains, polyaniline lacks solution processability and can only be dissolved in very few specific organic solvents, such as NMP, DMF, DMSO, etc. However, the boiling points of these organic solvents are as high as 150°C or above, and the boiling point of NMP is even more than 200°C. High boiling point solvents make it difficult to remove after processing and generally have certain toxicity. Improving the hydrophilicity of polyaniline has become the best strategy to enhance its processability. In order to realize this strategy, researchers have done a lot of work. Currently, there are two main methods: (1) Add hydrophilic sulfonic acid groups to the main chain of polyaniline. Polyaniline is usually sulfonated with fuming sulfuric acid or chlorosulfonic acid, which can greatly improve the water solubility of polyaniline. Yue et al. dissolved polyaniline emerald base in fuming sulfuric acid to prepare sulfonated polyaniline with an S / N of 0.5, but the product can only be dissolved in sodium hydroxide or ammonia water, which loses its practical application value (J. Am. Chem. Soc. 1990, 112, 7, 2800-2801). Shoji Ito et al. sulfonated polyaniline with chlorosulfonic acid. When the sulfonation degree (S / N) was 0.65, the product solubility was 22 mg / mL and the conductivity was 0.028 S / cm. When the sulfonation degree was 0.80, the product solubility was 51 mg / mL and its conductivity was 5.72×10 -3S / cm (Synthetic Metals 1998, 96, 161-163). It can be seen that the improvement of the water solubility of the product of this method is at the expense of conductivity. Moreover, fuming sulfuric acid and chlorosulfonic acid are extremely dangerous and are not conducive to practical production applications. Another method is to copolymerize aniline and m-aminobenzenesulfonic acid (MA). The disadvantage is that the different reactivity of the two monomers easily leads to uneven copolymer segments, and the product can only be dissolved in alkaline aqueous solution (Journal of Polymer Science Part A: Polymer Chemistry 2000, 38, 3390-3398). (2) Grafting hydrophilic polymers on the main chain of polyaniline, or synthesizing polyaniline in situ using hydrophilic polymers / nanoparticles as templates. Du et al. in situ polymerized aniline in the presence of chitosan, grafted chitosan onto polyaniline chains to make it dispersed in water, and then synthesized Chi-g-polyaniline-polyacrylamide hydrogel with acrylamide monomer (ACS Appl. Mater. Interfaces 2023, 15,23711-23724). Lv Yitong et al. used poly (2-acrylamide-2-methylpropanesulfonic acid) (PAMPS) as a doping acid and emulsifier, and utilized its unique long chain, hydrophilicity and strong acidic group effects to synthesize conductive polyaniline with high solubility in one step through emulsion polymerization. The polyaniline obtained by this method is soluble in water and has high conductivity. The reagents used are not dangerous, but other polymers need to be introduced, the preparation method is cumbersome, and the cost is high. In summary, the current methods for hydrophilic modification of polyaniline have corresponding defects. Therefore, it is very necessary to find a method for hydrophilic modification of polyaniline with a simple preparation method and low cost.

[0003] Electrochromic materials can stably and reversibly change their optical properties under the action of an applied electric field, and have important application prospects in energy-saving windows, smart displays, and military camouflage protection. Polyaniline has become a widely studied conductive polymer electrochromic material due to its simple preparation, low cost, rich color changes, and fast response time. The color change of polyaniline is within the applied potential range of ±1V, and its electrochemical redox process is closely related to the change of absorption spectrum in the visible light range (400-800 nm). The electrochromicity of polyaniline and the related differences in visible light transmission have led to the development of electrochromic displays and windows combined with complementary electrochromic materials.

[0004] At present, the main methods for preparing polyaniline electrochromic materials are electropolymerization, enzyme synthesis and solution processing (spin coating, blade coating, spray coating, etc.). For the electropolymerization method, the deposition of polyaniline is affected by the current density and the surface state of the electrode, which makes it difficult to accurately control the film thickness and uniformity, poor reproducibility, and not conducive to large-scale production. The enzyme synthesis method has the disadvantages of expensive enzymes, sensitivity to storage conditions, limited reaction conditions, and difficulty in large-scale production. The solution processing method has become the first strategy for preparing polyaniline electrochromic layers due to its good reproducibility, good coating uniformity, and suitability for large-scale production. The realization of the solution processing method requires hydrophilic modification of polyaniline. However, most of the current reports on the preparation of electrochromic materials by polyaniline solution processing mainly focus on grafting hydrophilic polymers on the main chain of polyaniline, or in situ synthesis of polyaniline using hydrophilic polymers / nanoparticles as templates, and the preparation process of this method is cumbersome and costly. Summary of the invention

[0005] The present invention aims at the deficiencies of the above-mentioned prior art and provides a method for preparing water-soluble conductive polyaniline and its application. The present invention introduces NMP into the aniline polymerization system, that is, NMP / H2O is used as a mixed solvent to synthesize polyaniline to regulate its molecular weight, and then sodium bisulfite or sodium sulfite is used as a sulfonating agent to hydrophilically modify the polyaniline. This method is simple to prepare, mild in conditions, and does not require a template. The modified product has both water solubility and conductivity, can be used for the preparation of large-area flexible electrochromic films, and has practical guiding significance for industrial production and application.

[0006] The method for preparing the water-soluble conductive polyaniline of the present invention comprises the following steps: Step 1: Synthesis of PANI Aniline monomer was dissolved in NMP / H2O mixed solvent, placed in a 0℃ ice water bath and stirred for 10 minutes; ammonium persulfate (APS) solid was dissolved in hydrochloric acid and then added dropwise to the aniline solution; after the addition was complete, the polymerization system was kept at 0℃ for one hour; after the reaction was completed, PANI was washed with deionized water and centrifuged, and the operation was repeated 5 times. After the last washing, it was filtered to obtain PANI solid.

[0007] Step 2: SPAN synthesis The PANI obtained in step 1 is dissolved in a NMP / H2O mixed solvent, stirred and dispersed evenly, the sulfonation reagent is dissolved in water and added to the reaction system, and reacted at 60-70°C for 0.5-2h; after the reaction is completed, the product SPAN is washed with deionized water and centrifuged, and the operation is repeated until the pH of the supernatant is 3-4.

[0008] The volume ratio of NMP to H2O in the NMP / H2O mixed solvent is 1:1 to 1:5.

[0009] The sulfonating agent is a water-soluble bisulfite or sulfite, preferably sodium bisulfite or sodium sulfite.

[0010] The molar ratio of the sulfonating agent to the aniline monomer is 1:1-1:5, and more preferably 1:2 to 1:4.

[0011] The polyaniline prepared by the present invention is a conjugated polymer composed of an oxidation unit quinone structure and a reduction unit benzene structure. The present invention adopts a chemical oxidation polymerization method to prepare the polyaniline, and the solvent is NMP and water. By adjusting the ratio of the two, polyaniline with different molecular weights can be obtained, and the molecular weight range of the polyaniline is 10,000-30,000.

[0012] The method for preparing a flexible electrochromic film using the water-soluble conductive polyaniline comprises the following steps: SPAN is dissolved in water, and the supernatant is taken after centrifugation to obtain a SPAN solution; a surfactant is added to the SPAN solution to obtain a coating liquid; and then a SPAN electrochromic film is prepared on an ITO-PET substrate by spin coating, scraping or spraying.

[0013] The concentration of the SPAN solution is 3-6 mg / mL.

[0014] The volume ratio of the surfactant to the SPAN solution is 1:15-1:25.

[0015] The surfactant includes polyethylene glycol octylphenyl ether (Triton X-100). The purpose of adding the surfactant is to increase the wettability and spreadability of the solution on the ITO-PET substrate.

[0016] The coating solution also includes PVP. The original SPAN solution can meet the requirements of spin coating, but its viscosity is too low for spraying and scraping, so PVP is added to thicken it to meet the requirements of scraping and spraying. In addition, PVP is polyvinyl pyrrolidone, and the carbonyl oxygen combines with the H on the N of the SPAN molecular chain through a hydrogen bond, making the molecular chain more stretched, which plays a role in stabilizing the SPAN solution.

[0017] The preparation method of SPAN electrochromic film is exemplified as follows: The SPAN electrochromic film was prepared by spin coating. The specific steps are as follows: Dissolve a certain amount of SPAN in water, centrifuge at a certain rate, take the supernatant, make the solution concentration 3-6 mg / ml, and obtain SPAN solution. Add 40-65 μL Ttiton X-100 to the SPAN solution to obtain the coating solution. Cut the ITO-PET into a rectangular block of 20 mm×35 mm in size and place it on the chassis of the spin coater. Take a certain amount of coating solution and spread it evenly on the substrate, with a speed of 700-1000 r / min for 4-6 seconds, heat and dry, and repeat the above spin coating steps 1-8 times to obtain a uniform SPAN electrochromic film.

[0018] The SPAN electrochromic film was prepared by the blade coating method. The specific steps are as follows: Dissolve a certain amount of SPAN in water, centrifuge at a certain rate, take the supernatant, and make the solution concentration 3-6 mg / ml to obtain SPAN solution. Add PVP to SPAN solution, stir to dissolve, and then add 40-65 μL Triton X-100 solution to SPAN-PVP solution to obtain coating solution. Take a certain amount of coating solution and spread it on one side of 30mm×60mm ITO-PET to form an area of ​​about 5mm×30mm, use a 50-200 μm wire rod to scrape the solution to the other side, heat and dry, and you will get SPAN electrochromic film.

[0019] The SPAN electrochromic film is prepared by spraying method, and the specific steps are as follows: Dissolve a certain amount of SPAN in water, centrifuge at a certain rate, take the supernatant, and make the solution concentration 3-6 mg / ml to obtain SPAN solution. Add PVP to the SPAN solution, stir and dissolve, and then add an appropriate amount of Triton X-100 solution to the SPAN-PVP solution to obtain a coating solution. Cut the ITO-PET into a rectangular block of 40mm×60 mm in size, and attach the hollow mask to its surface. Add the coating solution to the airbrush gun and spray the ITO-PET with the mask for 3-5 seconds. Heat and dry the film, peel off the mask, and you can get an electrochromic film with the corresponding pattern.

[0020] The method for preparing an electrochromic device using the flexible electrochromic film comprises the following steps: The SPAN electrochromic film is used as the positive electrode and the poly (3,4-ethylenedioxythiophene) (PEDOT) film is used as the negative electrode, an electrolyte solution is injected in the middle (the electrolyte solution formula is: 0.4g LiClO4 is added to 12ml PC, stirred until dissolved, and then 3g polymethyl methacrylate is added and stirred until dissolved), and then the device is placed under ultraviolet light for a certain period of time to obtain a SPAN-PEDOT electrochromic device.

[0021] The PEDOT film is prepared in the same way as the preparation of SPAN, that is, a proper amount of Triton X-100 is added to the PEDOT: PSS solution, and the solution is used as a coating to prepare the PEDOT film by spin coating, blade coating or spray coating.

[0022] The PEDOT: PSS solution is commercially available. Specifically, the PEDOT: PSS solution is diluted 5 times, and then 1 ml of the diluted solution is taken, and 40-65 μL Triton-X (the volume ratio of Triton-X to the solution is 1:15-1:25) is added, and this is used as a coating to prepare a PEDOT film by spin coating, blade coating or spray coating.

[0023] The SPAN-PEDOT electrochromic device of the present invention has large optical modulation amplitude, fast response time and excellent cycle stability.

[0024] The process of preparing sulfonated polyaniline of the present invention is divided into two steps, namely, the synthesis of polyaniline and the sulfonation modification of polyaniline. In the first step, the present invention uses NMP / H2O as a solvent to synthesize polyaniline. Since NMP (N-methylpyrrolidone) is a good solvent for polyaniline, the addition of NMP will affect the polymerization rate of aniline, so polyaniline with different molecular weights can be obtained by adjusting the content of NMP. In the second step, the present invention uses sodium bisulfite or sodium sulfite as a sulfonating agent to sulfonate polyaniline (the reaction mechanism is as follows). Since the sulfonation degree, water solubility and conductivity of polyaniline with different molecular weights are different under different conditions, sulfonated polyaniline (SPAN) with both water solubility and conductivity can be obtained by controlling the conditions for synthesizing polyaniline and the conditions for sulfonation.

[0025]

[0026] The sulfonation mechanism of sodium bisulfite on polyaniline is different from that of oleum / chlorosulfonic acid. It is a relatively common nucleophilic reagent and is usually used for nucleophilic addition to aldehyde and ketone carbonyl groups. The "C=C" on the quinone ring of polyaniline becomes electron-deficient due to the protonated imine nitrogen atom and has nucleophilic addition activity. Therefore, the present invention uses sodium bisulfite or sodium sulfite as a nucleophilic reagent to perform nucleophilic addition on the quinone ring of polyaniline, so that the main chain of polyaniline is connected to the sulfonic acid group, which improves its water solubility and does not cause degradation to polyaniline. This method is simple to prepare, has mild conditions, low cost, and does not require the introduction of other hydrophilic substances.

[0027] The present invention utilizes spin coating, scraping coating, spraying and other techniques to process the modified polyaniline aqueous solution to prepare a flexible large-area and patterned electrochromic film, and uses PEDOT as a counter electrode to assemble an electrochromic device with high optical contrast, fast response time and excellent cycle stability. The device has broad application prospects and is expected to generate huge social and economic value. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 XRD spectra of PANI, SPAN (1:2), SPAN (1:3) and SPAN (1:4). After sulfonation, the diffraction peak of SPAN is not as sharp as that of PANI. This is because the sulfonic acid groups on the PANI molecular chain increase the steric hindrance between the segments and the gaps between the segments, which reduces the crystallinity of polyaniline and weakens the degree of conjugation.

[0029] Figure 2 FT-IR spectra of PANI, SPAN(1:2), SPAN(1:3) and SPAN(1:4). 1073 and 1019 cm -1 They are the O=S=O symmetric and asymmetric stretching vibration peaks, 704 cm -1 The peaks corresponded to the symmetric stretching vibration of SO, which indicated the successful synthesis of SPAN.

[0030] Figure 3 UV-Vis spectra of PANI, SPAN (1:2), SPAN (1:3) and SPAN (1:4). The two absorption peaks of polyaniline are near 365 nm and 625 nm, respectively. The absorption peak at 365 nm is the absorption peak of the π-π* electron transition of the benzene ring, and the absorption peak at 625 nm is the absorption peak of the PANI polaron / bipolaron transition. Compared with PANI, the peak of SPAN at 625 nm red-shifts with the increase of the sulfonation degree, that is, the bipolaron / polaron transition becomes easier after sulfonation, which may be due to the additional protonation of the sulfonic acid group and the formation of a self-doped six-membered stable ring structure, thereby improving the stability of the conjugated system.

[0031] Figure 4 Cyclic voltammetry curve of SPAN film prepared by spin coating in 0.1 mol / L LiClO4 / PC. The voltage range is -0.4 to 1.2 V, and the scan rate is 0.05 V / s. When scanning in the forward direction, two oxidation peaks appear at about 0.35 V and about 0.9 V, respectively, corresponding to the changes between the reduction of polyaniline salt-emeraldine salt and emeraldine salt-polyparaphenylene imide salt, respectively. The polyaniline film will appear yellow-green, green and blue in turn; when scanning in the reverse direction, two reduction peaks appear at about 0.66 V and about 0.07 V, corresponding to the reversible process of the forward scan.

[0032] Figure 5 Color change of SPAN film in LiClO4 / PC. As the voltage changes from -0.4 to 1.2 V, SPAN undergoes a yellow-green-green-blue transition.

[0033] Figure 6(a) Transmittance curve (300-800 nm) of the SPAN film after six spin coatings from -0.4 to 1.2 V; (b) Time response curve of the SPAN film. The light modulation amplitude of the SPAN film reaches 44.7% at a wavelength of 684 nm, the coloring time is 2.7 seconds, and the fading time is 2 seconds.

[0034] Figure 7 Color change of the SPAN-PEDOT device between -1.2 and 1.4 V. The device is green at low voltage and dark blue-purple at high voltage.

[0035] Figure 8 (a) Transmittance curve of the SPAN-PEDOT device prepared by spin coating at 300-800 nm; (b) Time response curve of the SPAN-PEDOT device. The light modulation amplitude of the device at 582 nm reaches 40.1%, the coloring time is 2.2 seconds, and the fading time is 1.8 seconds.

[0036] Fig. 9 (a) CV graphs of the SPAN-PEDOT device at the beginning and after 1000, 2000, 3000, 4000, and 5000 color change cycles; (b) Curve graph of the cyclic stability of the SPAN-PEDOT device tested by the potential step method.

[0037] Fig.10 (a) Transmittance curve of SPAN-PEDOT device prepared by scraping method at 300-800 nm; (b) Time response curve of SPAN-PEDOT device. The light modulation amplitude of the device reaches 39.4% at 582 nm, the coloring time is 2.5 seconds, and the fading time is 2 seconds.

[0038] Fig.11 (a) CV graphs of the SPAN-PEDOT device at the beginning and after 1000, 2000, 3000, 4000, and 5000 color change cycles; (b) Curve graph of the cyclic stability of the SPAN-PEDOT device tested by the potential step method.

[0039] Fig.12 A large-area (60 mm × 60 mm) SPAN-PEDOT device fabricated by blade coating was demonstrated.

[0040] Fig.13 Color change diagram of SPAN-PEDOT patterned electrochromic device prepared by spray coating. DETAILED DESCRIPTION

[0041] The technical solution of the present invention is further analyzed and explained below through specific embodiments.

[0042] Example 1: Synthesis of PANI 1. Dissolve 3.6 g aniline in 15 ml NMP and 25 ml 1 mol / L hydrochloric acid, and stir at 0°C. Dissolve 9.13 g APS in 20 ml 1 mol / L hydrochloric acid, and then drop the APS solution into the aniline solution at a rate of 3-5 seconds / drop.

[0043] 2. After the addition is complete, the polymerization system is allowed to react for one hour.

[0044] 3. After the reaction is completed, the product PANI is washed with deionized water and centrifuged, and the operation is repeated 5 times. After the last washing, the product is filtered to obtain a dark green PANI solid.

[0045] Example 2: Sodium bisulfite is used in the synthesis of SPAN 1. Disperse the PANI obtained in the previous step in 9 ml NMP and 27 ml water and stir to make it evenly dispersed.

[0046] 2. Dissolve 2.08 g of sodium bisulfite in 6 ml of water (the molar ratio of sodium bisulfite to aniline monomer in the PANI synthesis step is 1:2), add to the reaction system, and react at 65°C for 1 hour.

[0047] 3. After the reaction is completed, the dark green product SPAN is washed with deionized water and centrifuged, and the operation is repeated until the pH of the supernatant is 3-4.

[0048] Example 3: Sodium bisulfite is used in the synthesis of SPAN 1. Disperse the PANI obtained in the previous step in 9 ml NMP and 27 ml water, stir to make it dispersed evenly. Adjust the pH of the reaction system to 2-4 with acetic acid.

[0049] 2. Dissolve 2.52 g of sodium sulfite in 6 ml of water (the molar ratio of sodium sulfite to aniline monomer in the PANI synthesis step is 1:2), add it to the reaction system, and react at 65°C for 1 hour.

[0050] 3. After the reaction is completed, the dark green product SPAN is washed with deionized water and centrifuged, and the operation is repeated until the pH of the supernatant is 3.5.

[0051] Table 1 shows the molecular weight of polyaniline synthesized at different NMP / H2O ratios.

[0052] Table 2 shows the optimal NMP / H2O solvent ratio for the sulfonation of polyaniline synthesized at different NMP / H2O ratios. The molecular weight of each sample is different, resulting in different dispersibility in NMP / H2O. Sodium bisulfite is poorly soluble in NMP, so the optimal solvent ratio for sulfonation is different for each sample.

[0053] Table 3 shows the sulfonation degree (S / N), conductivity and solubility of polyaniline synthesized in different NMP / H2O solvent ratios at different n(sodium bisulfite) / n(ANI) ratios. It can be seen that different molecular weights of polyaniline lead to different conductivity. As the amount of NaHSO3 increases, the sulfonation degree increases, the solubility increases, and the conductivity decreases.

[0054]

[0055]

[0056]

[0057] Example 4: Preparation of SPAN film by spin coating 1. Dissolve 1 g SPAN (1:2) in 5 ml water, centrifuge at 3000 r / min, and take the supernatant to obtain SPAN solution. Add 60 μL of Ttiton X-100 to the SPAN solution to obtain a coating solution.

[0058] 2. Ultrasonic clean the ITO-PET in toluene, acetone, ethanol, and deionized water for 10 minutes respectively, and then dry it. Cut the ITO-PET into a rectangular block of 20 mm × 35 mm and place it on the chassis of the spin coater. Take 1 mL of the coating liquid and spread it evenly on the substrate at a speed of 900 r / min for 5 seconds to obtain a uniform SPAN film.

[0059] 3. Place the SPAN film in a 65°C oven and dry it for a while, then take it out and repeat the above spin coating steps 6 times.

[0060] Example 5: Assembly of SPAN-PEDOT electrochromic device prepared by spin coating 1. Take 1 ml of PEDOT: PSS solution, add 60 μL Triton X-100, and then take out 50 μL of the coating solution and spread it on ITO-PET. The speed is 900 r / min and the time is 5 seconds to obtain a uniform PEDOT film.

[0061] 2. Use the SPAN film as the positive electrode and the PEDOT film as the negative electrode, inject the electrolyte solution in the middle, and then place the device under ultraviolet light for 5 minutes to obtain the SPAN-PEDOT electrochromic device.

[0062] Example 6: Preparation of SPAN film by blade coating 1. Dissolve 1 g SPAN in 5 ml water, centrifuge at 3000 r / min, and take the supernatant to obtain SPAN solution. Add 0.1 g PVP to 10 ml SPAN solution, stir and dissolve to obtain SPAN-PVP solution.

[0063] 2. Add 60 μL Triton X-100 solution to 1 ml SPAN-PVP solution, take 50 μL of the solution and spread it on one side of the 30 mm×60 mm ITO-PET to form an area of ​​about 5 mm×30 mm, use a 100 μm wire rod to scrape the solution to the other side, and dry it at 65°C to obtain the SPAN electrochromic film.

[0064] The steps of assembling the SPAN-PEDOT device prepared by the scraping coating method provided by the present invention and testing its electrochromic performance are consistent with those of the spin coating method.

[0065] Example 7: Preparation of SPAN patterned electrochromic film by spraying 1. Dissolve 1 g SPAN in 5 ml water, centrifuge at 3000 r / min, and take the supernatant to obtain SPAN solution. Add 0.1 g PVP to 10 ml SPAN solution, stir and dissolve to obtain SPAN-PVP solution.

[0066] 2. Cut the ITO-PET into a rectangular block of 40 mm × 60 mm in size, and stick the hollow mask printed with "EC" on it. Add 300 μL Triton X-100 solution to 5 ml SPAN-PVP solution, pour the spray liquid into the airbrush gun, and spray the ITO-PET with the mask for 4 seconds.

[0067] 3. Dry the film at 65°C. Remove the mask to obtain an electrochromic film printed with an "EC" pattern.

[0068] The PEDOT patterned electrochromic film was prepared in the same way. The SPAN film and the PEDOT film were assembled to obtain a patterned electrochromic device. The performance test steps of SPAN flexible electrochromic film are as follows:

[0069] (1) The SPAN membrane was placed in a three-electrode system as the working electrode, with a platinum wire as the counter electrode, Ag / AgCl as the reference electrode, and LiClO4 / propylene carbonate (PC) as the electrolyte. The electrochemical workstation was connected and a cyclic voltammetry scan test was performed within a certain voltage range to record the CV curve.

[0070] (2) Place the entire device in the colorimetric cell of a UV-visible spectrophotometer, use the blank electrolyte as a reference, and use the voltage step method to test the transmission spectra of the SPAN membrane in the faded and colored states in the range of 300-800 nm. Find the wavelength corresponding to the maximum transmittance difference of the spectrum, and use this as a single wavelength to test the coloration / fading time of the SPAN membrane. The electrochromic performance test steps of SPAN-PEDOT device are as follows:

[0071] The CV curves were recorded using an electrochemical workstation within a certain voltage range. The transmission spectra of the device in the faded and colored states within the range of 300-800 nm were recorded using a UV-visible spectrophotometer to test the coloration / fading time of the device. The cyclic color change performance of the SPAN-PEDOT device within a certain voltage range was tested using the step method.

[0072] Table 4 shows the light modulation amplitude and coloring / fading time of the SPAN film with different spin coating times. It can be seen that the light modulation amplitude of the SPAN film with 6 spin coating times is the largest.

[0073]

Claims

1. A method for preparing water-soluble conductive polyaniline, characterized in that: Polyaniline was synthesized using NMP / H2O as a mixed solvent to regulate its molecular weight, and then the polyaniline was hydrophilically modified by sulfonation to obtain water-soluble conductive polyaniline.

2. The preparation method according to claim 1, characterized in that The steps include: Step 1: Synthesis of PANI Aniline monomer is dissolved in NMP / H2O mixed solvent, placed in a 0°C ice water bath and stirred for 10 minutes; ammonium persulfate solid is dissolved in hydrochloric acid, and then added dropwise to the aniline solution; after the addition is complete, the polymerization system is kept at 0°C for reaction; after the reaction is completed, PANI is washed with deionized water, centrifuged, and filtered to obtain PANI solid; Step 2: SPAN synthesis The PANI obtained in step 1 is dissolved in a NMP / H2O mixed solvent, stirred and dispersed evenly, the sulfonation reagent is dissolved in water and added to the reaction system, and reacted at 60-70°C for 0.5-2h; after the reaction is completed, the product SPAN is washed with deionized water and centrifuged, and the operation is repeated until the pH of the supernatant is 3-4.

3. The preparation method according to claim 2, characterized in that The volume ratio of NMP to H2O in the NMP / H2O mixed solvent is 1:1 to 1:

5.

4. The preparation method according to claim 2, characterized in that The sulfonating agent is a water-soluble bisulfite or sulfite.

5. The preparation method according to claim 4, characterized in that The sulfonating agent is sodium bisulfite or sodium sulfite.

6. The preparation method according to claim 4, characterized in that The molar ratio of the sulfonating agent to the aniline monomer is 1:1-1:

5.

7. A flexible electrochromic film prepared by using the water-soluble conductive polyaniline obtained by the preparation method according to any one of claims 1 to 6, characterized in that The steps include: SPAN is dissolved in water, and the supernatant is taken after centrifugation to obtain a SPAN solution; a surfactant is added to the SPAN solution to obtain a coating liquid; and then a SPAN electrochromic film is prepared on an ITO-PET substrate by spin coating, scraping or spraying.

8. The method according to claim 7, characterized in that: The concentration of the SPAN solution is 3-6 mg / mL.

9. An electrochromic device constructed using the flexible electrochromic film prepared according to claim 7 or 8, characterized in that: The SPAN electrochromic film is used as the positive electrode, the poly (3,4-ethylenedioxythiophene) film is used as the negative electrode, an electrolyte solution is injected in the middle, and then the device is placed under ultraviolet light to obtain a SPAN-PEDOT electrochromic device.

Citation Information

Patent Citations

  • Preparation method of water-soluble conductive polyaniline

    CN102604087A

  • Method for preparing soluble aniline and derivatives with various molecular wt.

    CN1141310A

  • Method for preparing fusible conductive polyaniline

    CN1415645A

  • Sulfonated aliphatic compounds

    US5919976A

  • Method of processing electrically conductive polyanilines in solvent mixtures

    WO1992011644A1

Cited By

  • Water-based carbon-coated aluminum foil coating and preparation method thereof

    CN121343484A