Preparation and application method of carbon-silicon-based polymer soil conditioner capable of enhancing crop stress resistance
By using straw waste and methyl silicone oil and other materials in Xinjiang for prepolymerization, a carbon-silica-based polymer soil conditioner with water-retaining and salt absorption function was prepared, which solved the problem of crop growth in salinization and drought environments. It improves the water retention and stress resistance of the soil, achieves an increase in crop yield, and reduces preparation costs and pollution risks.
Patent Information
- Application Number
- CN202411181928.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
AI Technical Summary
Salt-alkali soil and drought environment in Xinjiang have limited crop growth. The existing soil conditioner components lack synergies, making it difficult to effectively improve the soil's water retention and stress resistance. In addition, harmful solvents are often used during the preparation process, which poses a risk of pollution. .
Prepolymerization reaction with reactants such as methyl silicone oil, urea, potassium persulfate, etc. is prepared to retain water and salt absorption function, and then the carbon silicon-based polymer material is prepared with calcium lignin sulfonate, Polyacrylamide and other polymerization reactions form a soil conditioner that enhances crop stress resistance.
This soil conditioner improves the soil's water and fertilizer retention ability, enhances the stress resistance of crops, reduces the harm of salinization to crops, achieves a continuous increase in crop yield, and reduces the preparation cost and pollution risk.
Smart Images

Figure CN118994603A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of soil remediation, and specifically relates to a preparation method of a carbon-silicon-based polymer soil conditioner capable of enhancing crop stress resistance and an application method thereof. Background Art
[0002] Medium and low-yield fields not only have low soil organic matter nutrient content, but also have other environmental factors that limit crop production, which is an important factor hindering the continuous increase of my country's grain production. The total cultivated land area in Xinjiang irrigation area is about 90 million mu, of which about 35 million mu is salinized, accounting for 37.7% of the total cultivated land area. Soil salinization refers to the phenomenon that salt in the bottom of the soil rises to the surface with water and accumulates in the soil arable layer. In the saline soil environment, crops are forced to absorb Na + , Cl - , resulting in salt ion poisoning of crops, causing plant physiological drought, making crops unable to grow or even die. In addition, due to the high temperature and low rainfall in Xinjiang all year round, nearly 2 / 3 of the land suffers from drought damage, which seriously affects the sustainable development of Xinjiang agriculture. Although Xinjiang has promoted sub-film drip irrigation technology on a large scale, which has reduced the impact of drought on crop growth to a certain extent, the technology is currently unable to solve this problem fundamentally. Therefore, developing a soil conditioner, how to increase the content of soil organic matter, maintain soil nutrients, and maximize soil moisture retention is a fundamental solution to the defects of regional geographical and climatic characteristics. Patent CN107841314A discloses a soil conditioner, the core components of which include organic components such as amino acids and citric acid, which can regulate the pH value of the soil, alleviate soil salt damage, and achieve the goal of low cost and high return. Patent CN103756685A discloses a soil conditioner, the main components of which include humic acid, attapulgite powder, potassium feldspar powder, etc. The conditioner has the function of regulating the pH of the soil and activating the nutrients in the soil, thereby enhancing the salt-alkali resistance of crops and playing a good saline-alkali soil improvement effect. Although the above-mentioned soil conditioners contain organic, inorganic and biological components, the components are simply mixed without forming a complex, which reduces the synergy between the components and makes it difficult to exert the long-term effectiveness of the materials.
[0003] In recent years, researchers have used straw biomass raw materials to prepare a series of highly absorbent materials. Patent CN202111513908.9 discloses a straw-based water-absorbing and water-retaining agent and a preparation method thereof. After pre-treating the straw with urea alkaline solution, the etherifying agent propylene oxide is added for etherification reaction, and catalysts such as formaldehyde are added for reaction to prepare a water-retaining material with water absorption capacity. Although the preparation method uses cheap straw as the base material, the preparation process adds a certain toxic organic reaction solvent, which is easy to cause secondary pollution problems. Patent CN201710718420.7 discloses a straw biomass-based water-retaining agent and a preparation method thereof. After the straw is treated with yeast fermentation, acrylic acid, ammonium persulfate, and N,N methylenebisacrylamide are added and mixed and reacted to prepare a straw-based material with water absorption capacity. This method needs to react in a nitrogen environment, which is difficult to form large-scale production.
[0004] In response to the outstanding problems of continuous soil salinization and decreased quality of the tillage layer, the present invention utilizes cheap and readily available straw waste, adds methyl silicone oil, urea, potassium persulfate, potassium thiosulfate and other reactants, obtains carbon-containing silicon-based natural polymer materials with water-retaining and salt-absorbing functions through prepolymerization, and prepares soil conditioners with enhanced crop resistance through a series of polymerization reactions with calcium lignin sulfonate, polyacrylamide and the like. The conditioner is polymerized from organosilicon, organic polymer water-retaining materials and other trace element components, has the functions of water-retaining and fertilizer-retaining, and can also prevent physiological drought of crops caused by soil salinization, thereby improving soil structure, enhancing crop resistance, promoting crop growth, and achieving a continuous increase in crop yields. Summary of the invention
[0005] The present invention establishes a method for preparing a carbon-silicon-based polymer soil conditioner capable of enhancing crop stress resistance and its application method. The method uses straw waste and urea, persulfate and other pretreatments to prepare a carbon-silicon-based natural polymer material, and through a series of prepolymerization reactions, prepares a soil conditioner with water-retaining and salt-absorbing functions. The soil conditioner has a simple synthesis process and low cost, and can be used on a large scale to improve saline-alkali land, improve the soil's ability to retain water and fertilizer, enhance crop stress resistance, and thus increase crop yields.
[0006] The technical solution of the present invention:
[0007] A method for preparing a carbon-silicon-based polymer soil conditioner capable of enhancing crop stress resistance comprises the following steps:
[0008] (1) 20-30 parts by weight of powdered straw, 1-5 parts by weight of methyl silicone oil as a branching monomer, 1-2 parts by weight of urea as an activator, and 10-20 parts by weight of N,N-dimethylformamide as a reaction solution are mixed thoroughly and allowed to stand at room temperature for 5-8 hours to allow the methyl silicone oil to fully penetrate into the cellulose hydroxyl surface of the straw powder and obtain a natural network branched macromolecular complex containing silicone oil through the hydrogen bond protection formed by the urea amino group and the branching monomer; then 1-2 parts by weight of potassium hydroxide are added in sequence to adjust the pH of the reaction solution, 5-10 parts by weight of potassium thiosulfate as a reducing agent, and 1-2 parts by weight of ammonium persulfate as an initiator and an oxidant, and the mixture is stirred thoroughly, and a grafting and polymerization reaction is carried out at 30-50° C. for 10-15 hours. After standing, the solid and liquid are separated to obtain a carbon-containing silicon-based natural polymer material a having a water-retaining and salt-absorbing function;
[0009] (2) 20 parts by weight of calcium lignin sulfonate, 1-5 parts by weight of urea as a cross-linking agent, 5-10 parts by weight of ferrous sulfate cation exchanger, and 50-100 parts by weight of distilled water are placed in a reaction kettle, stirred, and fully reacted at 50-80° C. for 20-30 hours to fully exchange calcium lignin sulfonate with ferrous sulfate cations to form lignin iron salt, and at the same time, urea amino groups form hydrogen bonds with benzene hydroxyl groups on lignin, thereby prepolymerizing to obtain a macromolecular chain of lignin iron and calcium lignin sulfonate complex; then, 1- 10 parts by weight of polyacrylamide monomer, 1-5 parts by weight of ammonium persulfate as an initiator, 10-50 parts by weight of bentonite as a pore-forming agent, and 5-10 parts by weight of polyvinyl alcohol as a cross-linking agent are continuously stirred to completely dissolve, and allowed to stand for polymerization reaction at 30-80° C. for 10-24 hours, so that the hydroxyl groups on the lignin iron and calcium lignin sulfonate complexes form hydrogen bonds with the amino groups on the polyacrylamide monomer, and at the same time, macromolecular chains are formed under the action of the initiator and the cross-linking agent, thereby obtaining a viscous mixed solution b with a water-retaining function;
[0010] (3) Under room temperature conditions, 20 parts by mass of the carbon-silicon-based natural polymer material a prepared above and 20 parts by mass of the viscous mixed solution b are fully stirred and mixed, 1-2 parts by mass of manganese sulfate and 1-5 parts by mass of zinc sulfate are added in sequence, and stirred thoroughly. Distilled water is added to make the above liquid reach 1000 parts by mass, and the reaction is oscillated at room temperature for 15-48 hours, and the mixture is allowed to stand for 10-15 hours. The solid-liquid separation and natural drying are performed to obtain a carbon-silicon-based polymer soil conditioner having salt absorption and water retention functions and capable of enhancing crop stress resistance.
[0011] The application of the carbon silicon-based polymer soil conditioner obtained above needs to be applied according to the farmland and soil conditions and crop types. The prepared soil conditioner can be used under flushing / fertilization or drip irrigation conditions, and the specific use is as follows.
[0012] Saline-alkali land: The application amount is 10-100L / mu, flushing or dripping with water or determined according to crop type and irrigation frequency. The application amount for mild saline-alkali land is 10-40L / mu; the application amount for moderate saline-alkali land is 20-80L / mu; the application amount for severe saline-alkali land is 40-100L / mu.
[0013] Medium and low yield fields: The application amount is 10-100L / mu, flushing or dripping with water or determined according to crop type and irrigation frequency. When the yield is lower than 70% of the local crop yield, the application amount is 10-100L / mu; when the yield is lower than 50% of the local crop yield, the application amount is 40-100L / mu.
[0014] Desertified land: The application amount is 30-100L / mu, which can be applied by flushing or dripping with water or determined according to the crop type and irrigation frequency. When the soil layer of 0-60cm and below is all desertified, the application amount is 60-100L / mu, when the soil layer of 0-40cm is desertified, the application amount is 40-100L / mu, and when the soil layer of 0-20cm is desertified, the application amount is 30-100L / mu.
[0015] The straw waste includes crop straws such as cotton, corn, wheat, and rice.
[0016] The method for using the soil conditioner includes applying it into the soil with water before sowing, applying it successively with water and fertilizer during the crop growth period, and applying it once with water during the crop growth season.
[0017] When the soil conditioner is applied in the field, the application amount per mu is 10-100 L, and it is diluted 500-1000 times.
[0018] Beneficial effects of the present invention: The present invention utilizes cheap and readily available straw waste, adds methyl silicone oil, urea, ammonium persulfate, potassium thiosulfate and other reactants, breaks the dense structure of the straw under mild conditions, and obtains a carbon-containing silicon-based natural polymer material with water-retaining and salt-absorbing functions through prepolymerization reaction. The material has a loose and porous structure, which helps to improve the adsorption capacity of the material; then through a series of polymerization reactions of the carbon-containing silicon-based natural polymer material with calcium lignin sulfonate, polyacrylamide and the like, and at the same time adds beneficial metal elements Zn and Mn required for crop growth, the stress resistance of the crop is improved, and a soil conditioner with enhanced crop stress resistance is prepared. The soil conditioner has a simple synthesis process and low cost, and the main synthetic components can be used as nutrients required for crop growth. It can be used on a large scale to improve saline-alkali land, improve the soil's ability to retain water and fertilizer, enhance crop stress resistance, and thus increase crop yields. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is the salt-absorbing and water-retaining effect of soil conditioners.
[0020] Figure 2 It is the improvement effect of soil adjustment on saline-alkali sandy soil. DETAILED DESCRIPTION
[0021] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.
[0022] Example 1 Preparation and Performance Evaluation of Soil Conditioner
[0023] Weigh 50.0 g of crushed straw waste, 2.5 g of methyl silicone oil, and 3.0 g of urea respectively, add them to 50 mL of N,N-dimethylformamide solution, mix thoroughly, and let stand at room temperature for 5 h to allow the methyl silicone oil to fully penetrate into the hydroxyl surface of the straw powder cellulose, then add 2.5 g of potassium hydroxide to adjust the pH of the reaction solution, add 15.0 g of potassium thiosulfate and 4.0 g of ammonium persulfate, stir thoroughly, and react at 40 ° C for 10 h. After the reaction is completed, let stand for solid-liquid separation to obtain carbon-containing silicon-based natural polymer material a1. This step is repeated 3 times to obtain 3 identical portions of carbon-containing silicon-based natural polymer material a1.
[0024] Weigh 20.0g of calcium lignin sulfonate, 2.0g of urea, and 5.0g of ferrous sulfate in three portions, add them into a reactor containing 50mL of distilled water, stir them thoroughly, and react them at 50°C for 20h. Then add 1.0g, 2.0g, and 5.0g of polyacrylamide monomer, 1.0g of ammonium persulfate, 20.0g of bentonite, and 10.0g of polyvinyl alcohol in sequence, stir them continuously to completely dissolve them, and carry out polymerization reaction at 40°C for 15h to obtain viscous mixed solutions b1, b2, and b3 with water retention function.
[0025] At room temperature, stir and mix 3 parts of carbon-silicon-based natural polymer materials a1 with viscous mixed solutions b1, b2, and b3 respectively, add 1.0g of manganese sulfate and 2.0g of zinc sulfate in turn, stir thoroughly, add distilled water to make the above liquid reach 1000 parts by mass, oscillate and react at room temperature for 15 hours, let stand for 10 hours, separate the solid and liquid, and dry under natural conditions for 2 days to obtain carbon-silicon-based polymer soil conditioners A1, A2, and A3 that have the function of absorbing salt and retaining water and can enhance crop resistance. The salt and water absorption test was used to analyze the water and salt absorption capacity of the soil conditioner. As shown in the attached Figure 1 As shown, as the amount of polyacrylamide monomer increased from 1.0g to 5.0g, the water absorption and salt absorption of the prepared soil conditioner increased by 38.1% and 47.4%, respectively. This indicates that the increase in the amount of polyacrylamide monomer is helpful to improve the water absorption and salt absorption capacity of the soil conditioner.
[0026] Example 2 Preparation of carbon-containing silicon-based natural polymer material with good water absorption capacity
[0027] Weigh 50.0 g of crushed straw waste, 5.0 g of methyl silicone oil, and 4.0 g of urea respectively, add them to 50 mL of N,N-dimethylformamide solution, mix thoroughly, and let stand at room temperature for 5 h to allow the methyl silicone oil to fully penetrate into the hydroxyl surface of the straw powder cellulose, then add 2.5 g of potassium hydroxide to adjust the pH of the reaction solution, add 20.0 g of potassium thiosulfate and 4.0 g of ammonium persulfate, stir thoroughly, and react at 30°C, 40°C, and 50°C for 15 h, respectively. After the reaction is completed, let stand for solid-liquid separation to obtain carbon-containing silicon-based natural polymer materials prepared under different temperature conditions.
[0028] In order to compare the water absorption capacity of the materials, according to the above conditions, carbon-containing biomass materials were prepared without adding methyl silicone oil and urea. 50.0g of crushed straw waste was weighed and added to 50mL N,N dimethylformamide solution, mixed thoroughly, and then 2.5g of potassium hydroxide was added to adjust the pH of the reaction solution. 20.0g of potassium thiosulfate and 4.0g of ammonium persulfate were added and stirred thoroughly. The reaction was carried out at 30℃, 40℃, and 50℃ for 15h. After the reaction was completed, the solid-liquid separation was allowed to stand, and the carbon-containing biomass materials were prepared without adding methyl silicone oil and urea. The water absorption test was used to compare the water absorption properties of the materials prepared under different conditions. The results showed that under the three reaction temperature conditions of 30℃, 40℃ and 50℃, the water absorption of the carbon-containing silicon-based biomass materials prepared under the conditions of adding methyl silicone oil and urea increased by 6.1%-13.7% compared with the carbon-containing biomass materials prepared without adding methyl silicone oil and urea. At the same time, with the increase of reaction temperature, the water absorption of the prepared carbon-containing silicon-based biomass materials increased, which further indicates that the reaction temperature makes a positive contribution to the water absorption capacity of the material.
[0029] Example 3 Preparation of lignin-based polymer material with good salt absorption ability
[0030] Weigh 20.0g of calcium lignin sulfonate, 3.0g of urea, and 6.0g of ferrous sulfate in three portions, add them into a reactor containing 50mL of distilled water, stir them thoroughly, and react them at 50°C, 60°C, 70°C, and 80°C for 30h. Then, add 5.0g of polyacrylamide monomer, 2.0g of ammonium persulfate, 20.0g of bentonite, and 10.0g of polyvinyl alcohol in turn, stir them continuously to completely dissolve them, and carry out polymerization reaction at 40°C for 15h to obtain viscous mixed solutions with water retention function prepared under different temperature conditions.
[0031] In order to compare the effects of urea and ferrous sulfate, a control test was set up. 20.0g of calcium lignin sulfonate was weighed and added to a reactor containing 50mL of distilled water. After sufficient stirring, it was fully reacted at 50℃, 60℃, 70℃, and 80℃ for 30h. Then 5.0g of polyacrylamide monomer, 2.0g of ammonium persulfate, 20.0g of bentonite, and 10.0g of polyvinyl alcohol were added in sequence, and stirred continuously to completely dissolve. The polymerization reaction was carried out at 40℃ for 15h to obtain a viscous mixed solution prepared without adding urea and ferrous sulfate. The salt absorption test was conducted to compare the salt absorption performance of the materials prepared under different conditions. The results showed that under the three reaction temperature conditions of 50℃, 60℃, 70℃ and 80℃, the salt absorption of the viscous mixed solution prepared under the conditions of adding urea and ferrous sulfate increased by 4.8%-15.2% compared with the viscous mixed solution prepared without adding urea and ferrous sulfate. At the same time, with the increase of reaction temperature, the salt absorption of the prepared carbon-silicon-based biomass materials increased, which further indicates that with the increase of reaction temperature, more composite products will be produced.
[0032] Example 4 Evaluation of the improvement effect of soil conditioning on saline-alkali soil
[0033] This test was conducted on sandy land. Soil conditioners A1, A2, and A3 prepared in Example 1 were used and applied according to different soil types. After the materials were diluted with water, they were applied by dripping with water.
[0034] When the soil layer of 0-60cm and below is all sandy, the application rate is 60L / mu, when the soil layer of 0-40cm is sandy, the application rate is 40L / mu, and when the soil layer of 0-20cm is sandy, the application rate is 30L / mu. Collect soil surface samples regularly to test the salt content in the soil, and do a good job of control treatment. The results are shown in the attached Figure 2 As shown in the figure, with the increase of the dosage of polyacrylamide monomer in the soil conditioner, the salt content in the soil layers of different sandy soils gradually decreased, with the maximum reduction being 65.3% (0-60cm), 21.6% (0-40cm), and 38.5% (0-20cm), respectively. This also shows that the soil conditioner has a better salt control effect on deep salt.
Claims
1. A method for preparing a carbon-silicon-based polymer soil conditioner capable of enhancing crop stress resistance, characterized in that: Here are the steps: (1) 20-30 parts by weight of powdered straw, 1-5 parts by weight of methyl silicone oil as a branching monomer, 1-2 parts by weight of urea as an activator, and 10-20 parts by weight of N,N-dimethylformamide as a reaction solution are mixed thoroughly and allowed to stand at room temperature for 5-8 hours to allow the methyl silicone oil to fully penetrate into the cellulose hydroxyl surface of the straw powder and obtain a natural network branched macromolecular complex containing silicone oil through the hydrogen bond protection formed by the urea amino group and the branching monomer; then 1-2 parts by weight of potassium hydroxide are added in sequence to adjust the pH of the reaction solution, 5-10 parts by weight of potassium thiosulfate as a reducing agent, and 1-2 parts by weight of ammonium persulfate as an initiator and an oxidant, and the mixture is stirred thoroughly, and a grafting and polymerization reaction is carried out at 30-50° C. for 10-15 hours. After standing, the solid and liquid are separated to obtain a carbon-containing silicon-based natural polymer material a having a water-retaining and salt-absorbing function; (2) 20 parts by weight of calcium lignin sulfonate, 1-5 parts by weight of urea as a cross-linking agent, 5-10 parts by weight of ferrous sulfate cation exchanger, and 50-100 parts by weight of distilled water are placed in a reaction kettle, stirred, and fully reacted at 50-80° C. for 20-30 hours to fully exchange calcium lignin sulfonate with ferrous sulfate cations to form lignin iron salt, and at the same time, urea amino groups form hydrogen bonds with benzene hydroxyl groups on lignin, thereby prepolymerizing to obtain a macromolecular chain of lignin iron and calcium lignin sulfonate complex; then, 1- 10 parts by weight of polyacrylamide monomer, 1-5 parts by weight of ammonium persulfate as an initiator, 10-50 parts by weight of bentonite as a pore-forming agent, and 5-10 parts by weight of polyvinyl alcohol as a cross-linking agent are continuously stirred to completely dissolve, and allowed to stand for polymerization reaction at 30-80° C. for 10-24 hours, so that the hydroxyl groups on the lignin iron and calcium lignin sulfonate complexes form hydrogen bonds with the amino groups on the polyacrylamide monomer, and at the same time, macromolecular chains are formed under the action of the initiator and the cross-linking agent, thereby obtaining a viscous mixed solution b with a water-retaining function; (3) Under room temperature conditions, 20 parts by mass of the carbon-silicon-based natural polymer material a prepared above and 20 parts by mass of the viscous mixed solution b are fully stirred and mixed, 1-2 parts by mass of manganese sulfate and 1-5 parts by mass of zinc sulfate are added in sequence, and stirred thoroughly. Distilled water is added to make the above liquid reach 1000 parts by mass, and the reaction is oscillated at room temperature for 15-48 hours, and the mixture is allowed to stand for 10-15 hours. The solid-liquid separation and natural drying are performed to obtain a carbon-silicon-based polymer soil conditioner having salt absorption and water retention functions and capable of enhancing crop stress resistance.
2. The method for preparing a carbon silicon-based polymer soil conditioner according to claim 1, characterized in that: The straw waste includes cotton, corn, wheat and rice straw.
3. The use of the carbon silicon-based polymer soil conditioner obtained by the method for preparing the carbon silicon-based polymer soil conditioner according to claim 1 or 2, characterized in that: The application method of the carbon silicon-based polymer soil conditioner needs to be based on the farmland and soil conditions and crop types; the specific usage is as follows: Saline-alkali land: The application amount of carbon silicon-based polymer soil conditioner for slightly saline-alkali land is 10-40L / mu; the application amount of carbon silicon-based polymer soil conditioner for moderate saline-alkali land is 20-80L / mu; the application amount of carbon silicon-based polymer soil conditioner for severely saline-alkali land is 40-100L / mu; flushing or dripping with water once or determined according to crop type and irrigation frequency; Medium and low-yield fields: When the yield is lower than the local crop yield by more than 70%, the application amount of carbon silicon-based polymer soil conditioner is 10-100L / mu; when the yield is lower than the local crop yield by more than 50%, the application amount of carbon silicon-based polymer soil conditioner is 40-100L / mu; flushing or dripping with water or determined according to crop type and irrigation frequency; Desertified land: When the soil layer of 0-60cm and below is desertified, the application amount of carbon silicon-based polymer soil conditioner is 60-100L / mu; when the soil layer of 0-40cm is desertified, the application amount of carbon silicon-based polymer soil conditioner is 40-100L / mu, and when the soil layer of 0-20cm is desertified, the application amount of carbon silicon-based polymer soil conditioner is 30-100L / mu; flush application or drip application with water or determine according to crop type and irrigation frequency.
4. The use according to claim 3, characterized in that: The method of using the carbon silicon-based polymer soil conditioner includes applying it to the soil with water before sowing, applying it successively with water and fertilizer during the crop growth period, and applying it once with water during the crop growth season.
5. The use according to claim 3, characterized in that: When the soil conditioner is applied in the field, the application amount per mu is 10-100 L, and it is diluted 500-1000 times.
Citation Information
Patent Citations
Granular saline-alkali soil conditioner and production method thereof
CN103756685A
Straw biomass based water retaining agent and preparation method thereof
CN107513139A
Liquid saline alkali soil pH conditioner and preparation method of pH conditioner
CN107841314A
Straw-based water-absorbing and water-retaining agent and preparation method thereof
CN114106841A
Cited By
Water-retaining seedling-raising substrate compounding method capable of increasing emergence rate
CN121195807A
Soil conditioner derived from hydrothermal liquid as well as preparation method and application of soil conditioner
CN121343607A
Preparation and use method for carbon- and silicon-based polymer soil conditioner capable of enhancing crop stress resistance
WO2026045093A1