Super-tensile high-sensitivity anti-fatigue conductive hydrogel as well as preparation method and application thereof

By introducing functional materials such as MXene and Fe-MIL-88NH2 into the conductive hydrogel, a dual network structure is formed, which solves the problem of maintaining mechanical and sensor performance in simplified preparation and rapid glue formation, and realizes the Ultra-stretch, highly sensitive and fatigue-resistant conductive hydrogels suitable for wearable devices.

CN118994641AActive Publication Date: 2024-11-22SICHUAN UNIV

Patent Information

Application Number
CN202411079972.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

While simplifying the preparation steps and shortening the glue formation time, existing conductive hydrogels are difficult to maintain a variety of mechanical properties and sensing properties, and are highly dependent on external energy, limiting their application in flexible wearable devices.

Method used

The method of co-dispersing of MXene material, metal frame material, sodium oxidized alginate, hydrophilic monomer and metal ion salt is used to initiate the reaction through persulfate solution to form a conductive hydrogel with a dual network structure, and Fe-MIL- The catalytic formation of free radicals by 88NH2, achieving rapid gel formation.

Benefits of technology

Prepare ultra-stretched, highly sensitive, fatigue-resistant conductive hydrogels, with excellent mechanical properties and conductivity, can be prepared quickly and easily, suitable for wearable human physiological signal monitoring sensors, and do not require external energy input. Mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994641A_ABST
    Figure CN118994641A_ABST
Patent Text Reader

Abstract

The invention discloses super-tensile high-sensitivity anti-fatigue conductive hydrogel as well as a preparation method and application thereof, and belongs to the technical field of hydrogel. The preparation method comprises the following steps: (1) jointly dispersing an MXene material, a metal organic framework material, oxidized sodium alginate, a hydrophilic monomer and metal ion salt in water to obtain a precursor solution; and (2) adding a persulfate solution into the precursor solution, uniformly mixing, and reacting to obtain the catalyst. The preparation method disclosed by the invention is simple and rapid, low in cost and capable of realizing large-scale production, and the dual-network conductive hydrogel is endowed with various excellent properties including super-tensile property, strong adhesion, fatigue resistance and high conductivity through excellent structural design and introduction of functional materials. After being further assembled, the electrophysiological gel not only can be used for monitoring the movement of a human body, but also can be assembled into a conductive patch to monitor electrophysiological signals including electrocardio and myoelectricity in real time, and shows a better effect than commercial gel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogel preparation, and in particular to an ultra-stretched, highly sensitive, fatigue-resistant conductive hydrogel and a preparation method and application thereof. Background Art

[0002] In recent years, flexible wearable electronic devices have attracted widespread attention from researchers because they can continuously monitor and record human physiological signals, avoiding the traditional and cumbersome long-term health monitoring that requires large instruments. These wearable devices provide key data for some diseases that require long-term monitoring for diagnosis, and further facilitate the realization of personalized medicine. More and more research is focused on the development of wearable electronic devices based on flexible substrates, such as strain sensors, electronic skins, and soft robots. Such devices simulate the perception of human skin by converting external stimuli into electrical signals, or directly transduce a variety of weak electrical signals in the human body, ultimately achieving real-time monitoring of human physiological signals. The core of flexible wearable devices lies in the selection of conductive fillers and matrix materials and the design of their structures. A variety of flexible matrices combined with conductive fillers, such as conductive polymers, carbon nanotubes, graphene, etc., have been developed and introduced into the design and preparation of flexible wearable devices. However, due to the poor compatibility of conductive materials with some flexible substrates and poor skin adhesion, such wearable devices have problems such as low sensitivity, poor wearing experience, and incomplete monitoring signals. Therefore, it is necessary to select suitable flexible substrates and conductive materials to prepare high-performance wearable electronic devices.

[0003] Hydrogels are ideal materials for building flexible wearable electronic devices due to their unique three-dimensional (3D) network structure, good flexibility, stretchability and biocompatibility. In recent years, significant progress has been made in the preparation of conductive hydrogels, but their poor mechanical properties, low electrical conductivity and fatigue resistance, which are difficult to meet the needs of long-term monitoring, have seriously hindered their application in the construction of high-performance flexible electronic devices. In addition, traditional conductive hydrogels are difficult to simultaneously achieve high-sensitivity and low-noise monitoring of full-scale human activities and tiny electrophysiological signals, which also limits their application in the fields of human health monitoring and smart medical diagnosis.

[0004] The introduction of a variety of functional materials and network structures into hydrogels provides a potential solution to the existing difficulties in hydrogel design. However, these methods usually require complex procedures and long manufacturing times, and often rely on the input of external energy (such as light, heat or ultrasound). These not only put forward higher requirements on related equipment and facilities, but also increase the cost and safety issues in the production process. In addition, the complex manufacturing process and long time cycle also limit the large-scale production of these multifunctional hydrogels. Therefore, how to simplify the preparation process, reduce energy dependence and production costs has become an important topic in the study of multifunctional hydrogels. One of the current cutting-edge research directions in the field of conductive hydrogels is to simplify the preparation steps and minimize the dependence on external energy while giving hydrogel materials excellent mechanical properties, sensing properties and multifunctionality through reasonable structural design and the introduction of functional materials. This helps to overcome the application limitations of conductive hydrogels in flexible wearable devices and promote their application in a wider range of usage scenarios. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide an ultra-stretchable, highly sensitive, fatigue-resistant conductive hydrogel and its preparation method and application, so as to solve the problem that the existing conductive hydrogels are difficult to maintain the multiple mechanical properties and sensing properties of the hydrogel while simplifying the preparation steps and shortening the gelation time, and the multifunctionality of the conductive hydrogel.

[0006] The technical solution of the present invention to solve the above technical problems is as follows:

[0007] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0008] (1) dispersing MXene material, metal framework material, oxidized sodium alginate, hydrophilic monomer and metal ion salt in water to obtain a precursor solution;

[0009] (2) Add persulfate solution to the precursor solution, mix well, and react to obtain the product.

[0010] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel, the preparation method is simple, and the gelation rate is fast. The conductive hydrogel has the characteristics of ultra-stretchability, high sensitivity, and fatigue resistance, and can be used to assemble wearable human physiological signal monitoring sensors.

[0011] Furthermore, the MXene material in step (1) is a two-dimensional Ti 2 C 3 T x MXene nanosheets, with a mass of 0.1%-0.5% of the total mass of the precursor solution; the metal organic framework material is Fe-MIL-88NH2 , the mass is 0.002%-0.008% of the total mass of the precursor solution.

[0012] Preferably, the MXene material in step (1) is a two-dimensional Ti 2 C 3 T x MXene nanosheets, with a mass of 0.25% of the total mass of the precursor solution; the metal organic framework material is Fe-MIL-88NH 2 , the mass is 0.004% of the total mass of the precursor solution.

[0013] The beneficial effects of adopting the above further technical solution are as follows: the present invention introduces a new two-dimensional MXene material, which has excellent electrical conductivity and rich surface functional groups (-OH, -O, -F, etc.), and can be used as a high-performance conductive filler while also being able to react with Fe-MIL-88NH with peroxidase activity. 2 At room temperature, it catalyzes the rapid decomposition of persulfate to generate free radicals. Finally, it reacts with oxidized sodium alginate and Ca 2+ By forming a double network structure, a conductive hydrogel with ultra-stretchable, high sensitivity and anti-fatigue properties was obtained.

[0014] Furthermore, the hydrophilic monomer is acrylic acid, and its mass accounts for 10%-30% of the total mass of the precursor solution.

[0015] Preferably, the hydrophilic monomer is acrylic acid, and its mass accounts for 21% of the total mass of the precursor solution.

[0016] Furthermore, in step (1), the mass ratio of the hydrophilic monomer to the oxidized sodium alginate is 10:1-100:1; the mass ratio of the hydrophilic monomer to the metal ion salt is 2:1-10:1, and the metal ion salt includes at least one of calcium chloride, ferric chloride and zirconium chloride.

[0017] Preferably, in step (1), the mass ratio of the hydrophilic monomer to the oxidized sodium alginate is 30:1; the mass ratio of the hydrophilic monomer to the metal ion salt is 5:1, and the metal ion salt is calcium chloride.

[0018] The beneficial effects of the above further technical solution are as follows: the present invention prepares a double network conductive hydrogel structure by combining hydrophilic monomers, functional fillers and oxidized sodium alginate. The first layer of the double network hydrogel structure is composed of oxidized sodium alginate and metal ions, and the second layer of the network structure is composed of hydrophilic monomer polymers and MXene, Fe-MIL-88NH 2 The double network structure and the rich bonding interactions inside the hydrogel, including multiple hydrogen bonds, ionic bonds and coordination bonds, give the conductive hydrogel excellent mechanical properties, self-adhesion and conductivity.

[0019] Furthermore, in step (2), the concentration of the persulfate solution is 100-200 mg / mL, the volume ratio of the persulfate solution to the precursor solution is 1:5-1:20; and the persulfate is sodium persulfate.

[0020] Preferably, in step (2), the concentration of the persulfate solution is 120 mg / mL, the volume ratio of the persulfate solution to the precursor solution is 1:10; and the persulfate is sodium persulfate.

[0021] The beneficial effects of the above further technical solution are as follows: the present invention uses persulfate as an initiator to undergo a redox reaction with MXene, and utilizes Fe-MIL-88NH 2 Excellent catalytic properties generate a large number of free radicals, thereby achieving rapid polymerization of hydrophilic monomers to form the main structure of the hydrogel. 2 With a variety of surface functional groups (-OH, -O and -NH 2 etc.), can replace traditional cross-linking agents, form a cross-linked network with polymer segments, and then combine OSA and Ca 2+ Co-construction of double network high-toughness hydrogel: polyacrylic acid / MXene / oxidized sodium alginate / Fe-MIL-88NH 2 (PAA / MXene / OSA / Fe-MIL-88NH 2 , abbreviated as PM x OF y , where x and y are MXene and Fe-MIL-88NH 2 mass and mass percentage of acrylic acid monomer in the precursor solution).

[0022] Furthermore, in step (2), the reaction temperature is 20-30° C. and the reaction time is 10-900 s.

[0023] The beneficial effects of adopting the above further technical solution are: the present invention can quickly form gel at room temperature, the preparation method is simple and fast, the cost is low, and large-scale production can be achieved.

[0024] An ultra-stretchable, highly sensitive, fatigue-resistant conductive hydrogel is prepared by the preparation method.

[0025] The above-mentioned ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel is used in the preparation of sensors.

[0026] A sensor comprises the above-mentioned ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel.

[0027] The beneficial effects of the present invention are as follows: the sensor prepared using the hydrogel obtained by the present invention as the original element has excellent sensing performance. The experimental results of the present invention show that the hydrogel sensor has high sensitivity and good cycle stability.

[0028] The application of the above sensors in monitoring human joint activities and electrophysiological signals.

[0029] The beneficial effects of the present invention are as follows: the sensor prepared with the hydrogel obtained by the present invention as the original element can well monitor the strain signal generated during human body movement, and has good reliability for monitoring human body movement. At the same time, the assembled electrocardiogram test equipment and electromyography test system can well display electrocardiogram signals and electromyography signals. Compared with commercial gel electrodes, they have clearer signals, lower signal-to-noise ratio, and the ability to monitor human electrophysiological signals in real time.

[0030] The present invention has the following beneficial effects:

[0031] (1) The present invention combines the reduction properties of MXene itself and utilizes Fe-MIL-88NH 2 The characteristics of peroxidase are used to construct an efficient catalytic system to catalyze the decomposition of persulfate, generate free radicals, and form a hydrogel within tens of seconds without external energy input. At the same time, MXene also acts as a conductive filler and cross-linking agent in the hydrogel system and participates in the gelation process. Without the need to introduce traditional hydrogel cross-linking agents and external energy, high-performance conductive hydrogels are prepared within tens of seconds. The preparation method is simple, fast, low-cost, and can be mass-produced.

[0032] (2) The present invention endows the double network conductive hydrogel with a variety of excellent properties, including ultra-stretching performance, strong adhesion, fatigue resistance and high conductivity, through excellent structural design and the introduction of functional materials. After further assembly, it can not only be used to monitor human body movement, but also be assembled into a conductive patch to monitor electrophysiological signals including electrocardiogram and electromyography in real time, and show better signals than commercial gels.

[0033] (3) The present invention controls the Fe-MIL-88NH 2 The added amount can effectively control the various properties of the conductive hydrogel, including stretchability, adhesion, conductivity and stability, and thus has the potential to achieve personalized customization of flexible wearable devices based on conductive hydrogels. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The schematic diagram and optical photograph of the gelation reaction of the PMOF hydrogel in Experimental Example 1 and the scanning electron microscope image of the hydrogel, wherein a is a schematic diagram of the gelation of the hydrogel, b is an optical photograph of the gelation process of the hydrogel, and c is a scanning electron microscope image of different hydrogel samples;

[0035] Figure 2 In Experiment 2, different proportions of Fe-MIL-88NH 2 or MXene on the mechanical properties of PMOF hydrogels and the macroscopic mechanical properties of Example 1, where a is different proportions of Fe-MIL-88NH 2 Effect of the tensile properties of PMOF on the performance of the hydrogel. (b) Young's modulus and fracture stress of the hydrogel obtained from the tensile stress-strain diagram in (a). (c) Different proportions of Fe-MIL-88NH 2 Effect on the compression properties of PMOF, d is the compression modulus and maximum stress of the hydrogel obtained from the compression stress-strain diagram in Figure c, e is the effect of different proportions of MXene on the tensile properties of PMOF, f is the Young's modulus and fracture stress of the hydrogel obtained from the tensile stress-strain diagram in Figure e, g is the mechanical properties in the macroscopic state, including stretching, kinking, knotting, extension, high toughness (bearing 500g) and compression recovery;

[0036] Figure 3 Characterization of the adhesion of the PMOF hydrogel in Experimental Example 3, wherein a is an optical photograph of the adhesion of the PMOF hydrogel to various surfaces in a macroscopic state, b is the adhesion strength of the PMOF hydrogel to different substrates, and c is a schematic diagram of the adhesion principle of the PMOF hydrogel;

[0037] Figure 4 The conductivity diagram of the PMOF hydrogel in Experimental Example 4 and the sensing performance test of the sensor assembled by PMOF, where a is the conductivity of the hydrogel with different MXene contents, and b is the conductivity of the hydrogel with different Fe-MIL-88NH 2 The conductivity of the hydrogel with the content of 100%, c is the response time of the connection and disconnection of the hydrogel, d is the sensor sensitivity diagram of the sensor assembled by PMOF, e and f are the characterization diagrams of the strain frequency response characteristics and strain size response characteristics of the PMOF hydrogel-based sensor, g is the fatigue resistance of the sensor assembled by PMOF in 1500 cycles of stretching, and the small figure in g is an enlarged diagram of the local resistance change rate in ten seconds before and after 400s, 800s and 1200s;

[0038] Figure 5 Graph showing the relative resistance change of the PMOF hydrogel used for real-time monitoring of human joint activity in Experimental Example 5, wherein a is a schematic diagram of the monitoring process, b is a graph showing the relative resistance change signal generated by finger movement, c is a graph showing the relative resistance change signal generated by wrist joint movement, d is a graph showing the relative resistance change signal generated by elbow joint movement, e is a graph showing the relative resistance change generated by a facial smile, and f is a graph showing the resistance signal change when the throat detects the word "MXene";

[0039] Figure 6The signal diagram of the electrophysiological signal sensor assembled with the PMOF hydrogel electrode in Experimental Example 6 for monitoring human electrophysiological signals, wherein a is the electrocardiographic signal diagram recorded by the PMOF electrode and the commercial electrode, b is the muscle electrical signal diagram generated by the biceps brachii recorded by the PMOF electrode and the commercial electrode, c is the muscle electrical signal diagram generated by the brachioradialis under different forces recorded by the PMOF electrode, and d is the muscle electrical signal diagram generated by the brachioradialis under different gestures recorded by the PMOF electrode. DETAILED DESCRIPTION

[0040] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0041] Embodiment 1:

[0042] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0043] (1) 2D Ti 2 C 3 T x Synthesis of MXene nanosheets

[0044] Specific etching of MAX phase Ti using minimum layer strength peeling (MILD) 2 AlC 3 , synthesized Ti 2 C 3 T x MXene, the process is as follows: 1g LiF is dispersed in 20mL concentrated hydrochloric acid solution (9mol / L), reacted at 35℃ for 24h, and the generated HF is used to specifically etch away Ti 2 AlC 3 The Al atomic layer of MAX material is then further ultrasonicated and centrifuged to obtain Ti 2 C 3 T x MXene solution, and finally freeze-dried to obtain Ti with metallic luster in flake form 2 C 3 T x MXene, after sealing, was stored at 4 °C for future use.

[0045] (2) Metal-organic framework materials (MOFs) with octahedral structure Fe-MIL-88NH 2 Synthesis

[0046] Synthesis of Fe-MIL-88NH by solvothermal method2 The specific process is as follows: 0.2507g NH 2 -BDC (1.3838 mmol) and 0.3743 g FeCl 3 6H 2 O (1.3838 mmol) was dissolved in 30 mL DMF, stirred vigorously, and then reacted at 120° C. for 12 h. The product was washed and dried in vacuo at 40° C. and stored in a light-proof sealed container for later use.

[0047] (3) Synthesis of oxidized sodium alginate

[0048] The specific process is as follows: 1g of sodium alginate is prepared into a 1wt.% sodium alginate solution with deionized water, and 1.08g of NaIO 4 The mixture was stirred in the dark for 4 h. 1.5 mL of ethylene glycol was then added to quench the reaction, and the solution was collected and dialyzed in deionized water for three days (maximum molecular weight cutoff 3500). The dialyzed solution was collected and freeze-dried to obtain spongy oxidized sodium alginate.

[0049] (4) Weigh 3 g of acrylic acid, 3.0% sodium alginate oxide, 20% calcium chloride and 0.015% Fe-MIL-88NH 2 The above percentage contents are the mass percentages of the added substances in acrylic acid. After vortexing, stirring and ultrasound, they were evenly dispersed in 4 mL of deionized water; and mixed with 5 mL of 6.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0050] (5) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (4), mix quickly and evenly, then pour into a mold, and wait for several tens of seconds to gel to obtain an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel PM. 1 OF 0.015 .

[0051] Embodiment 2:

[0052] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0053] (1) 2D Ti 2 C 3 T x Synthesis of MXene nanosheets

[0054] Same as Example 1.

[0055] (2) Metal-organic framework materials (MOFs) with octahedral structure Fe-MIL-88NH 2 Synthesis

[0056] Same as Example 1.

[0057] (3) Synthesis of oxidized sodium alginate

[0058] Same as Example 1.

[0059] (4) Weigh 3 g of acrylic acid, 3.0% sodium alginate oxide, 20% calcium chloride and 0.010% Fe-MIL-88NH 2 The above percentage contents are the mass percentages of the added substances in acrylic acid. After vortexing, stirring and ultrasound, they were evenly dispersed in 4 mL of deionized water; and mixed with 5 mL of 6.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0060] (5) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (4), mix quickly and evenly, then pour into a mold and wait for several tens of seconds to gel to obtain a conductive hydrogel PM. 1 OF 0.01 .

[0061] Embodiment 3:

[0062] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0063] (1) 2D Ti 2 C 3 T x Synthesis of MXene nanosheets

[0064] Same as Example 1.

[0065] (2) Metal-organic framework materials (MOFs) with octahedral structure Fe-MIL-88NH 2 Synthesis

[0066] Same as Example 1.

[0067] (3) Synthesis of oxidized sodium alginate

[0068] Same as Example 1.

[0069] (4) Weigh 3 g of acrylic acid, 3.0% sodium alginate oxide, 20% calcium chloride and 0.0200% Fe-MIL-88NH 2The above percentage contents are the mass percentages of the added substances in acrylic acid. After vortexing, stirring and ultrasound, they were evenly dispersed in 4 mL of deionized water; and mixed with 5 mL of 6.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0070] (5) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (4), mix quickly and evenly, then pour into a mold and wait for several tens of seconds to gel to obtain a conductive hydrogel PM. 1 OF 0.02 .

[0071] Embodiment 4:

[0072] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0073] (1) 2D Ti 2 C 3 T x Synthesis of MXene nanosheets

[0074] Same as Example 1.

[0075] (2) Metal-organic framework materials (MOFs) with octahedral structure Fe-MIL-88NH 2 Synthesis

[0076] Same as Example 1.

[0077] (3) Synthesis of oxidized sodium alginate

[0078] Same as Example 1.

[0079] (4) Weigh 3 g of acrylic acid, 3.0% sodium alginate oxide, 20% calcium chloride and 0.030% Fe-MIL-88NH 2 The above percentage contents are the mass percentages of the added substances in acrylic acid. After vortexing, stirring and ultrasound, they were evenly dispersed in 4 mL of deionized water; and mixed with 5 mL of 6.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0080] (5) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (4), mix quickly and evenly, then pour into a mold and wait for several tens of seconds to gel to obtain a conductive hydrogel PM. 1 OF 0.03 .

[0081] Embodiment 5:

[0082] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0083] (1) 2D Ti 2 C 3 T x Synthesis of MXene nanosheets

[0084] Same as Example 1.

[0085] (2) Metal-organic framework materials (MOFs) with octahedral structure Fe-MIL-88NH 2 Synthesis

[0086] Same as Example 1.

[0087] (3) Synthesis of oxidized sodium alginate

[0088] Same as Example 1.

[0089] (4) Weigh 3 g of acrylic acid, 3.0% sodium alginate oxide, 20% calcium chloride and 0.015% Fe-MIL-88NH 2 The above percentage contents are the mass percentages of the added substances in acrylic acid. After vortexing, stirring and ultrasound, they were evenly dispersed in 4 mL of deionized water; and mixed with 5 mL of 3.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0090] (5) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (4), mix quickly and evenly, then pour into a mold and wait for several tens of seconds to gel to obtain a conductive hydrogel PM. 0.5 OF 0.015 .

[0091] Embodiment 6:

[0092] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0093] (1) 2D Ti 2 C 3 T x Synthesis of MXene nanosheets

[0094] Same as Example 1.

[0095] (2) Metal-organic framework materials (MOFs) with octahedral structure Fe-MIL-88NH2 Synthesis

[0096] Same as Example 1.

[0097] (3) Synthesis of oxidized sodium alginate

[0098] Same as Example 1.

[0099] (4) Weigh 3 g of acrylic acid, 3.0% sodium alginate oxide, 20% calcium chloride and 0.015% Fe-MIL-88NH 2 The above percentage contents are the mass percentages of the added substances in acrylic acid. After vortexing, stirring and ultrasound, they were evenly dispersed in 4 mL of deionized water; and mixed with 5 mL of 9.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0100] (5) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (4), mix quickly and evenly, then pour into a mold and wait for several tens of seconds to gel to obtain a conductive hydrogel PM. 1.5 OF 0.015 .

[0101] Embodiment 7:

[0102] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0103] (1) 2D Ti 2 C 3 T x Synthesis of MXene nanosheets

[0104] Same as Example 1.

[0105] (2) Metal-organic framework materials (MOFs) with octahedral structure Fe-MIL-88NH 2 Synthesis

[0106] Same as Example 1.

[0107] (3) Synthesis of oxidized sodium alginate

[0108] Same as Example 1.

[0109] (4) Weigh 3 g of acrylic acid, 3.0% sodium alginate oxide, 20% calcium chloride and 0.015% Fe-MIL-88NH 2The above percentage contents are the mass percentages of the added substances in acrylic acid. After vortexing, stirring and ultrasound, they were evenly dispersed in 4 mL of deionized water; and mixed with 5 mL of 12.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0110] (5) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (4), mix quickly and evenly, then pour into a mold and wait for several tens of seconds to gel to obtain a conductive hydrogel PM. 2 OF 0.015 .

[0111] Comparative Example 1:

[0112] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0113] (1) 2D Ti 2 C 3 T x Synthesis of MXene nanosheets

[0114] Same as Example 1.

[0115] (2) Synthesis of oxidized sodium alginate

[0116] Same as Example 1.

[0117] (3) Weigh 3 g of acrylic acid, 3.0% sodium alginate oxide, and 20% calcium chloride, respectively. The above percentages are the mass percentages of the added substances to the acrylic acid. Vortex, stir, and sonicate to uniformly disperse them in 4 mL of deionized water. Mix with 5 mL of 6.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0118] (4) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (3), mix quickly and evenly, then pour into a mold and wait for a few minutes to gel to obtain a conductive hydrogel PM. 1 OF 0.00 , abbreviated as PMO hydrogel.

[0119] Comparative Example 2:

[0120] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0121] (1) 2D Ti 2 C3 T x Synthesis of MXene nanosheets

[0122] Same as Example 1.

[0123] (2) Synthesis of oxidized sodium alginate

[0124] Same as Example 1.

[0125] (3) Weigh 3 g of acrylic acid, 1.0% sodium alginate, 20% calcium chloride, and 0.015% Fe-MIL-88NH 2 The above percentage contents are the mass percentages of the added substances in acrylic acid. After vortexing, stirring and ultrasound, they were evenly dispersed in 4 mL of deionized water; and mixed with 5 mL of 6.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0126] (4) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (3), mix quickly and evenly, pour into a mold, and wait for several tens of seconds to gel to obtain a conductive hydrogel.

[0127] Comparative Example 3:

[0128] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0129] (1) 2D Ti 2 C 3 T x Synthesis of MXene nanosheets

[0130] Same as Example 1.

[0131] (2) Synthesis of oxidized sodium alginate

[0132] Same as Example 1.

[0133] (3) Weigh 3 g of acrylic acid, 5.0% sodium alginate, 20% calcium chloride, and 0.015% Fe-MIL-88NH 2 The above percentage contents are the mass percentages of the added substances in acrylic acid. After vortexing, stirring and ultrasound, they were evenly dispersed in 4 mL of deionized water; and mixed with 5 mL of 6.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0134] (4) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (3), mix quickly and evenly, pour into a mold, and wait for several tens of seconds to gel to obtain a conductive hydrogel.

[0135] Comparative Example 4:

[0136] A method for preparing an ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel comprises the following steps:

[0137] (1) 2D Ti 2 C 3 T x Synthesis of MXene nanosheets

[0138] Same as Example 1.

[0139] (2) Synthesis of oxidized sodium alginate

[0140] Same as Example 1.

[0141] (3) Weigh 3 g of acrylic acid, 7.0% sodium alginate, 20% calcium chloride, and 0.015% Fe-MIL-88NH 2 The above percentage contents are the mass percentages of the added substances in acrylic acid. After vortexing, stirring and ultrasound, they were evenly dispersed in 4 mL of deionized water; and mixed with 5 mL of 6.0 mg / mL Ti 2 C 3 T x After the MXene dispersions are mixed, they are stirred and ultrasonically homogenized to obtain a hydrogel precursor solution.

[0142] (4) Add 1 mL of 120 mg / mL sodium persulfate solution to the hydrogel precursor solution obtained in step (3), mix quickly and evenly, pour into a mold, and wait for several tens of seconds to gel to obtain a conductive hydrogel.

[0143] Experimental Example 1: Hydrogel formation process and surface morphology

[0144] A schematic diagram of the gelation process of PMOF hydrogel was drawn, and optical photos of the gelation process were taken. Scanning electron microscopy (SEM) was used to characterize the different Fe-MIL-88NH 2 The addition amount (Examples 1-4 and Comparative Example 1) has an effect on PM 1 O y F. Effect of hydrogel micromorphology.

[0145] The experimental results are as follows Figure 1 shown.

[0146] like Figure 1 As shown in Figures a and b, PMOF hydrogel can form a complete hydrogel structure at room temperature in about 50 seconds. Figure 1 As shown in Figure c, without adding Fe-MIL-88NH 2 The hydrogel prepared in Comparative Example 1 exhibits a dense structure. 2 With the increase of the addition amount, the internal structure of PMOF hydrogel gradually changed from dense to loose, and the number and size of pores gradually increased. This is due to the initial Fe-MIL-88NH 2 The amount of MXene / Fe-MIL-88NH 2 The efficient catalytic system triggers the rapid decomposition of persulfate and produces oxygen, which in turn promotes the formation of pores inside the PMOF hydrogel.

[0147] Test Example 2: Mechanical Properties

[0148] Using a universal testing machine, characterize different Fe-MIL-88NH 2 The effects of different addition amounts of MXene (Examples 1-4 and Comparative Example 1) and different addition amounts of MXene (Example 1 and Examples 8-10) on the mechanical properties of PMOF hydrogels, including tensile properties and compressibility, were calculated, and the changes in Young's modulus and fracture stress were obtained. The macroscopic mechanical properties of PMOF hydrogels were photographed.

[0149] The experimental results are as follows Figure 2 shown.

[0150] like Figure 2 As shown in Figure a, as the hydrogel structure changes from the dense non-porous structure of Comparative Example 1 to the porous structure of Examples 1-4, the mechanical properties of the hydrogel change significantly. The increase in the number and diameter of pores will provide an energy dissipation structure in the hydrogel structure, further improving the tensile strength and elongation at break. However, as the structure becomes looser, the mechanical properties also decrease, and the fracture stress and strain show a trend of first increasing and then decreasing. The fracture strain and stress increase from PM to PM respectively. 1 OF 0.00 1215% and 76kPa increase to PM 1 OF 0.015 The hydrogel fracture strain of 2200% and stress of 110 kPa then dropped to PM 1 OF 0.03 1455% and 63.5kPa, the overall mechanical properties first increase and then decrease. 2 The addition of also changes the compression properties of PMOF hydrogels, such as Figure 2 As shown in Figure b, under a fixed compressive strain of 65%, different Fe-MIL-88NH 2The maximum stress of PMOF hydrogel with a content of 1.57kPa also showed a trend of gradual decrease, from 155kPa of PMO hydrogel to 2.5kPa of PM hydrogel. 1 OF 0.03 The hydrogel has a value of 13 kPa, indicating that Fe-MIL-88NH 2 The PMOF hydrogel gradually softens with increasing MXene content. The effect of MXene content on the mechanical properties of PMOF hydrogel was further investigated. Figure 2 As shown in Figures e and f, with the increase of MXene addition, the Young's modulus of PMOF hydrogel gradually increases with the increase of crosslinking degree, from 5.46 kPa to 12.22 kPa, while the fracture stress shows a trend of increasing and then decreasing. This is also related to the degree of crosslinking inside the hydrogel. The degree of crosslinking is proportional to the MXene content, and excessive crosslinking will reduce the toughness of the hydrogel and lead to premature fracture. According to the obtained mechanical properties data, PM 1 OF 0.015 Further macroscopic mechanical studies, such as Figure 2 As shown in Figure g, the results show that PM 1 OF 0.015 It has excellent mechanical properties, can maintain its shape under various external influences, lift a 500g weight without breaking, and can recover its original shape after being compressed by a weight of 500g, showing high tensile strength, high toughness and excellent recovery performance.

[0151] Test Example 3: Self-adhesion

[0152] The adhesion performance of the hydrogel was tested by sandwiching the PMOF hydrogel between a variety of materials and applying a tensile force. Specifically, the hydrogel and the test object were cut into rectangles with a length, width and thickness of 30 mm, 20 mm and 3 mm respectively. After applying a fixing force so that the material package clamped the PMOF hydrogel, it was installed on a universal testing machine, and a tensile force was applied to both sides. The adhesion force was recorded, and the adhesion strength was obtained by combining the contact area between the material and the substrate. The self-adhesion test was performed on the samples obtained in Examples 1-4 and Comparative Example 1.

[0153] The experimental results are as follows Figure 3 shown.

[0154] like Figure 3 In the middle a figure, PMOF hydrogel exhibits strong adhesion to a variety of surfaces, such as polypropylene, glass, polytetrafluoroethylene, metal, paper, and wood, showing multi-surface adhesion, and the adhesion strength is enough to lift a 200g weight. Although it shows high viscosity, there is no residue after it is removed from the skin, showing high practicality. 2As the amount of addition increases, the number and size of pores in the hydrogel structure increase, further increasing the contact area between the hydrogel and the substrate surface, and thus the adhesion strength of the PMOF hydrogel increases. Figure 3 In Figure b, although PMO hydrogels show certain adhesion to different substrates, the adhesion strength is low and they are prone to detachment. 2 With the increase of content, PMOF hydrogel showed enhanced adhesion, and the gradient increased with the increase of added amount. The maximum adhesion strength of PMOF hydrogel to wood, cardboard, metal and pig skin were 18.24kPa, 24.24kPa, 8.4kPa and 9.6kPa respectively, indicating that PMOF hydrogel has good adhesion and potential adhesive strength adjustability. Figure 3 Figure c shows the principle of adhesion of PMOF hydrogel. Various functional groups inside the hydrogel can interact with specific groups on the surface of the substrate to produce various bonding effects such as hydrogen bonds and coordination bonds, giving the material excellent adhesion. 2 The increase in the amount of addition increases the pore structure on the hydrogel surface, which increases the contact area with the substrate, leading to an increase in free functional groups such as carboxyl, aldehyde and hydroxyl groups involved in the adhesion interaction, and further leads to an increase in the adhesion strength.

[0155] Test Example 4: Electrochemical Performance and Sensing Performance

[0156] The conductivity of the PMOF hydrogel was tested using a digital bridge (LCR) and assembled into a strain sensor to test the corresponding resistance change under applied tension. The resistance change rate of the sensor when stretched (ΔR / R 0 ) and the strain change ε ​​to calculate the sensitivity, where R and R 0 The real-time resistance and initial resistance are respectively represented, and the linearity is obtained by linear fitting; the cycle stability test is performed by recording the relative resistance change rate of the strain sensor under continuous 1500 cycles of stretching to 60% strain, and the cycle and resistance change rate waveform is obtained. The hydrogels prepared in Examples 1-4 and Examples 8-10 are characterized.

[0157] The experimental results are as follows Figure 4 As shown. With the addition of MXene and Fe-MIL-88NH 2 As the amount of addition increases, the conductivity of the hydrogel will increase accordingly, such as Figure 4 In the middle figure (a), as the amount of MXene added increases, the conductivity of the hydrogel changes from PM 0.5 OF 0.015 3.24S / m increases to PM 2 OF 0.0153.79S / m, while Fe-MIL-88NH 2 As the amount of addition increased, the conductivity of the hydrogel increased from 2.8S / m of PMO to PM 1 OF 0.03 The electrical conductivity of PMOF hydrogel was 3.92S / m, which proved that PMOF hydrogel had excellent electrical conductivity. At the same time, the electrical self-healing property of PMOF hydrogel disconnection and connection was tested by electrochemical workstation (Gamry Reference 600). Figure 4 c, the PMOF hydrogel cut off in the circuit can restore the circuit after re-contacting in just 40ms, proving the excellent electrical self-healing property of the hydrogel. The present invention further verifies through experiments that the PM prepared by the above method 1 OF 0.015 The sensitivity of the flexible strain sensor (defined as the percentage of the ratio of the relative change rate of resistance to strain) can maintain good linearity over a large strain range of 0-1000%. Figure 4 In the middle d figure, the sensitivities of the three linear regions 0%-300%, 300%-700% and 700%-1000% are 3.03, 6.53 and 9.51 respectively. The strain frequency response and strain size responsiveness of PMOF hydrogel are further verified, such as Figure 4 e and f, the results show that PMOF hydrogel can respond to strains of different frequencies and sizes in a specific and repeatable manner, proving that the hydrogel has the ability to recognize various strains and can be further assembled into wearable sensors to recognize strain signals generated by various joint movements, facial expressions, and sounds of the human body. At the same time, the sensor has good stability, such as Figure 4 Figure g shows that after 1500 stretching cycles at 60% strain, the output signal remains stable. 1 OF 0.015 Hydrogel sensors have high sensitivity and good cyclic stability, and can be used well for long-term detection of various human behaviors.

[0158] Experimental Example 5: Application of hydrogel in strain sensor

[0159] The hydrogel PM prepared in Example 1 1 OF 0.015 The strain sensor was assembled with the LCR instrument and attached to the target areas of the body, including the fingers, wrists, and elbows, to record the relative rate of change of resistance of the strain sensor during joint movement, and further calculate the relative resistance change.

[0160] The experimental results are as follows Figure 5 shown.

[0161] PM 1 OF 0.015First, as a strain sensor for human motion detection, the measurement diagram is as follows Figure 5 As shown in Figure a, the resistance signals caused by the periodic bending and recovery movements of the joints such as fingers, wrists and elbows are monitored to obtain significant repeatable signals, and the signals obtained with different movement amplitudes are different. For example, the relative resistance change rate caused by the bending of the fingers is about 60%, while the relative resistance change caused by the bending of the elbow is about 175%. Figure 5 As shown in Figures b-d, the results show that the hydrogel prepared by the present invention has the ability to record and identify different joint movements for monitoring human body movements, and has good reliability. At the same time, the strain sensor can also be used to monitor small strain signals such as facial expressions and sounds, such as the resistance change caused by smiling expressions and saying the word "MXene", Figure 5 Chinese EF picture.

[0162] Test Example 6: Application of hydrogel in ECG test system

[0163] The hydrogel PM prepared by the embodiment 1 OF 0.015 It is assembled with an ECG test chip (BMD101, Wuxi Borunyin) to form an ECG test device. The signal is transmitted to the computer (PC) through a Bluetooth adapter to display the real-time heart rate of the person being tested. At the same time, it is assembled with a dual-channel electromyography test device (Wuxi Borunyin) to form a human electromyography test system to test the muscle electrical signals generated by the human body.

[0164] The experimental results are as follows Figure 6 shown.

[0165] The results show that the hydrogel PM prepared by the present invention 1 OF 0.015 The ECG signals measured by the electrodes are comparable to those of commercial gel electrodes (Hangzhou Xunda Radio Equipment Co., Ltd.), and the signals are clearer, with P, Q, R, S, and T peaks clearly visible (e.g. Figure 6 The assembled electromyography test system can display the electromyography signals of the test volunteers in real time, as shown in Figure a. Figure 6 Figure b, and PM 1 OF 0.015 The signal obtained by the test has a lower signal-to-noise ratio (PM) than the commercial gel electrode. 1 OF 0.015 gel: 11.40dB, commercial gel: 5.18dB). Figure 6 In Figures c-d, the electromyographic testing device can record and distinguish electromyographic signals generated by different force outputs and different gestures, proving that PMOF conductive hydrogel has the ability to assemble wearable devices to monitor human electrophysiological signals in real time.

[0166] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an ultra-stretchable, highly sensitive, anti-fatigue conductive hydrogel, characterized in that: The following steps are involved: (1) dispersing MXene material, metal organic framework material, oxidized sodium alginate, hydrophilic monomer and metal ion salt in water to obtain a precursor solution; (2) Add persulfate solution to the precursor solution, mix well, and react to obtain the product.

2. The method for preparing the ultra-stretchable, highly sensitive, anti-fatigue conductive hydrogel according to claim 1, characterized in that: The MXene material in step (1) is a two-dimensional Ti2C3T x The mass of MXene nanosheets is 0.1%-0.4% of the total mass of the precursor solution; the mass of the metal organic framework material is Fe-MIL-88NH2, and the mass of the precursor solution is 0.0025%-0.0075%.

3. The method for preparing the ultra-stretchable, highly sensitive, anti-fatigue conductive hydrogel according to claim 1, characterized in that: In the step (1), the hydrophilic monomer is acrylic acid, and its mass accounts for 20%-30% of the total mass of the precursor solution.

4. The method for preparing the ultra-stretchable, highly sensitive, anti-fatigue conductive hydrogel according to claim 1, characterized in that: In the step (1), the mass ratio of the hydrophilic monomer to the oxidized sodium alginate is 15:1-100:1; the mass ratio of the hydrophilic monomer to the metal ion salt is 4:1-10:1, and the metal ion salt includes at least one of calcium chloride, ferric chloride and zirconium chloride.

5. The method for preparing the ultra-stretchable, highly sensitive, anti-fatigue conductive hydrogel according to claim 1, characterized in that: In the step (2), the concentration of the persulfate solution is 100-200 mg / mL, the volume ratio of the persulfate solution to the precursor solution is 1:5-1:20; and the persulfate is sodium persulfate.

6. The method for preparing the ultra-stretchable, highly sensitive, anti-fatigue conductive hydrogel according to claim 1, characterized in that: In the step (2), the reaction temperature is 20-30° C. and the reaction time is 10-900 s.

7. An ultra-stretchable, highly sensitive, anti-fatigue conductive hydrogel, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the ultra-stretchable, highly sensitive, and fatigue-resistant conductive hydrogel according to claim 7 in preparing sensors.

9. A sensor, characterized in that: It includes the ultra-stretchable, highly sensitive, and anti-fatigue conductive hydrogel as described in claim 7.

10. Application of the sensor according to claim 9 in the recognition and monitoring of human joint movements, facial micro-expressions, sounds and electrophysiological signals.

Citation Information

Patent Citations

  • Preparation method of MXene enhanced dual-network self-healing conductive hydrogel

    CN112679755A

  • Preparation method of high-toughness, high-sensitivity and self-adhesion conductive hydrogel

    CN115141384A

  • Preparation method and application of double-network conductive ion hydrogel

    CN116444820A

  • Pure physical network hydrogel as well as preparation method and application thereof

    CN117924745A

  • Preparation method of spherical MOF material

    CN118206763A

Cited By

  • Preparation method of hydrogel film sensor for predicting muscle force and sensor

    CN119374766A

  • Preparation method of sodium alginate-based gradient hydrogel sensor

    CN119431693A