Expandable polystyrene with low solvent residue and preparation method thereof
By adjusting the ratio of functional additives and preparation technology, the problem of high solvent residues in existing radiable polystyrene products is solved, and low solvent residue products that meet food safety standards are realized, which are suitable for food packaging.
Patent Information
- Application Number
- CN202411479930.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing emitable polystyrene products cannot meet the food safety standards of "Quick Packaging Heavy Metals and Specific Substances Limited" GB43352-2023 and "National Food Safety Standard Plastic Materials and Products for Food Contact" GB4806.7-2023, and there are high solvents Residual problems.
By adjusting the ratio of functional additives to styrene, especially the use of sodium dodecylbenzenesulfonate and hydroxyethyl cellulose, the molecular weight and structure of polystyrene are ensured by combining the composite regulation of multiple initiators. , reduce solvent residue; preparation methods include mixing, emulsification, heating, pressure treatment and surface treatment to ensure low solvent residue of the product.
It achieves low-solvent residual inducible polystyrene that meets food safety standards, which is suitable for food packaging and reduces the limits of heavy metals and specific substances in food contact.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of foaming materials, and in particular to an expandable polystyrene with low solvent residue and a preparation method thereof. Background Art
[0002] Expandable polystyrene is a polystyrene product with a foaming agent added, abbreviated as "EPS". It appears as colorless and transparent beads.
[0003] Expandable polystyrene has been widely used in daily life, agriculture, transportation, military industry, aerospace industry, etc. due to its excellent and long-lasting thermal insulation, unique cushioning and shock resistance, anti-aging and waterproof properties, especially in the fields of construction, packaging, electronic and electrical products, ships, vehicles and aircraft manufacturing. For example, household appliances such as televisions, refrigerators, washing machines, air conditioners, refrigeration systems, civilian light industrial products such as electronic instruments, precision instruments, glassware, ceramic products, art crafts, fish fillets for marine aquaculture, seafood freezing, vegetable preservation, incubators, cold storage, refrigerated trucks, railways, municipal construction, etc., all of which are inseparable from EPS sheets and packaging products.
[0004] When expandable polystyrene products are used as food packaging materials, there are relatively high requirements for the food safety of expandable polystyrene products. However, the expandable polystyrene products currently on the market cannot meet the requirements of "Limits of Heavy Metals and Specific Substances in Express Packaging" GB43352-2023 and "National Food Safety Standard for Plastic Materials and Products for Food Contact" GB4806.7-2023. Summary of the invention
[0005] In order to reduce the solvent residue of expandable polystyrene and meet the standard requirements of GB43352-2023 and GB4806.7-2023, the present application provides an expandable polystyrene with low solvent residue and a preparation method thereof.
[0006] In a first aspect, the present application provides an expandable polystyrene with low solvent residue, which adopts the following technical solution.
[0007] The invention discloses an expandable polystyrene with low solvent residue. The raw materials of the polystyrene include styrene and the following raw materials in weight percentage: 0.1-0.3% of a nucleating agent, 0.65-1.5% of an initiator, 0.1-0.4% of a suspending agent, 0.001-0.003% of sodium dodecylbenzene sulfonate, 0.04-0.07% of sodium phosphate, 0.001-0.002% of hydroxyethyl cellulose, 5-8% of a foaming agent, 0.1-0.5% of a plasticizer, 0.001-0.002% of zinc stearate, 0.15-0.30% of glyceryl stearate, 0.01-0.02% of an antistatic agent and 90-140% of pure water.
[0008] By adopting the above technical scheme, the ratio of each functional additive to styrene is adjusted. Among them, sodium dodecylbenzene sulfonate changes the interfacial properties of the reaction system in the production of expandable polystyrene, affects the diffusion rate of styrene monomer molecules to the polymerization active center, thereby adjusting the rate of polymerization reaction, helping styrene monomer to form a stable emulsion in water, which is beneficial to the subsequent polymerization reaction. Hydroxyethyl cellulose can effectively disperse styrene monomer and other additives in the production process of expandable polystyrene, ensuring their uniform distribution in the reaction system. This uniform distribution helps to improve the efficiency of the polymerization reaction and the quality of the product, so that the final expandable polystyrene particles have a more regular shape, a looser structure and a more suitable apparent specific gravity. The initiator and other additives work together to regulate the molecular weight of polystyrene, thereby affecting its solubility in the solvent, ensuring that the residual monomers and other soluble substances in the product are at a low level.
[0009] Furthermore, based on the weight percentage of styrene and the total weight of the initiator, the initiator includes 3-6 parts of benzoyl peroxide, 1-2 parts of tert-butyl perbenzoate, 0-2 parts of tert-amyl peroxide-2-ethylhexyl carbonate, and 2.5-5 parts of diisopropylbenzene peroxide.
[0010] By adopting the above technical solution, the type and ratio of the initiator are set. Benzoyl peroxide is used as an initiator. When heated, it will decompose to produce benzoyl radicals. The benzoyl radicals produced in the chain initiation stage will add to the styrene monomer to form styrene radicals. This newly generated styrene radical is very active and will continue to react with the styrene monomer to generate a longer radical chain. This chain growth process will continue until the radical chain meets another radical chain and a termination reaction occurs. Tert-butyl peroxybenzoate will decompose to produce tert-butyl benzoate radicals. The tert-butyl benzoate radicals react with the styrene monomer to capture a hydrogen atom in the monomer molecule to generate styrene radicals and a tert-butyl benzoate molecule (or fragment). This styrene radical becomes a new active center and can continue to initiate polymerization. The styrene radicals react with more styrene monomers to generate longer radical chains. This chain growth process will continue until the radical chain meets another radical chain and a termination reaction occurs. When heated, tert-amyl-2-ethylhexyl carbonate decomposes to generate free radicals. The free radicals generated by the decomposition react with styrene monomers, taking a hydrogen atom from the monomer molecule to generate styrene free radicals. This styrene free radical becomes a new active center and can continue to undergo addition reactions with more styrene monomers. The generated styrene free radicals undergo continuous addition reactions with styrene monomers to form longer free radical chains. This chain growth process will continue until the free radical chain meets another free radical chain and terminates. Diisopropylbenzene peroxide decomposes under conditions such as heat or light to generate two free radicals (CH3C(O)·). The free radicals generated by the decomposition of diisopropylbenzene peroxide react with styrene monomers, taking a hydrogen atom from the monomer molecule to generate styrene free radicals. This styrene free radical becomes a new active center and can continue to undergo addition reactions with more styrene monomers. The generated styrene free radicals undergo continuous addition reactions with styrene monomers to form longer free radical chains. This chain growth process will continue until the free radical chain meets another free radical chain and terminates.
[0011] The present application uses a composite regulation through different initiator mechanisms to control the molecular weight of polystyrene, thereby affecting its solubility in the solvent, ensuring that the residual monomers and other soluble substances in the product are at a low level.
[0012] Furthermore, according to the weight percentage of styrene, based on the total weight of the initiator, the initiator includes 5 parts of benzoyl peroxide, 2 parts of tert-butyl perbenzoate, 1 part of tert-amyl peroxide-2-ethylhexyl carbonate, and 3 parts of diisopropylbenzene peroxide.
[0013] Furthermore, the suspending agent is calcium phosphate.
[0014] Furthermore, the plasticizer comprises xylene and white oil in a weight ratio of 1:(1-3).
[0015] Furthermore, the nucleating agent is low molecular weight PE wax.
[0016] In a second aspect, the present application provides a method for preparing expandable polystyrene with low solvent residue, using the following technical solution.
[0017] A method for preparing expandable polystyrene with low solvent residue, characterized in that it comprises the following steps: S1. According to the raw material ratio, styrene, a low nucleating agent, an initiator, and a plasticizer are mixed to obtain a mixture; S2. Add pure water to mixture 1 to obtain mixture 2; S3. Add part of the suspending agent, emulsifier, sodium phosphate, hydroxyethyl cellulose to the mixture and mix well to obtain a mixture of three; S4. The mixture was heated to 85-90°C and kept at this temperature for 3.5-4h, and the particles were allowed to sink; S5. Continue to maintain constant temperature for 5-6 hours, add suspending agent to the system to stabilize the suspension system; S6. A protective gas is introduced into the suspension system and a foaming agent is added; S7. The reaction system is heated to 115-130°C, the system pressure is 0.8-0.9MPa, and the temperature is kept for 2-4h; S8. Lowering the temperature of the reaction system to 30-40°C; S9. Dehydrating and drying the reaction product beads; S10. The dried beads are surface treated with zinc stearate, glyceryl stearate and an antistatic agent to obtain expandable polystyrene with low solvent residue.
[0018] Furthermore, the weight ratio of the suspending agent added to S3 and S5 is (0.85-3.00):1.
[0019] By adopting the above technical scheme and combining a specific production process with a raw material ratio, expandable polystyrene with low solvent residue can be obtained.
[0020] In summary, this application has the following beneficial effects: This application adjusts the ratio of functional additives to styrene in expandable polystyrene and produces it through a specific production process. The expandable polystyrene obtained can meet the standard requirements of "Limits of Heavy Metals and Specific Substances in Express Packaging" GB43352-2023 and "National Food Safety Standard Food Contact Plastic Materials and Products" GB4806.7-2023, and is suitable for food packaging. DETAILED DESCRIPTION
[0021] The present application is further described in detail below with reference to the embodiments.
[0022] raw material The raw materials in the examples of this application can be obtained from the market: Styrene, analytical grade; Nucleating agent, low molecular weight PE wax, Thailand SCG Chemical LP1020P; Foaming agent, pentane.
[0023] Example Examples 1-3 A low-solvent-residue expandable polystyrene, the preparation method of which is as follows: S1. According to the raw material ratio, styrene was added to the reactor, and then a low nucleating agent, an initiator, and a plasticizer were added, and stirred at room temperature for 30 minutes to obtain a mixture; S2. Pure water was added to the reactor to obtain a mixture of two; S3. Add 0.85 / (0.85+1) of suspending agent, emulsifier, sodium phosphate, hydroxyethyl cellulose to the reactor and stir for 30 minutes to obtain a mixture of three; S4. The suspension system in the reactor was heated to 90 ° C with steam and kept at a constant temperature for 3.5 h, and the particles sank; S5. Continue to maintain constant temperature for 5 hours and 20 minutes, add the remaining suspending agent to the system to stabilize the suspension system; S6. Seal the sampling port of the reactor, fill the reactor with nitrogen, check the sealing of the system, and start adding the foaming agent after there is no leakage; S7. The reaction system was heated to 120°C, the system pressure was 0.8MPa, and the temperature was kept for 3h; S8. The temperature of the reaction system is lowered to 35°C; S9. Dehydrating and drying the reaction product beads; S10. After drying, the expandable polystyrene beads were added to a ribbon mixer with 10 grams of zinc stearate, monoglyceride of stearate, sprayed with an antistatic agent, and coated for 10 minutes to obtain a low solvent residual expandable polystyrene raw material; S11. Expandable polystyrene raw materials are packed in multi-layer nylon composite polyethylene bags and stored in a cool and ventilated place.
[0024] Table 1 Raw material ratio table of Example 1-3 (g)
[0025] Among them, the nucleating agent is low molecular weight PE wax; the initiator is benzoyl peroxide, tert-butyl perbenzoate, tert-amyl peroxide-2-ethylhexyl carbonate, and diisopropylbenzene peroxide in a weight ratio of 5:2:1:3; the suspending agent is calcium phosphate; and the plasticizer is xylene and white oil in a weight ratio of 1:2.
[0026] Example 4 Different from Example 2, the initiator in Example 4 is benzoyl peroxide, tert-butyl perbenzoate, tert-amyl peroxide-2-ethylhexyl carbonate, and diisopropylbenzene peroxide in a weight ratio of 3:2:0.5:5.
[0027] Example 5 Different from Example 2, the initiator in Example 5 is benzoyl peroxide, tert-butyl perbenzoate, tert-amyl peroxide-2-ethylhexyl carbonate, and diisopropylbenzene peroxide in a weight ratio of 6:1:2:2.5.
[0028] Example 6 Different from Example 2, the initiator in Example 6 is benzoyl peroxide, tert-butyl perbenzoate, and diisopropylbenzene peroxide in a weight ratio of 4:2:3.5.
[0029] Example 7 Different from Example 2, the initiator in Example 7 is benzoyl peroxide.
[0030] Example 8 Different from Example 2, the initiator in Example 8 is tert-butyl perbenzoate.
[0031] Example 9 Different from Example 2, the initiator in Example 9 is tert-amyl peroxide-2-ethylhexyl carbonate.
[0032] Example 10 Different from Example 2, the initiator in Example 10 is dicumyl peroxide.
[0033] Comparative Example Comparative Example 1 Different from Example 1, the amount of initiator used in Comparative Example 1 is 250 g.
[0034] Comparative Example 2 Different from Example 1, the amount of initiator used in Comparative Example 2 is 850 g.
[0035] Comparative Example 3 Different from Example 1, Comparative Example 3 does not contain sodium dodecylbenzene sulfonate.
[0036] Comparative Example 4 Different from Example 1, Comparative Example 4 does not contain hydroxyethyl cellulose.
[0037] Performance Testing The solvent residues of the products in the embodiments and comparative examples were tested with reference to "Limits of Heavy Metals and Specific Substances in Express Packaging" GB43352-2023. The standard requirements are shown in Table 2, and the test results are shown in Table 3.
[0038] Refer to the "National Food Safety Standard for Plastic Materials and Products for Food Contact" GB4806.7-2023, the standard requirements are shown in Table 2 and the test results are shown in Table 3.
[0039] Table 2 Standard requirements
[0040] Note: 1. The total amount of residual solvent is the sum of methanol, ethanol, n-propanol, isopropanol, n-butanol, isoamyl alcohol, acetone, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, propylene glycol methyl ether, benzene, toluene, ethylbenzene and xylene; 2. The immersion solution obtained in the migration test was prepared by the full immersion method; 3. Not detected means less than the method detection limit. The method detection limit of aromatic primary amine migration is 0.001 mg / kg.
[0041] Table 3 Performance test results ;
[0042] Combining the embodiments with the comparative examples, it can be seen from Table 3 that the solvent residue of the expandable polystyrene obtained in the embodiments is lower than that in the comparative example, and the total migration amount and potassium permanganate consumption in the embodiments are also lower than those in the comparative example 1, which indicates that the solvent residue of the expandable polystyrene obtained in the present application is low and meets the food safety requirements and is suitable for food packaging.
[0043] Combining Example 2 with Examples 4-6 and Table 3, it can be seen that the type and ratio of the initiator will affect the solvent residue of the expandable polystyrene, and the ratio in Example 2 is more optimal. This may be because the molecular weight of the polystyrene is controlled by composite regulation through different initiator mechanisms, thereby affecting its solubility in the solvent, ensuring that the residual monomers and other soluble substances in the product are at a low level.
[0044] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A low-solvent-residue expandable polystyrene, the raw material of which includes styrene, characterized in that: According to the weight percentage of styrene, the following raw materials are also included in weight percentage: nucleating agent 0.1-0.3%, initiator 0.65-1.5%, suspending agent 0.1-0.4%, sodium dodecylbenzene sulfonate 0.001-0.003%, sodium phosphate 0.04-0.07%, hydroxyethyl cellulose 0.001-0.002%, foaming agent 5-8%, plasticizer 0.1-0.5%, zinc stearate 0.001-0.002%, glyceryl stearate 0.15-0.30%, antistatic agent 0.01-0.02%, and pure water 90-140%.
2. The low-solvent-residue expandable polystyrene according to claim 1, characterized in that: Based on the total weight of the initiator, the initiator includes 3-6 parts of benzoyl peroxide, 1-2 parts of tert-butyl perbenzoate, 0-2 parts of tert-amyl peroxide-2-ethylhexyl carbonate, and 2.5-5 parts of diisopropylbenzene peroxide.
3. The low-solvent-residue expandable polystyrene according to claim 2, characterized in that: Based on the total weight of the initiator, the initiator includes 5 parts of benzoyl peroxide, 2 parts of tert-butyl perbenzoate, 1 part of tert-amyl peroxide-2-ethylhexyl carbonate, and 3 parts of diisopropylbenzene peroxide.
4. The low-solvent-residue expandable polystyrene according to claim 1, characterized in that: The suspending agent is calcium phosphate.
5. The low-solvent-residue expandable polystyrene according to claim 1, characterized in that: The plasticizer includes xylene and white oil in a weight ratio of 1:(1-3).
6. The low-solvent-residue expandable polystyrene according to claim 1, characterized in that: The nucleating agent is low molecular weight PE wax.
7. A method for preparing expandable polystyrene with low solvent residue according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. According to the raw material ratio, styrene, a low nucleating agent, an initiator, and a plasticizer are mixed to obtain a mixture; S2. Add pure water to mixture 1 to obtain mixture 2; S3. Add part of the suspending agent, emulsifier, sodium phosphate, hydroxyethyl cellulose to the mixture II and mix well to obtain a mixture III; S4. The mixture was heated to 85-90°C and kept at this temperature for 3.5-4h, and the particles were allowed to sink; S5. Continue to maintain constant temperature for 5-6 hours, add suspending agent to the system to stabilize the suspension system; S6. A protective gas is introduced into the suspension system and a foaming agent is added; S7. The reaction system is heated to 115-130°C, the system pressure is 0.8-0.9MPa, and the temperature is kept for 2-4h; S8. Lowering the temperature of the reaction system to 30-40°C; S9. Dehydrating and drying the reaction product beads; S10. The dried beads are surface treated with zinc stearate, glyceryl stearate and an antistatic agent to obtain expandable polystyrene with low solvent residue.
8. The method for preparing expandable polystyrene with low solvent residue according to claim 7, characterized in that: The weight ratio of the suspending agent added to S3 and S5 is (0.85-3.00):1.
Citation Information
Patent Citations
Method for preparing spherical polystyrol of low volatile
CN101289521A
Low-VOC (volatile organic compound)-content flame-retardant expandable polystyrene resin and preparation method thereof
CN102863569A
Preparation method for synthesizing expandable polystyrene through efficient composite fire retardation agent
CN103848934A
The Suspension Polymerization Process of ExpandablePolystyrene Which Has the Good Effect for Environmentand Human Body