Green oil-resistant special flexible cable material and preparation method thereof
Through the combination of halogen-free flame retardant and composite filler, the problem of insufficient oil resistance and flame retardant performance of flexible cables in harsh environments is solved, and a green and environmentally friendly high-performance cable material is achieved, with excellent oil resistance and flexibility, and avoiding the need for The use of halogen elements.
Patent Information
- Application Number
- CN202411257181.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
AI Technical Summary
The existing flexible cables are insufficient in harsh environments, especially when used in oil and corrosive gases, and the oil resistance and flame retardant properties are often contained in traditional flame retardants, which have environmental problems.
Using a combination of halogen-free flame retardant and composite filler, stable mixing is prepared by ball milling of resorcinol bis(diphenylphosphate), polyphosphate and alumina, combined with carboxymethyl chitosan treatment. The flame retardant and flexibility of the cable material are enhanced by ball milling of modified graphene and diboron trioxide and glass powder.
It achieves excellent oil resistance and flexibility of cable materials, and the flame retardant does not contain halogen elements, which is green and environmentally friendly, improving the performance of cables under high temperature and mechanical loads.
Smart Images

Figure BDA0005034446170000101 
Figure BDA0005034446170000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cable materials and relates to a green, oil-resistant special flexible cable material and a preparation method thereof. Background Art
[0002] Flexible cables, also known as drag chain cables, towing cables, mobile cables, etc., are mainly the preferred cables for power transmission materials and signal transmission carriers in drag chain motion systems during specific applications. They are mainly suitable for installation under continuous reciprocating motion, especially in frequent bending occasions under industrial action environments, and need to cope with harsh environments such as heavy mechanical loads and high temperatures in the wild. The preparation of flexible cables is particularly important.
[0003] In some outdoor scenarios, it is also necessary to bury the wires directly in a special soil containing mineral oil without an outer tube. They can be widely used as connecting wires for power tools and various mobile electrical equipment in harsh environments with oil and corrosive gases, and work in an oil-immersed state for a long time. Summary of the invention
[0004] The purpose of the present invention is to provide a green and oil-resistant special flexible cable material and a preparation method thereof. The prepared cable material has excellent oil resistance and flexibility, and the flame retardant does not contain halogen elements and is green and environmentally friendly.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A green and oil-resistant special flexible cable material, comprising the following raw materials in parts by weight: 45-55 parts of nitrile rubber, 10-15 parts of polyphenylene ether, 12-18 parts of polyolefin elastomer, 25-35 parts of halogen-free flame retardant, 8-15 parts of composite filler, 4-7 parts of plasticizer, 3-5 parts of antioxidant, 1-2 parts of coupling agent, 3-5 parts of compatibilizer and 1.5-2.5 parts of lubricant;
[0007] The preparation process of the halogen-free flame retardant is as follows:
[0008] S11, grinding 40 to 50 parts by weight of resorcinol bis(diphenyl phosphate), 30 to 36 parts by weight of polyphosphate, 1 to 3 parts by weight of polyethylene glycol 200 and 3 to 5 parts by weight of alumina in a ball mill at a speed of 400 to 500 r / min for 4 hours to prepare a mixed powder;
[0009] S12, 10 to 20 parts by weight of the mixed powder and 70 to 90 parts by weight of deionized water are uniformly mixed, and then 7 to 13 parts by weight of carboxymethyl deacetylated chitosan are added, and the mixture is heated to 45 to 50° C., and mixed and stirred for 2 to 3 hours to obtain a mixed solution;
[0010] S13, heating the mixed solution to 95-105° C., stirring until the water in the solution evaporates to obtain a solid, washing with ethanol and deionized water, and vacuum drying to obtain the halogen-free flame retardant.
[0011] As a preferred technical solution of the present invention, the preparation process of the composite filler is as follows:
[0012] S21, under a nitrogen atmosphere, vacuum drying and dehydrating 20 to 30 parts by weight of castor oil, mixed with 20 to 25 parts by weight of isophorone diisocyanate, 0.5 to 0.7 parts by weight of stannous octoate as a catalyst and 30 to 40 parts by weight of tetrahydrofuran, stirring at 80 to 90° C. for 5 to 6.5 hours, then cooling to 40° C. and keeping warm for 1 hour to obtain a modified terminal isocyanate polyurethane prepolymer;
[0013] S22, adding graphene and modified terminal isocyanate polyurethane prepolymer in a mass ratio of (10-15): (1-3) in a high-speed disperser, dispersing for 2 hours at a rotation speed of 1000-1200 r / min, performing surface coating modification on the graphene, and obtaining modified graphene;
[0014] S23. Grind the modified graphene, boron trioxide and glass powder in a mass ratio of (3-5):1:1 in a ball mill at a speed of 400 r / min for 3 hours to obtain the composite filler.
[0015] As a preferred technical solution of the present invention, the lubricant is selected from one of stearic acid, polyethylene wax and zinc stearate.
[0016] As a preferred technical solution of the present invention, the plasticizer is one of diisobutyl phthalate, trioctyl trimellitate and dipentaerythritol ester.
[0017] As a preferred technical solution of the present invention, the antioxidant is one of antioxidant 1010, antioxidant 168 and antioxidant 1076.
[0018] As a preferred technical solution of the present invention, the coupling agent is one or more of KH550, KH560 and KH570.
[0019] As a preferred technical solution of the present invention, the compatibilizer is one of maleic anhydride grafted ethylene butene copolymer, ethylene-vinyl acetate maleic anhydride grafted copolymer and maleic anhydride grafted polypropylene.
[0020] A method for preparing a green, oil-resistant special flexible cable material comprises the following steps:
[0021] S81, mixing the nitrile rubber, polyphenylene ether and polyolefin elastomer at a high speed of 1600 to 2000 r / min for 15 to 20 minutes, adding a halogen-free flame retardant, a composite filler, a plasticizer, an antioxidant, a coupling agent, a compatibilizer and a lubricant, and continuing to mix at a high speed for 20 to 25 minutes to obtain a mixture A;
[0022] S82, melt blending the mixture A by an internal mixer, first mixing at 170-180° C. for 15-20 min, then heating to 220-240° C. for 15-20 min, with a rotation speed of 60-100 rpm, to obtain a mixture B;
[0023] S83. Vulcanize and mold the mixture B using a vulcanizer at a pressure of 13 to 16 MPa and a temperature of 160 to 180° C. for 5 to 8 minutes to obtain the green, oil-resistant special flexible cable material.
[0024] The present invention uses a halogen-free flame retardant, and resorcinol bis(diphenyl phosphate), polyphosphate and aluminum oxide are ground in a ball mill under the lubrication of polyethylene glycol 200 to fully mix the three, thereby maintaining uniformity at the microscopic level and obtaining a stable mixed powder, wherein the mixture of the phosphorus-based flame retardant and the aluminum oxide can improve the flame retardancy, can not only release flame retardants such as water and phosphoric acid, but also can help the cable form a dense carbonized layer on the surface; the ball-milled mixed powder is treated with carboxymethyl chitosan, which has excellent water solubility and biofilm-forming properties, and is evenly loaded on the surface of the mixed powder after solution immersion and evaporation. The carboxymethyl chitosan has good biocompatibility and degradability, can help improve the interface compatibility between the flame retardant and the polymer matrix, and the carboxymethyl chitosan can form a carbon layer at high temperature, which synergizes with other components in the flame retardant to help inhibit combustion.
[0025] When preparing the composite filler, castor oil is first dehydrated and then ether groups are introduced therein to obtain a terminal isocyanate polyurethane prepolymer having a long molecular chain and containing a polyether polyol. The modified terminal isocyanate polyurethane prepolymer is uniformly mixed with graphene, and the surface of the graphene is modified to weaken the interaction between graphene particles. At the same time, the graphene surface is coated by covalent bonds between active groups such as hydroxyl groups on the surface and intermolecular forces, thereby inhibiting the agglomeration of the filler. The composite filler is then fully ball-milled with boron trioxide and glass powder to obtain the composite filler.
[0026] The polymer matrix in the cable material component prepared by the present invention is a blend of nitrile rubber, polyphenylene ether and polyolefin elastomer. The nitrile rubber molecule contains a strongly polar cyano group, so it has high stability to non-polar or weakly polar oils and organic solvents, thereby showing excellent oil resistance. At the same time, in order to increase the flexibility of the polymer matrix, polyphenylene ether is added. The benzene ring in the molecular chain of polyphenylene ether contains an oxygen atom, which increases the curvature of the molecular chain, thereby increasing the flexibility of the polymer molecule. The electronegativity of the oxygen atom is higher than that of the carbon atom, and it is easier to generate a hydrogen bond structure with the surrounding molecules. This local interaction can enhance the flexibility of the polymer chain and reduce the mutual attraction between the chains. The polyolefin elastomer has a small density and is easy to process, which can help the cable material to have better flexibility while maintaining strength. Therefore, the polymer matrix prepared by blending the three can optimize the flexibility, mechanical strength and overall performance of the cable material.
[0027] During the smelting process, the modified flame retardants and fillers can improve their compatibility with the polymer matrix through the surface carboxymethyl deacetylated chitosan or terminal isocyanate polyurethane prepolymer, thereby improving the dispersibility and interfacial adhesion, thereby effectively playing the barrier role of the filling particles and improving the oil resistance and mechanical properties of the cable material.
[0028] Beneficial effects of the present invention:
[0029] The cable material obtained by mixing, melting and vulcanizing a polymer matrix of nitrile rubber, polyphenylene ether and polyolefin elastomer with a halogen-free flame retardant, a composite filler and other additives has excellent oil resistance and flexibility, and the flame retardant does not contain halogen elements and is green and environmentally friendly. DETAILED DESCRIPTION
[0030] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0031] In the present invention:
[0032] Polyphenylene ether: purchased from Shanghai Yuqing Plastic Products Co., Ltd., product number: 67665634;
[0033] Nitrile rubber: purchased from Wuhan Jiyesheng Chemical Co., Ltd.
[0034] Polyolefin elastomer: purchased from Suzhou Gangtai Plastic Chemical Co., Ltd., product number: DF940;
[0035] Carboxymethyl chitosan: purchased from Henan Weitixi Chemical Technology Co., Ltd., product number: A512850;
[0036] Resorcinol bis(diphenyl phosphate): purchased from Hunan Jiahang Pharmaceutical Technology Co., Ltd.;
[0037] Polyphosphate: purchased from Dongguan Guangsiyuan Polyurethane Materials Co., Ltd.;
[0038] Polyethylene glycol 200: purchased from Shanghai Fangye Chemical Co., Ltd.;
[0039] Alumina: purchased from Anhui Kerun Nanotechnology Co., Ltd.;
[0040] Castor oil: purchased from Shandong Fengpan New Materials Co., Ltd.;
[0041] Isophorone diisocyanate: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: I811865;
[0042] Stannous octoate: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: T818482;
[0043] Diisobutyl phthalate: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: D806857;
[0044] Antioxidant 1010, antioxidant 168, antioxidant 1076: purchased from Hubei Qifei Pharmaceutical Chemical Co., Ltd.;
[0045] KH550 and KH560 were purchased from Wuhan Rongcan Biotechnology Co., Ltd.;
[0046] Maleic anhydride grafted ethylene butene copolymer: purchased from Dongguan Yucheng Plastic Chemical Co., Ltd.
[0047] Stearic acid: purchased from Shanghai Fangye Chemical Co., Ltd.
[0048] Graphene: purchased from Hubei Qifei Pharmaceutical Chemical Co., Ltd., product number: QF210;
[0049] Boron trioxide: purchased from Hubei Hengjingrui Chemical Co., Ltd.
[0050] Glass powder: purchased from Wuhan Jiyesheng Chemical Co., Ltd.;
[0051] Trioctyl trimellitate: purchased from Wuhan Rongcan Biotechnology Co., Ltd.;
[0052] Ethylene-vinyl acetate maleic anhydride graft copolymer: purchased from Dongguan Bailing New Materials Co., Ltd.;
[0053] Polyethylene wax: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: U790488;
[0054] Dipentaerythritol ester: purchased from Wuhan Shuer Biotechnology Co., Ltd.
[0055] Example 1
[0056] Preparation of halogen-free flame retardant:
[0057] S11, grinding 40 parts by weight of resorcinol bis(diphenyl phosphate), 30 parts by weight of polyphosphate, 1 part by weight of polyethylene glycol 200 and 3 parts by weight of alumina in a ball mill at a speed of 400 r / min for 4 hours to prepare a mixed powder;
[0058] S12, 10 parts by weight of the mixed powder and 70 parts by weight of deionized water were mixed evenly, and then 7 parts by weight of carboxymethyl deacetylated chitosan were added, and the mixture was heated to 45° C. and stirred for 2 hours to obtain a mixed solution;
[0059] S13, heating the mixed solution to 95° C., stirring until the water in the solution evaporates to obtain a solid, washing it with ethanol and deionized water, and vacuum drying it to obtain a halogen-free flame retardant.
[0060] Preparation of composite fillers:
[0061] S21, under a nitrogen atmosphere, vacuum drying and dehydrating 20 parts by weight of castor oil, mixed with 20 parts by weight of isophorone diisocyanate, 0.5 parts by weight of stannous octoate as a catalyst and 30 parts by weight of tetrahydrofuran, stirred at 80° C. for 5 h, then cooled to 40° C. and kept warm for 1 h to obtain a modified terminal isocyanate polyurethane prepolymer;
[0062] S22, adding graphene and modified terminal isocyanate polyurethane prepolymer in a mass ratio of 10:1 in a high-speed disperser, dispersing for 2 hours at a rotation speed of 1000 r / min, performing surface coating modification on the graphene, and obtaining modified graphene;
[0063] S23. Grind the modified graphene, boron trioxide and glass powder in a mass ratio of 3:1:1 in a ball mill at a speed of 400 r / min for 3 hours to obtain a composite filler.
[0064] Preparation of green oil-resistant special flexible cable materials:
[0065] S81. After mixing 45 parts of nitrile rubber, 10 parts of polyphenylene ether and 12 parts of polyolefin elastomer at a speed of 1600 r / min for 15 min, 25 parts of halogen-free flame retardant, 8 parts of composite filler, 4 parts of diisobutyl phthalate, 3 parts of antioxidant 1010, 1 part of KH550, 3 parts of maleic anhydride grafted ethylene butene copolymer and 1.5 parts of stearic acid were added, and the mixture was mixed at a high speed for 20 min to obtain a mixture A.
[0066] S82, melt-blending the mixture A by an internal mixer, first mixing at 170° C. for 15 min, then heating to 220° C. for 15 min, with a rotation speed of 60 rpm, to obtain a mixture B;
[0067] S83. Vulcanize the mixture B in a vulcanizer at a pressure of 13 MPa and a temperature of 160° C. for 5 minutes to obtain a green, oil-resistant special flexible cable material.
[0068] Example 2
[0069] Preparation of halogen-free flame retardant:
[0070] S11, grinding 45 parts by weight of resorcinol bis(diphenyl phosphate), 33 parts by weight of polyphosphate, 2 parts by weight of polyethylene glycol 200 and 4 parts by weight of alumina in a ball mill at a speed of 450 r / min for 4 hours to prepare a mixed powder;
[0071] S12, 15 parts by weight of the mixed powder and 80 parts by weight of deionized water were mixed evenly, and then 11 parts by weight of carboxymethyl deacetylated chitosan were added, heated to 47° C., and mixed and stirred for 2.5 hours to obtain a mixed solution;
[0072] S13, heating the mixed solution to 100° C., stirring until the water in the solution evaporates to obtain a solid, washing it with ethanol and deionized water, and vacuum drying it to obtain a halogen-free flame retardant.
[0073] Preparation of composite fillers:
[0074] S21, under a nitrogen atmosphere, vacuum drying and dehydrating 25 parts of castor oil, mixed with 22 parts by weight of isophorone diisocyanate, 0.6 parts by weight of stannous octoate as a catalyst and 35 parts by weight of tetrahydrofuran, stirred at 85° C. for 6 h, then cooled to 40° C. and kept warm for 1 h to obtain a modified terminal isocyanate polyurethane prepolymer;
[0075] S22, adding graphene and modified terminal isocyanate-based polyurethane prepolymer in a mass ratio of 12:2 in a high-speed disperser, dispersing for 2 hours at a rotation speed of 1100 r / min, performing surface coating modification on the graphene, and obtaining modified graphene;
[0076] S23. Grind the modified graphene, boron trioxide and glass powder in a mass ratio of 4:1:1 in a ball mill at a speed of 400 r / min for 3 hours to obtain a composite filler.
[0077] Preparation of green oil-resistant special flexible cable materials:
[0078] S81. After mixing 50 parts of nitrile rubber, 12 parts of polyphenylene ether and 16 parts of polyolefin elastomer at a speed of 1700 r / min for 18 min, 30 parts of halogen-free flame retardant, 11 parts of composite filler, 6 parts of trioctyl trimellitate, 4 parts of antioxidant 168, 1.5 parts of KH560, 4 parts of ethylene-vinyl acetate maleic anhydride graft copolymer and 2 parts of polyethylene wax were added by weight, and the mixture was mixed at a high speed for 22 min to obtain a mixture A.
[0079] S82, melt blending the mixture A by an internal mixer, first mixing at 175° C. for 17 min, then heating to 230° C. for 17 min, with a rotation speed of 80 rpm, to obtain a mixture B;
[0080] S83. Vulcanize the mixture B in a vulcanizer at a pressure of 14 MPa and a temperature of 170° C. for 7 minutes to obtain a green, oil-resistant special flexible cable material.
[0081] Example 3
[0082] Preparation of halogen-free flame retardant:
[0083] S11, grinding 50 parts by weight of resorcinol bis(diphenyl phosphate), 36 parts by weight of polyphosphate, 3 parts by weight of polyethylene glycol 200 and 5 parts by weight of alumina in a ball mill at a speed of 500 r / min for 4 hours to prepare a mixed powder;
[0084] S12, 20 parts by weight of the inorganic mixed powder and 90 parts by weight of deionized water were mixed evenly, and 13 parts by weight of carboxymethyl deacetylated chitosan were added, and the mixture was heated to 50° C. and stirred for 3 hours to obtain a mixed solution;
[0085] S13, heating the mixed solution to 105° C., stirring until the water in the solution evaporates to obtain a solid, washing it with ethanol and deionized water, and vacuum drying it to obtain a halogen-free flame retardant.
[0086] Preparation of composite fillers:
[0087] S21, under a nitrogen atmosphere, vacuum drying and dehydrating 30 parts by weight of castor oil, mixed with 25 parts by weight of isophorone diisocyanate, 0.7 parts by weight of stannous octoate as a catalyst and 40 parts by weight of tetrahydrofuran, stirred at 90° C. for 6.5 h, then cooled to 40° C. and kept warm for 1 h to obtain a modified terminal isocyanate polyurethane prepolymer;
[0088] S22, adding graphene and modified terminal isocyanate polyurethane prepolymer in a mass ratio of 15:3 in a high-speed disperser, dispersing for 2 hours at a rotation speed of 1200 r / min, performing surface coating modification on the graphene, and obtaining modified graphene;
[0089] S23. Grind the modified graphene, boron trioxide and glass powder in a mass ratio of 5:1:1 in a ball mill at a speed of 400 r / min for 3 hours to obtain a composite filler.
[0090] Preparation of green oil-resistant special flexible cable materials:
[0091] S81. After mixing 55 parts of nitrile rubber, 15 parts of polyphenylene ether and 18 parts of polyolefin elastomer at a speed of 2000 r / min for 20 min, 35 parts of halogen-free flame retardant, 15 parts of composite filler, 7 parts of dipentaerythritol ester, 5 parts of antioxidant 1076, 2 parts of KH560, 5 parts of maleic anhydride grafted ethylene butene copolymer and 2.5 parts of stearic acid were added, and the mixture was mixed at a high speed for 25 min to obtain a mixture A.
[0092] S82, melt-blending the mixture A by using an internal mixer, first mixing at 180° C. for 20 min, then heating to 240° C. for 20 min, with a rotation speed of 100 rpm, to obtain a mixture B;
[0093] S83. The mixture B is vulcanized and molded by a vulcanizer at a pressure of 16 MPa and a temperature of 180° C. The vulcanization time is 8 minutes to obtain a green and oil-resistant special flexible cable material.
[0094] Comparative Example 1
[0095] The difference between Comparative Example 1 and Example 1 is that the halogen-free flame retardant in Comparative Example 1 is not treated with carboxymethyl deacetylated chitosan, and the other operations are the same.
[0096] Comparative Example 2
[0097] The difference between Comparative Example 2 and Example 1 is that the castor oil in Comparative Example 2 is not subjected to vacuum dehydration treatment, and the other operations are the same.
[0098] Comparative Example 3
[0099] The difference between Comparative Example 3 and Example 1 is that the graphene in Comparative Example 3 is not treated with a modified terminal isocyanate-based polyurethane prepolymer, and the other operations are the same.
[0100] Performance Test:
[0101] 1. Tensile strength and elongation at break: in accordance with GB / T 528-1998;
[0102] 2. Oxygen index: measured using an oxygen index meter according to standard LOI (ASTM D2863-97), with each sample size of 120*6.5*3.2mm;
[0103] 3. Oil resistance: Mineral oil resistance: Soak in test oil IRM902 at (100±2)℃ for 72h; Fuel oil resistance: Soak in test oil IRM903 at (100±2)℃ for 168h.
[0104] The test results are shown in the following table:
[0105]
[0106]
[0107] According to the above data, the data of the embodiments are better than those of the comparative examples, indicating that the modification method in the present invention is beneficial to improving the performance of the cable material, and has excellent oil resistance and flame retardancy. In addition, it can be seen from the tensile strength and elongation at break that the cable material of the present invention has good flexibility.
[0108] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A green and oil-resistant special flexible cable material, characterized in that: The invention comprises the following raw materials in parts by weight: 45 to 55 parts of nitrile rubber, 10 to 15 parts of polyphenylene ether, 12 to 18 parts of polyolefin elastomer, 25 to 35 parts of halogen-free flame retardant, 8 to 15 parts of composite filler, 4 to 7 parts of plasticizer, 3 to 5 parts of antioxidant, 1 to 2 parts of coupling agent, 3 to 5 parts of compatibilizer and 1.5 to 2.5 parts of lubricant; The preparation process of the halogen-free flame retardant is as follows: S11, grinding 40 to 50 parts by weight of resorcinol bis(diphenyl phosphate), 30 to 36 parts by weight of polyphosphate, 1 to 3 parts by weight of polyethylene glycol 200 and 3 to 5 parts by weight of alumina in a ball mill at a speed of 400 to 500 r / min for 4 hours to prepare a mixed powder; S12, 10 to 20 parts by weight of the mixed powder and 70 to 90 parts by weight of deionized water are uniformly mixed, and then 7 to 13 parts by weight of carboxymethyl deacetylated chitosan are added, and the mixture is heated to 45 to 50° C., and mixed and stirred for 2 to 3 hours to obtain a mixed solution; S13, heating the mixed solution to 95-105° C., stirring until the water in the solution evaporates to obtain a solid, washing with ethanol and deionized water, and vacuum drying to obtain the halogen-free flame retardant.
2. The green oil-resistant special flexible cable material according to claim 1, characterized in that: The preparation process of the composite filler is as follows: S21, under a nitrogen atmosphere, vacuum drying and dehydrating 20 to 30 parts by weight of castor oil, mixed with 20 to 25 parts by weight of isophorone diisocyanate, 0.5 to 0.7 parts by weight of stannous octoate as a catalyst and 30 to 40 parts by weight of tetrahydrofuran, stirring at 80 to 90° C. for 5 to 6.5 hours, then cooling to 40° C. and keeping warm for 1 hour to obtain a modified terminal isocyanate polyurethane prepolymer; S22, adding graphene and modified terminal isocyanate polyurethane prepolymer in a mass ratio of (10-15): (1-3) in a high-speed disperser, dispersing for 2 hours at a rotation speed of 1000-1200 r / min, performing surface coating modification on the graphene, and obtaining modified graphene; S23. Grind the modified graphene, boron trioxide and glass powder in a mass ratio of (3-5):1:1 in a ball mill at a speed of 400 r / min for 3 hours to obtain the composite filler.
3. The green oil-resistant special flexible cable material according to claim 1, characterized in that: The lubricant is selected from one of stearic acid, polyethylene wax and zinc stearate.
4. The green oil-resistant special flexible cable material according to claim 1, characterized in that: The plasticizer is one of diisopropyl phthalate, trioctyl trimellitate and dipentaerythritol ester.
5. The green oil-resistant special flexible cable material according to claim 1, characterized in that: The antioxidant is one of antioxidant 1010, antioxidant 168 and antioxidant 1076.
6. The green oil-resistant special flexible cable material according to claim 1, characterized in that: The coupling agent is one or more of KH550, KH560 and KH570.
7. The green oil-resistant special flexible cable material according to claim 1, characterized in that: The compatibilizer is one of maleic anhydride grafted ethylene butene copolymer, ethylene-vinyl acetate maleic anhydride grafted copolymer and maleic anhydride grafted polypropylene.
8. A method for preparing a green, oil-resistant special flexible cable material according to any one of claims 1 to 7, characterized in that: The following steps are involved: S81, mixing the nitrile rubber, polyphenylene ether and polyolefin elastomer at a high speed of 1600 to 2000 r / min for 15 to 20 minutes, adding a halogen-free flame retardant, a composite filler, a plasticizer, an antioxidant, a coupling agent, a compatibilizer and a lubricant, and continuing to mix at a high speed for 20 to 25 minutes to obtain a mixture A; S82, melt blending the mixture A by an internal mixer, first mixing at 170-180° C. for 15-20 min, then heating to 220-240° C. for 15-20 min, with a rotation speed of 60-100 rpm, to obtain a mixture B; S83. Vulcanize and mold the mixture B using a vulcanizer at a pressure of 13 to 16 MPa and a temperature of 160 to 180° C. for 5 to 8 minutes to obtain the green, oil-resistant special flexible cable material.