Resin composition
Patent Information
- Application Number
- CN202410587759.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-22
AI Technical Summary
根据本发明,能够提供可获得介电特性低、能抑制晕圈现象的固化物的树脂组合物,包含该树脂组合物的粘接膜,具备使用该树脂组合物形成的绝缘层的印刷布线板、及半导体装置。
Smart Images

Figure BDA0004836223760000081 
Figure BDA0004836223760000131 
Figure BDA0004836223760000431
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition and further to an adhesive film, a printed wiring board and a semiconductor device obtained by using the resin composition. Background Art
[0002] As a manufacturing technology for a printed wiring board, a manufacturing method using a build-up method in which insulating layers and conductive layers are alternately stacked is known.
[0003] As an insulating material for a printed wiring board used in such an insulating layer, for example, Patent Document 1 discloses a resin composition.
[0004] Prior art literature Patent Literature Patent document 1: International Publication No. 2022 / 038893. Summary of the invention
[0005] Technical problem to be solved by the invention In recent years, there has been an increasing demand for resin compositions that can form insulating layers having low relative permittivity and dielectric loss tangent. The relative permittivity and dielectric loss tangent are sometimes collectively referred to as dielectric properties.
[0006] If the dielectric properties of the insulating layer are to be reduced, materials that reduce the dielectric properties, such as active ester curing agents, may be considered. However, it is known that the cured product of the resin composition containing materials that reduce the dielectric properties will produce a halo phenomenon that reduces the conduction reliability. Here, the halo phenomenon refers to interlayer peeling between the insulating layer and the inner substrate around the through hole. Such a halo phenomenon is usually caused by the degradation of the resin around the through hole when the through hole is formed, and the degraded part is corroded during the roughening process. It should be noted that the degraded part is usually observed as a discolored portion.
[0007] The present invention is proposed in view of the above-mentioned problems, and the object of the present invention is to provide a resin composition that can obtain a cured product with low dielectric properties and capable of suppressing the halo phenomenon, an adhesive film containing the resin composition, a printed wiring board having an insulating layer formed using the resin composition, and a semiconductor device.
[0008] Means used to solve technical problems The present inventors have conducted intensive studies on the above-mentioned problems and have found that the above-mentioned problems can be solved by combining (A) an epoxy resin, (B) an active ester curing agent, (C) an inorganic filler, and (D) a silane compound having a silicon atom as a ring atom, thereby completing the present invention.
[0009] That is, the present invention includes the following contents. [1] A resin composition comprising: (A) Epoxy resin, (B) Active ester curing agent, (C) Inorganic filler materials, and (D) A silane compound having a silicon atom as a ring-constituting atom. [2] The resin composition according to [1], wherein the component (C) comprises any one of (C-1) a hollow inorganic filler and (C-2) a solid inorganic filler. [3] The resin composition according to [1] or [2], wherein the component (C) contains (C-1) a hollow inorganic filler. [4] The resin composition according to any one of [1] to [3], wherein the component (C) is surface-treated with the component (D). [5] The resin composition according to any one of [1] to [4], wherein the content of the component (C) is 50% by mass or more when the nonvolatile component in the resin composition is 100% by mass. [6] The resin composition according to any one of [1] to [5], wherein the content of the component (D) is 0.1% by mass or more and 5% by mass or less, based on 100% by mass of the resin component in the resin composition. [7] An adhesive film comprising: a support; and a resin composition layer comprising the resin composition according to any one of [1] to [6], provided on the support. [8] A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to any one of [1] to [6]. [9] A semiconductor device comprising the printed wiring board described in [8].
[0010] Effects of the Invention According to the present invention, a resin composition that can produce a cured product having low dielectric properties and suppressing the halo phenomenon, an adhesive film comprising the resin composition, a printed wiring board having an insulating layer formed using the resin composition, and a semiconductor device can be provided.
[0011] Brief description of the attached figure Figure 1 This is a cross-sectional view schematically showing an insulating layer obtained by curing the resin composition according to the first embodiment of the present invention into a sheet form together with an inner layer substrate. Figure 2 This is a plan view schematically showing the surface of the insulating layer opposite to the conductor layer, which is obtained by curing the resin composition according to the first embodiment of the present invention into a sheet shape. Figure 3This is a cross-sectional view schematically showing an insulating layer after roughening treatment, which is obtained by curing the resin composition according to the first embodiment of the present invention into a sheet form, together with an inner layer substrate. DETAILED DESCRIPTION
[0012] Hereinafter, the present invention will be described in detail with reference to its preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and any changes can be made within the scope of the claims and their equivalents.
[0013] [Resin composition] The resin composition of the present invention contains (A) epoxy resin, (B) active ester curing agent, (C) inorganic filler, and (D) silane compound having silicon atom as ring atom. In the present invention, by making it contain (A) component, (B) component, (C) component and (D) component in combination, a cured product with low dielectric properties and suppressed halo phenomenon can be obtained. In addition, a cured product with excellent elongation at break can also be obtained.
[0014] The resin composition may further include any component in combination with components (A) to (D). Examples of the arbitrary component include (E) a curing agent (excluding the curing agent belonging to component (B)), (F) a curing accelerator, (G) a thermoplastic resin, (H) other additives, and (I) a solvent. The components contained in the resin composition are described in detail below.
[0015] <(A) Epoxy resin> The resin composition contains an epoxy resin (A) as the component (A). By making the resin composition contain the epoxy resin (A), a cured product having good mechanical strength and insulation reliability can be obtained. The epoxy resins (A) may be used alone or in combination of two or more.
[0016] Examples of the epoxy resin (A) include bixylene type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butylcatechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidylester type epoxy resins, glycidylcyclohexane type epoxy resins. The epoxy resins include epoxy resins of alkyl diglycidyl ether type, cresol novolac type, biphenyl type, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexanedimethanol type epoxy resin, naphthyl ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, phenolphthalimidine type epoxy resin, etc. The epoxy resins may be used alone or in combination of two or more.
[0017] In the resin composition, it is preferred that the epoxy resin having two or more epoxy groups is included in one molecule as component (A). From the viewpoint of significantly obtaining the desired effect of the present invention, relative to 100 mass % of the epoxy resin (A), the ratio of the epoxy resin having two or more epoxy groups in one molecule is preferably 50 mass %, more preferably 60 mass %, and particularly preferably 70 mass % or more.
[0018] Epoxy resins include epoxy resins that are liquid at 20°C (hereinafter referred to as "liquid epoxy resins") and epoxy resins that are solid at 20°C (hereinafter referred to as "solid epoxy resins"). The resin composition may contain only a liquid epoxy resin as component (A), or only a solid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin. Among them, from the viewpoint of significantly obtaining the effects of the present invention, a combination of a liquid epoxy resin and a solid epoxy resin is preferred.
[0019] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0020] As the liquid epoxy resin, preferably bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexanedimethanol type epoxy resin, glycidyl amine type epoxy resin, and epoxy resin having a butadiene structure, glycidyl cyclohexane type epoxy resin, phenol benzopyrrolone type epoxy resin, alkyl diglycidyl ether type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, alkyl diglycidyl ether type epoxy resin is more preferable, and bisphenol A type epoxy resin is further preferable.
[0021] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene-type epoxy resins) manufactured by DIC Corporation, "828US", "jER828EL", "825", and "EPIKOTE 828EL" (bisphenol A-type epoxy resins) manufactured by Mitsubishi Chemical Corporation, "jER807" and "1750" (bisphenol F-type epoxy resins) manufactured by Mitsubishi Chemical Corporation, "jER152" (phenol novolac-type epoxy resin) manufactured by Mitsubishi Chemical Corporation, "630" and "630LSD" (glycidylamine-type epoxy resins) manufactured by Mitsubishi Chemical Corporation, "ZX1059" (a mixture of bisphenol A-type epoxy resin and bisphenol F-type epoxy resin) manufactured by Nippon Steel Chemical Materials Co., Ltd., and Nagase "EX-721" (glycidyl ester type epoxy resin) manufactured by ChemteX Corporation, "CELLOXIDE 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation, "PB-3600" (epoxy resin having a butadiene structure) manufactured by Daicel Corporation, "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel Chemical Materials Co., Ltd., "YED216D" (alkyl diglycidyl ether type epoxy resin) manufactured by Mitsubishi Chemical Corporation, etc. These resins may be used alone or in combination of two or more.
[0022] The solid epoxy resin is preferably a solid epoxy resin having two or more epoxy groups in one molecule, more preferably a solid epoxy resin having three or more epoxy groups in one molecule, and still more preferably an aromatic solid epoxy resin having three or more epoxy groups in one molecule.
[0023] As solid epoxy resins, preferred are biphenyl type epoxy resins, naphthalene type epoxy resins, naphthalene type tetrafunctional epoxy resins, cresol novolac type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol type epoxy resins, biphenyl type epoxy resins, naphthyl ether type epoxy resins, anthracene type epoxy resins, bisphenol A type epoxy resins, bisphenol AF type epoxy resins, and tetraphenylethane type epoxy resins, and better is biphenyl type epoxy resin.
[0024] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin), "HP-4700", "HP-4710" (naphthalene type tetrafunctional epoxy resin), "N-690" (cresol novolac type epoxy resin), "N-695" (cresol novolac type epoxy resin), "HP-7200", "HP-7200HH", "HP-7200H" (dicyclopentadiene type epoxy resin) manufactured by DIC Corporation. Resin), "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000", "HP6000L" (naphthyl ether type epoxy resin), "EPPN-502H" (trisphenol type epoxy resin), "NC7000L" (naphthol novolac type epoxy resin), "NC3000H", "NC3000" manufactured by Nippon Kayaku Co., Ltd. , "NC3000L", "NC3100" (biphenyl type epoxy resin), "ESN475V" (naphthalene type epoxy resin), "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel Chemical Materials Co., Ltd., "YX4000H", "YL6121" (biphenyl type epoxy resin), "YX4000HK" (biphenyl type epoxy resin), "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Corporation, "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd., "YL7760" (bisphenol AF type epoxy resin), "YL7800" (fluorene type epoxy resin), "jER1010" (solid bisphenol A type epoxy resin), "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Corporation, "WHR-991S" (phenol benzopyrrolidone type epoxy resin) manufactured by Nippon Kayaku Co., Ltd. These resins may be used alone or in combination of two or more.
[0025] When a liquid epoxy resin and a solid epoxy resin are used in combination as component (A), the mass ratio of the liquid epoxy resin to the solid epoxy resin is preferably 1:0.1 to 1:20, more preferably 1:0.15 to 1:10, and particularly preferably 1:0.2 to 1:5. By making the mass ratio of the liquid epoxy resin to the solid epoxy resin within the above range, the desired effect of the present invention can be significantly obtained.
[0026] The epoxy equivalent of component (A) is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., further preferably 80 g / eq. to 2000 g / eq., and further preferably 110 g / eq. to 1000 g / eq. By making it within this range, a cured product of the resin composition having a sufficient crosslinking density can be obtained. The epoxy equivalent is the mass of the epoxy resin containing 1 equivalent of epoxy groups. The epoxy equivalent can be measured in accordance with JIS K7236.
[0027] From the viewpoint of remarkably obtaining the desired effect of the present invention, the weight average molecular weight (Mw) of the component (A) is preferably from 100 to 5000, more preferably from 150 to 3000, further preferably from 200 to 1500. The weight average molecular weight of the epoxy resin is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).
[0028] From the viewpoint of obtaining the cured product showing good mechanical strength, insulation reliability, when the non-volatile component in the resin combination is made to 100 mass %, the content of (A) component is preferably more than 10 mass %, more preferably more than 20 mass %, further more preferably more than 30 mass %. The upper limit is preferably below 55 mass %, more preferably below 50 mass %, especially preferably below 45 mass %.
[0029] In the present invention, unless otherwise specified, the content of each component in the resin composition is a value when the nonvolatile component in the resin composition is 100% by mass, and the nonvolatile component refers to all nonvolatile components in the resin composition except the solvent.
[0030] From the viewpoint of obtaining a cured product showing good mechanical strength and insulation reliability, when the resin component in the resin composition is set to 100% by mass, the content of component (A) is preferably 30% by mass or more, more preferably 40% by mass or more, further preferably 50% by mass or more, preferably 70% by mass or less, more preferably 65% by mass or less, and further preferably 60% by mass or less.
[0031] In addition, in this invention, the resin component in a resin composition means the component other than (C) inorganic filler among the non-volatile components of a resin composition.
[0032] <(B) Active ester curing agent> The resin composition contains an active ester curing agent (B) as the component (B). The active ester curing agent (B) as the component (B) does not include substances belonging to the above-mentioned component (A). The active ester curing agent (B) can usually form a bond with the epoxy resin (A) and cure the resin composition. By combining the components (A) and (B) active ester curing agent in the resin composition, a cured product with low dielectric properties can be obtained. The components (B) can be used alone or in combination of two or more.
[0033] As (B) active ester curing agent, it is generally preferred to use a compound having ester groups with high reactive activity of more than 2 in 1 molecule, such as phenolic esters, thiophenolic esters, N-hydroxylamine esters, esters of heterocyclic hydroxy compounds, etc. The active ester curing agent is preferably a compound obtained by the condensation reaction of a carboxylic acid compound and / or a thiocarboxylic acid compound with a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, it is preferably an active ester curing agent obtained by a carboxylic acid compound and a hydroxy compound, and more preferably an active ester curing agent obtained by a carboxylic acid compound and a phenol compound and / or a naphthol compound. As a carboxylic acid compound, for example, benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, pyromellitic acid, etc. can be cited. Examples of the phenol compound or naphthol compound include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalein, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, pyrogallol, dicyclopentadiene-type diphenol compounds, and phenolic novolac. Here, the "dicyclopentadiene-type diphenol compound" refers to a diphenol compound obtained by condensing two molecules of phenol with one molecule of dicyclopentadiene.
[0034] Specifically, as component (B), there can be mentioned dicyclopentadiene type active ester curing agents, naphthalene type active ester curing agents containing naphthalene structure, active ester curing agents containing acetylated products of phenolic resin, active ester curing agents containing benzoylated products of phenolic resin, active ester curing agents as acetylated products of phenolic resin, active ester curing agents containing styryl and naphthalene structure, etc., preferably dicyclopentadiene type active ester curing agents. As dicyclopentadiene type active ester curing agents, active ester curing agents containing dicyclopentadiene type diphenol structure are preferred. "Dicyclopentadiene type diphenol structure" means a divalent structural unit formed by phenylene-dicyclopentylene-phenylene.
[0035] Commercially available products of component (B) include "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", "HPC-8000H-65TM", and "EXB-8000L-65TM" (manufactured by DIC Corporation) as active ester curing agents containing a dicyclopentadiene-type diphenol structure; and "HP-B-8151" as naphthalene-type active ester curing agents containing a naphthalene structure. -62T", "EXB9416-70BK", "EXB-8100L-65T", "EXB-8150L-65T", "EXB-8150-65T", "HPC-8150-60T", "HPC-8150-62T" (manufactured by DIC Corporation), "PC1300-02-65T" (manufactured by Airwater Corporation); Examples of phosphorus-containing active ester compounds include "EXB9401" ( DIC Corporation); as an active ester curing agent containing an acetylated product of a linear phenolic resin, "DC808" (Mitsubishi Chemical Corporation) can be cited; as an active ester curing agent containing a benzoylated product of a linear phenolic resin, "YLH1026" (Mitsubishi Chemical Corporation) can be cited; as an active ester curing agent containing an acetylated product of a linear phenolic resin, "DC808" (Mitsubishi Chemical Corporation) can be cited; as an active ester curing agent containing an acetylated product of a linear phenolic resin, "YLH1026" (Mitsubishi Chemical Corporation) can be cited; Examples of active ester curing agents of benzoylated products of lipids include "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), "YLH1048" (manufactured by Mitsubishi Chemical Corporation), and "EXB-8500-65T" (manufactured by DIC Corporation); examples of active ester curing agents containing styrene and naphthalene structures include "PC1300-02-65MA" (manufactured by Airwater Corporation) and the like.
[0036] From the viewpoint of obtaining a cured product having excellent peel strength while reducing dielectric loss tangent, the active ester group equivalent of component (B) is preferably 50 g / eq. to 500 g / eq., more preferably 50 g / eq. to 400 g / eq., and further preferably 100 g / eq. to 300 g / eq. The active ester group equivalent is the mass of the active ester curing agent containing 1 equivalent of active ester groups.
[0037] The amount ratio of (A) epoxy resin to (B) active ester curing agent is preferably 0.01 or more, more preferably 0.3 or more, further preferably 0.5 or more, preferably 5 or less, more preferably 4 or less, further preferably 3 or less, in terms of the ratio of [total number of active groups of active ester curing agent] / [total number of epoxy groups of epoxy resin]. Here, "the number of epoxy groups of epoxy resin" refers to the value obtained by summing up the values obtained by dividing the mass of non-volatile components of epoxy resin present in the resin composition by the epoxy equivalent. In addition, "the number of active groups of active ester curing agent" refers to the value obtained by summing up all the values obtained by dividing the mass of non-volatile components of active ester curing agent present in the resin composition by the active ester equivalent. By making the amount ratio of epoxy resin to active ester curing agent within the above range, the effect of the present invention can be significantly obtained.
[0038] From the viewpoint of obtaining the cured product of dielectric properties excellence, when the non-volatile component in the resin combination is made into 100 mass %, the content of (B) component is preferably more than 1 mass %, more preferably more than 3 mass %, further more preferably more than 5 mass %.In addition, the upper limit is preferably below 25 mass %, more preferably below 20 mass %, further more preferably below 15 mass %.
[0039] From the viewpoint of obtaining a cured product having excellent dielectric properties, when the resin component in the resin composition is set to 100% by mass, the content of component (B) is preferably 10% by mass or more, more preferably 15% by mass or more, further preferably 20% by mass or more, preferably 40% by mass or less, more preferably 35% by mass or less, further preferably 30% by mass or less.
[0040] <(C) Inorganic fillers> The resin composition contains an inorganic filler (C) as the component (C). By making the resin composition contain the inorganic filler (C), a cured product with low dielectric properties can be obtained. The inorganic filler (C) is usually contained in the resin composition in the form of particles. The component (C) can be used alone or in combination of two or more.
[0041] As the material of (C) inorganic filler, an inorganic compound is used. As the material of (C) inorganic filler, for example, silicon dioxide, aluminum oxide, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate, calcium zirconate, zirconium phosphate and zirconium tungstate phosphate, etc. can be cited. Among them, silicon dioxide is particularly preferred. As silicon dioxide, amorphous silicon dioxide, fused silica, crystalline silicon dioxide, synthetic silicon dioxide, hollow silica, etc. can be cited. In addition, as silicon dioxide, spherical silicon dioxide is preferred.
[0042] (C) Inorganic filler can be classified into (C-1) hollow inorganic filler having pores inside and (C-2) solid inorganic filler having no pores inside. (C) Inorganic filler preferably includes any one of (C-1) hollow inorganic filler and (C-2) solid inorganic filler, and from the viewpoint of obtaining a cured product with low dielectric properties, it is more preferable to include (C-1) hollow inorganic filler.
[0043] The (C-1) hollow inorganic filler may be a single hollow particle having only one hole inside the particle, may be a multi-hollow particle having two or more holes inside the particle, or may be a combination of a single hollow particle and a multi-hollow particle.
[0044] (C-1) hollow inorganic filling material has empty hole, so usually has the porosity greater than 0 volume %. (C-1) The porosity of hollow inorganic filling material is preferably more than 10 volume %, more preferably more than 15 volume %, especially preferably more than 20 volume %. In addition, from the viewpoint of the mechanical strength of the cured product of resin combination, the porosity of hollow inorganic filling material (C-1) is preferably below 80 volume %, more preferably below 75 volume %, especially preferably below 70 volume %.
[0045] The porosity P (volume %) of the inorganic filler is defined as the volume-based ratio of "the total volume of one or more pores existing inside the particle" to "the volume of the entire particle based on the outer surface of the particle" (total volume of pores / volume of the particle). For example, the measured value D of the actual density of the inorganic filler is used. M (g / cm 3 ), and the theoretical value D of the material density of the material forming the inorganic filler T (g / cm 3 ), calculated by the following formula (1): [Mathematical formula 1]
[0046] (C-1) hollow inorganic filling material generally has a hole formed in the particle and an outer shell formed by an inorganic material surrounding the hole. Usually, the hole is partitioned with the particle outside by the outer shell. At this time, the hole is preferably not connected to the particle outside. Thus, the outer shell is preferably a non-porous shell without a hole connecting the hole and the particle outside. The shell without pores can be confirmed by using a transmission electron microscope (TEM) to observe.
[0047] From the viewpoint of significantly obtaining the effects of the present invention, the average particle size of the hollow inorganic filler (C-1) is preferably at least 0.01 μm, more preferably at least 0.1 μm, particularly preferably at least 0.3 μm, preferably at most 5 μm, more preferably at most 4 μm, particularly preferably at most 3 μm.
[0048] The average particle size of the particles can be measured by the laser diffraction scattering method based on Mie scattering theory. Specifically, the particle size distribution of the particles can be made on a volume basis by a laser diffraction scattering particle size distribution measuring device, and the median particle size can be measured as the average particle size. The sample of the inorganic filler can be a sample obtained by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the sample for 10 minutes by ultrasonic wave. For the sample, a laser diffraction particle size distribution measuring device can be used, and the light source wavelength is blue and red, and the particle size distribution of the volume basis of the inorganic filler is measured in a flow cell mode, and the average particle size is calculated as the median particle size according to the obtained particle size distribution. As a laser diffraction particle size distribution measuring device, for example, "LA-960" made by Horiba, Ltd. can be cited.
[0049] From the viewpoint of significantly obtaining the effects of the present invention, the BET specific surface area of the hollow inorganic filler (C-1) is preferably 1 m 2 / g or more, preferably 2m 2 / g or more, particularly preferably 5m 2 / g or more, preferably 100m 2 / g or less, preferably 50m 2 / g or less, particularly preferably 30m 2 The BET specific surface area of the particles can be measured by adsorbing nitrogen gas on the surface of a sample using a specific surface area measuring apparatus (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method and calculating the specific surface area by a BET multipoint method.
[0050] (C-1) A commercially available hollow inorganic filler can be used. Examples of commercially available hollow inorganic fillers (C-1) include "MG-005" manufactured by Pacific Cement Co., Ltd. and "LHP-208" manufactured by Ube Exsymo Co., Ltd.
[0051] In addition, the hollow inorganic filling material (C-1) can be manufactured, for example, by the method described in Japanese Patent Gazette No. 5940188 or a method based thereon. If a specific example is given, the hollow silica particles as an example of the hollow inorganic filling material (C-1) can be manufactured by a method comprising the following steps: a step of preparing an aqueous solution containing a substance that can form pores and an alkaline compound; a step of mixing and stirring the aqueous solution with an alkoxysilane to precipitate silica particles; a step of removing the substance that can form pores from the silica particles to obtain a hollow silica precursor; and a step of calcining the hollow silica precursor.
[0052] In addition, the hollow inorganic filling material (C-1) can be manufactured, for example, by the method described in Japanese Patent Gazette No. 5864299 or a method based thereon. If a specific example is given, the hollow silica particles as an example of the hollow inorganic filling material (C-1) can be manufactured by a method comprising the following steps: (a) step of preparing an aqueous solution containing a substance that can form a hollow portion and an alkaline compound; (b) step of adding alkoxysilane to the aqueous solution and stirring at 0°C to 100°C to precipitate silica particles; (c) step of removing the substance that can form a hollow portion from the silica particles obtained by the (b) step to obtain a hollow silica precursor; and (c) step of calcining the hollow silica precursor obtained by the (c) step at a temperature exceeding 900°C to obtain a hollow silica.
[0053] From the viewpoint of improving moisture resistance and dispersibility, the hollow inorganic filler (C-1) can be treated by a surface treatment agent other than the component (D) described later. As a surface treatment agent other than the component (D), for example, a fluorine-containing silane coupling agent, an aminosilane coupling agent, an epoxysilane coupling agent, a mercaptosilane coupling agent, a silane coupling agent, an alkoxysilane, an organic silazane compound, a titanate coupling agent, etc. can be cited. The surface treatment agent can be used alone or in any combination of two or more.
[0054] Commercially available products of the surface treatment agent include, for example, “KBM403” (3-glycidoxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM803” (3-mercaptopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBE903” (3-aminopropyltriethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM573” (N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “SZ-31” (hexamethyldisilazane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM103” (phenyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM-4803” (long-chain epoxy-type silane coupling agent) manufactured by Shin-Etsu Chemical Co., Ltd., and “KBM-7103” (3,3,3-trifluoropropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd.
[0055] From the viewpoint of improving dispersibility, the degree of surface treatment performed by the surface treatment agent other than the component (D) is preferably within a specific range. Specifically, 100% by mass of the inorganic filler is preferably surface treated by the surface treatment agent other than the component (D) of 0.2% by mass to 8% by mass, more preferably surface treated by the surface treatment agent other than the component (D) of 0.2% by mass to 5% by mass, and further preferably surface treated by the surface treatment agent other than the component (D) of 0.3% by mass to 3% by mass.
[0056] The degree of surface treatment by a surface treatment agent other than component (D) can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is preferably 0.02 mg / m 2 More than 0.1 mg / m 2 More preferably, 0.2 mg / m 2 On the other hand, from the viewpoint of preventing the increase of the melt viscosity of the resin composition, 1.0 mg / m 2 Below, preferably 0.8mg / m 2 Below, more preferably 0.5 mg / m 2 the following.
[0057] The amount of carbon per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is cleaned with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK is added as a solvent to the inorganic filler surface-treated by a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid component, a carbon analyzer can be used to measure the amount of carbon per unit surface area of the inorganic filler. As a carbon analyzer, "EMIA-320V" manufactured by Horiba, Ltd. can be used.
[0058] From the viewpoint of significantly obtaining the effect of the present invention, when the non-volatile component in the resin composition is set to 100 mass %, the content (mass %) of the hollow inorganic filler (C-1) is preferably 0 mass % or more, more preferably 15 mass % or more, further preferably 20 mass % or more, preferably 70 mass % or less, more preferably 65 mass % or less, and further preferably 60 mass % or less.
[0059] From the viewpoint of significantly obtaining the effects of the present invention, when the non-volatile component in the resin composition is set to 100 volume %, the content (volume %) of the hollow inorganic filler (C-1) is preferably 1 volume % or more, more preferably 3 volume % or more, further preferably 5 volume % or more, preferably 70 volume % or less, more preferably 60 volume % or less, and further preferably 50 volume % or less.
[0060] From the viewpoint of remarkably obtaining the effects of the present invention, the specific gravity of the component (C-1) is preferably 3.50 g / cm 3 Below, preferably 3.00g / cm 3 Below, further preferably 2.50g / cm 3 Below, preferably 0.05g / cm 3 More than 0.5 g / cm 3 More preferably, 1.0 g / cm 3 The specific gravity can be measured by the method described in the examples described later.
[0061] (C-2) solid inorganic filler is an inorganic filler having a porosity of 0% by volume. (C-2) solid inorganic filler can use commercial products. Commercial products of (C-2) solid inorganic filler include, for example, "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical Materials Co., Ltd., "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", "SO-C1" manufactured by Yaduma Co., Ltd., "UFP-30", "DAW-03", "FB-105FD" manufactured by DENKA Co., Ltd., "SILFIL NSS-3N", "SILFIL NSS-4N", "SILFIL NSS-5N" manufactured by Tokuyama Co., Ltd., "CellSpheres", "MGH-005" manufactured by Pacific Cement Co., Ltd., etc.
[0062] The average particle size of the solid inorganic filler (C-2) is preferably 0.01 μm or more, more preferably 0.1 μm or more, further preferably 0.3 μm or more, preferably 10 μm or less, more preferably 5 μm or less, further preferably 3 μm or less. The average particle size of the component (C-2) can be measured by the same method as the average particle size of the hollow inorganic filler (C-1).
[0063] (C-2) The BET specific surface area of the solid inorganic filler is preferably 0.1 m 2 / g or more, preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, preferably 100m 2 / g or less, preferably 70m 2 / g or less, more preferably 40m 2 The BET specific surface area of the component (C-2) can be measured by the same method as the BET specific surface area of the component (C-1).
[0064] (C-2) The solid inorganic filler can be treated with a surface treatment agent other than the component (D) in the same manner as the hollow inorganic filler (C-1). The surface treatment agent other than the component (D), the degree of the surface treatment, the carbon content, etc. are as described above.
[0065] When the non-volatile component in the resin composition is set to 100 mass %, the content (mass %) of the (C-2) solid inorganic filler can be 0 mass % or greater than 0 mass %, preferably 10 mass % or more, more preferably 20 mass % or more, especially preferably 30 mass % or more, preferably 85 mass % or less, more preferably 80 mass % or less, especially preferably 75 mass % or less.
[0066] When the non-volatile component in the resin composition is set to 100 volume %, the content (volume %) of the (C-2) solid inorganic filler material can be 0 volume % or greater than 0 volume %, preferably 5 volume % or more, more preferably 10 volume % or more, further preferably 20 volume % or more, preferably 50 volume % or less, more preferably 40 volume % or less, further preferably 30 volume % or less.
[0067] The proportion of pores contained in the (C) inorganic filling material as a whole, including both (C-1) hollow inorganic filling material and (C-2) solid inorganic filling material, can be obtained as the porosity (volume %) of the (C) inorganic filling material. The porosity (volume %) of the (C) inorganic filling material is a representative value representing the proportion of pores in the volume of the (C) inorganic filling material on a volume basis, and is expressed as "total volume of pores / total volume of (C) inorganic filling material". The specific range of the porosity of the (C) inorganic filling material is preferably 10% by volume or more, more preferably 15% by volume or more, further preferably 20% by volume or more, preferably 80% by volume or less, more preferably 70% by volume or less, and further preferably 60% by volume or less.
[0068] From the viewpoint of significantly achieving the effects of the present invention, the average particle size of the (C) inorganic filler material as a whole, including both the (C-1) hollow inorganic filler material and the (C-2) solid inorganic filler material, is preferably greater than 0.01 μm, more preferably greater than 0.1 μm, further preferably greater than 0.3 μm, preferably less than 5 μm, more preferably less than 4 μm, further preferably less than 3 μm.
[0069] From the viewpoint of remarkably obtaining the effect of the present invention, the BET specific surface area of the entire inorganic filler (C) including both the hollow inorganic filler (C-1) and the solid inorganic filler (C-2) is preferably 1 m 2 / g or more, preferably 2m 2 / g or more, more preferably 5m 2 / g or more, preferably 100m 2 / g or less, preferably 50m 2 / g or less, more preferably 30m 2 / g or less.
[0070] When the (C) component includes both (C-1) hollow inorganic filler and (C-2) solid inorganic filler, from the viewpoint of significantly obtaining the effect of the present invention, when the content of all inorganic fillers is set to 100 volume %, the content (volume %) of the (C-1) hollow inorganic filler in all inorganic fillers is preferably 0 volume %, more preferably 0 volume % or more, further preferably 30 volume % or more, preferably 100 volume %, more preferably 100 volume % or less, and further preferably 75 volume % or less.
[0071] From the viewpoint of significantly obtaining the effects of the present invention, when the non-volatile component in the resin composition is set to 100 mass %, the content (mass %) of the (C) inorganic filler is preferably 50 mass % or more, more preferably 55 mass % or more, further preferably 60 mass % or more, preferably 85 mass % or less, more preferably 80 mass % or less, and particularly preferably 75 mass % or less.
[0072] From the viewpoint of significantly obtaining the effects of the present invention, when the non-volatile component in the resin composition is set to 100 volume %, the content (volume %) of the (C) inorganic filler is preferably 20 volume % or more, more preferably 30 volume % or more, further preferably 40 volume % or more, preferably 80 volume % or less, more preferably 75 volume % or less, and particularly preferably 70 volume % or less.
[0073] <(D) Silane compound having a silicon atom as a ring-constituting atom> The resin composition contains a silane compound having a silicon atom as a ring-forming atom (D) as the component (D). The silane compound having a silicon atom as a ring-forming atom as the component (D) does not include substances belonging to the above-mentioned components (A) to (C). By making the resin composition contain the component (D), the halo phenomenon can be suppressed. The component (D) may be used alone or in combination of two or more.
[0074] As component (D), a compound having a cyclic structure and containing a silicon atom as a ring-forming atom constituting the cyclic structure can be used. The cyclic structure may be a monocyclic, polycyclic, or condensed ring, and from the viewpoint of significantly obtaining the effect of the present invention, a monocyclic is preferred. In addition, the cyclic structure may be a saturated cyclic structure or an unsaturated cyclic structure, and from the viewpoint of significantly obtaining the effect of the present invention, a saturated cyclic structure is preferred. The cyclic structure is preferably a three- to ten-membered ring, more preferably a four- to six-membered ring, further preferably a five- or six-membered ring, and particularly preferably a five-membered ring.
[0075] The cyclic structure has a carbon atom as a ring-forming atom in addition to a silicon atom. In addition, the ring-forming atom may have a heteroatom such as a nitrogen atom, an oxygen atom, a sulfur atom, etc. From the viewpoint of significantly obtaining the effect of the present invention, the component (D) preferably has a silicon atom, a carbon atom, and a nitrogen atom as a ring-forming atom, and the component (D) is preferably a cyclic silazane compound.
[0076] The number of silicon atoms as ring-constituting atoms is preferably 1-5, more preferably 1 or 2, further preferably 1. When a hetero atom is contained as a ring-constituting atom, the number of the hetero atom is preferably 1-3, more preferably 1 or 2, further preferably 1.
[0077] The component (D) preferably has 1 to 3 cyclic structures in one molecule, more preferably 1 or 2 cyclic structures, further preferably 1 cyclic structure.
[0078] The silicon atom as the ring-forming atom in the component (D) is preferably combined with an alkoxy group. As the alkoxy group, methoxy, ethoxy, propoxy, isopropoxy, butoxy, pentyloxy, hexyloxy etc. can be mentioned. Among them, as the alkoxy group, methoxy is preferably used from the viewpoint of significantly obtaining the effect of the present invention.
[0079] As the component (D), a compound represented by the formula (D-1) is preferred. [Chemical formula 1] In the formula, R 1 and R 2 Each independently represents a monovalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, A represents a hetero atom, and n represents an integer of 1 to 4.
[0080] R 1 and R 2Each independently represents a monovalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. The monovalent hydrocarbon group having 1 to 20 carbon atoms is preferably a monovalent hydrocarbon group having 1 to 15 carbon atoms, more preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms, and further preferably a monovalent hydrocarbon group having 1 to 6 carbon atoms. The number of carbon atoms does not include the number of carbon atoms of the substituent. Examples of the monovalent hydrocarbon group include alkyl, alkenyl, and aryl groups. The alkyl group may be any of linear, branched, and cyclic, and the preferred number of carbon atoms is as described above. Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, sec-butyl, n-pentyl, isopentyl, neopentyl, cyclopentyl, n-hexyl, isohexyl, cyclohexyl, n-heptyl, isoheptyl, n-octyl, isooctyl, tert-octyl, n-nonyl, isononyl, n-decyl, and isodecyl. The alkenyl group may be any of a straight chain, a branched chain, and a cyclic group, and the preferred number of carbon atoms is as described above. Examples of the alkenyl group include vinyl, allyl, butenyl, methallyl, and the like. Examples of the aryl group include phenyl, tolyl, xylyl, and the like. Preferably, the aryl group is an aryl group. From the viewpoint of significantly obtaining the effect of the present invention, R 1 Preferably it is an aryl group, more preferably a phenyl group. In addition, from the viewpoint of significantly obtaining the effect of the present invention, R 2 Preferred is an alkyl group, more preferred is a methyl group.
[0081] R 1 and R 2 The monovalent hydrocarbon group represented by may have a substituent. The substituent is not particularly limited, and examples thereof include a halogen atom, -OH, -OC 1-6 Alkyl, -N(C 1-10 Alkyl)2, C 1-20 Alkyl, C 2-30 Alkenyl, C 2-30 Alkynyl, C 6-10 Aryl, -NH2, -CN, -C(O)OC 1-10 Alkyl, -COOH, -C(O)H, -NO2, etc. Here, the term "C p-q " means that the number of carbon atoms in the organic group immediately following the term is p to q, where p and q are positive integers and p < q. For example, "C 1-10 The expression "alkyl" means an alkyl group having 1 to 10 carbon atoms. These substituents may be combined with each other to form a ring, and the ring structure may include a spiro ring or a condensed ring.
[0082] A represents a heteroatom, and the heteroatom is as described above.
[0083] n represents an integer of 1 to 4, preferably 2 or 3, more preferably 3.
[0084] Examples of the component (D) include 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-methyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-methyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-butyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-butyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-butyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-methyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-methyl-1-aza-2-silacyclopentane, 2-Methyl-1-butyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-butyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-cyclohexyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-cyclohexyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-phenyl-1-aza-2 -Silacyclopentane, 2,2-dimethyl-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-phenyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-phenyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2-ethoxy-2 -methyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2,2-Dimethoxy-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-trimethoxysilylpropyl)- 1-Aza-2-silacyclopentane, 2,2-dimethyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane Silcyclopentane, 2,2-diethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silcyclopentane, 2-ethoxy-2-methyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silcyclopentane, 2,2-dimethoxy-1-methyldimethoxysilylmethyl-1-aza-2-silcyclopentane, 2-methoxy-2-methyl-1-methyldimethoxysilylmethyl-1-aza-2-silcyclopentane, 2,2-dimethyl-1-methyldimethoxysilylmethylmethyl-1-aza-2-silcyclopentane, 2,2-diethoxy-1-methyldimethoxysilylmethylmethyl-1-aza-2-silcyclopentane, 2-ethoxy- 2-Methyl-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Dimethoxy-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy 2-Methoxy-2-methyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane 2,2-Dimethoxy-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-dimethyl 2-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-(2-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-Dimethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-triethoxysilylbutyl)-1-aza-2- Silolane, 2-methoxy-2-methyl-1-(4-triethoxysilylbutyl)-1-aza-2-silolane, 2,2-dimethyl-1-(4-triethoxysilylbutyl)-1-aza-2-silolane, 2,2-diethoxy-1-(4-triethoxysilylbutyl)-1-aza-2-silolane, 2-ethoxy-2-methyl-1-(4-triethoxysilylbutyl)-1-aza-2-silolane, 2,2-dimethoxy-1-methyldiethoxysilylmethyl-1-aza-2-silolane, 2-methoxy-2-methyl-1-methyldiethoxysilylmethyl-1- Aza-2-silacyclopentane, 2,2-dimethyl-1-methyldiethoxysilylmethylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane 2,2-Dimethoxy-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-Dimethoxy ...2-Diethoxy-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl -1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2- Dimethoxy-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl -1-methyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-methyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-methyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-butyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-butyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-butyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-butyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-butyl-1-aza-2-silacyclopentane, 2,2-2-Dimethoxy-1-cyclohexyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-cyclohexyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-phenyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-phenyl-1-aza-2-silacyclopentane 2-Silacyclopentane, 2-ethoxy-2-methyl-1-phenyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(2-methoxycarbonyl-2- 2-Methoxy-2-methyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-trimethoxysilyl methyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-( 4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-methyldimethoxysilylmethylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane -2-silacyclopentane, 2-methoxy-2-methyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane Aza-2-silacyclopentane, 2,2-dimethyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2 -methyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2 -Dimethoxy-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane -2-silacyclopentane, 2,2-dimethyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-methyldiethoxysilylmethylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-methyldiethoxysilylmethylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-methyldiethoxysilylmethyl Silylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-methyldiethoxysilyl) 2-(4-Methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-dimethylethoxysilylmethyl-1 -Aza-2-silacyclopentane, 2,2-dimethyl-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2 -Dimethyl-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, tetrakis(3,4-epoxycyclohexylethyl)-tetramethylcyclotetrasiloxane, bis(3-glycidyloxypropyl)-hexaalkylcyclotetrasiloxane, etc.
[0085] (D) Component may be a commercially available product, such as "X-88-398" (2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane) manufactured by Shin-Etsu Chemical Co., Ltd., "KR-470", "X-40-2678", and "X-40-2728" manufactured by Shin-Etsu Silicone Co., Ltd.
[0086] The form of the component (D) contained in the resin composition of the present invention is not particularly limited, and it is preferably contained in the resin composition in any of the following forms (i) to (iii), more preferably in any of the forms (ii) and (iii), and further preferably in the form (iii). (i) The component (D) is contained alone in the resin composition; (ii) Component (D) contains as a surface treatment agent for (C) inorganic filler; (iii) The component (D) is contained as a surface treatment agent for the inorganic filler (C), and the component (D) is contained independently in the resin composition.
[0087] “(D) component is contained as a surface treatment agent for (C) inorganic filler” means that (C) inorganic filler is surface-treated with (D) component. In this case, (D) component is usually present on the surface of (C) inorganic filler. In addition, “(D) component is contained alone in the resin composition” means that (D) component is not contained as a surface treatment agent for (C) inorganic filler. It should be noted that when (D) component is not contained as a surface treatment agent for (C) inorganic filler, (D) component is free in the resin composition. In the present invention, (D) component can be used to uniformly treat the surface of (C) inorganic filler, so the halo phenomenon can be effectively suppressed.
[0088] When component (D) is contained as a surface treatment agent for component (C), from the viewpoint of suppressing the halo phenomenon, when the non-volatile component in the resin composition is set to 100% by mass, the content of component (D) is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, further preferably 0.5% by mass or more, preferably 3% by mass or less, more preferably 2.5% by mass or less, further preferably 2% by mass or less.
[0089] When component (D) is contained as a surface treatment agent for component (C), from the viewpoint of suppressing the halo phenomenon, when the resin component in the resin composition is set to 100% by mass, the content of component (D) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, further preferably 0.8% by mass or more, 1% by mass or more, 1.5% by mass or more, preferably less than 5% by mass, more preferably less than 4% by mass, further preferably less than 3% by mass.
[0090] When component (D) is contained as a surface treatment agent for component (C), from the viewpoint of suppressing the halo phenomenon, the degree of surface treatment with component (D) (content of component (D)) relative to 100% by mass of the inorganic filler (C) is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, further preferably 0.3% by mass or more, or 0.6% by mass or more, preferably 8% by mass or less, more preferably 5% by mass or less, further preferably 4% by mass or less.
[0091] When the content (mass %) of the component (B) when the non-volatile component in the resin composition is 100 mass % is b, and the content (mass %) of the component (D) when the non-volatile component in the resin composition is 100 mass % is d, b / d is preferably 1 or more, more preferably 2 or more, further preferably 3 or more, preferably 50 or less, more preferably 40 or less, further preferably 30 or less, 20 or less, 15 or less, or 10 or less. By adjusting the contents of the component (B) and the component (D) under the condition that b / d is within the range, a cured product with low dielectric properties can be obtained, and the halo phenomenon can also be suppressed.
[0092] <(E) Curing agent> In addition to the above-mentioned components, the resin composition may further include (E) a curing agent as an arbitrary component. The (E) curing agent as the (E) component does not include substances belonging to the above-mentioned (A) to (D) components. As the (E) curing agent, a compound having a function of reacting with the (A) component to cure the resin composition may be used, such as phenol curing agents, naphthol curing agents, carbodiimide curing agents, benzoxazine curing agents, cyanate curing agents, etc. Among them, from the viewpoint of significantly obtaining the effect of the present invention, the (E) curing agent preferably includes a phenol curing agent. The (E) curing agent may be used alone or in combination of two or more.
[0093] As phenolic curing agent and naphthol curing agent, from the viewpoint of heat resistance and water resistance, preferably a phenolic curing agent with a phenolic structure or a naphthol curing agent with a phenolic structure. In addition, from the viewpoint of adhesion with the conductor layer, preferably a nitrogen-containing phenolic curing agent, more preferably a phenolic curing agent containing a triazine skeleton.
[0094] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Chemicals Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN495V", "SN375", and "SN395" manufactured by Nippon Steel & Sumitomo Metal Chemicals Corporation, and "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA3018-50P", "EXB-9500", and "KA-1163" manufactured by DIC Corporation.
[0095] The carbodiimide curing agent is a compound having one or more carbodiimide groups (—N═C═N—) in one molecule, and the carbodiimide curing agent is preferably a compound having two or more carbodiimide groups in one molecule.
[0096] Specific examples of carbodiimide curing agents include commercially available carbodiimide curing agents such as CARBODILITE V-03 (carbodiimide group equivalent: 216 g / eq.), V-05 (carbodiimide group equivalent: 262 g / eq.), V-07 (carbodiimide group equivalent: 200 g / eq.), and V-09 (carbodiimide group equivalent: 200 g / eq.) manufactured by Nisshinbo Chemical Co., Ltd., and Stabaxol P (carbodiimide group equivalent: 302 g / eq.) manufactured by LANXESS.
[0097] Specific examples of the benzoxazine-based curing agent include "HFB2006M" manufactured by Showa Highpolymer Co., Ltd. and "Pd" and "Fa" manufactured by Shikoku Chemicals Co., Ltd.
[0098] Examples of the cyanate curing agent include difunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenylcyanate), 4,4'-ethylenediphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatephenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylene))benzene, bis(4-cyanatephenyl)sulfide, and bis(4-cyanatephenyl)ether; polyfunctional cyanate resins derived from phenol novolac resins and cresol novolac resins; and prepolymers obtained by partially triazinizing these cyanate resins. Specific examples of cyanate curing agents include "PT30" and "PT60" (linear phenolic multifunctional cyanate resins), "ULL-950S" (multifunctional cyanate resins), "BA230", and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate is triazine-treated to form trimers) manufactured by Arxada.
[0099] The amount ratio of component (A) to component (E) is preferably in the range of 1:0.01 to 1:10, more preferably 1:0.05 to 1:8, and further preferably 1:0.08 to 1:5, in terms of the ratio of [the total number of epoxy groups of component (A)]:[the total number of active groups of component (E)]. Here, the "total number of epoxy groups of the epoxy resin" refers to the value obtained by adding up all the values obtained by dividing the mass of the non-volatile components of component (A) present in the resin composition by the epoxy equivalent. In addition, the "total number of active groups of component (E)" refers to the value obtained by adding up all the values obtained by dividing the mass of the non-volatile components of component (E) present in the resin composition by the active group equivalent. As component (E), the effect of the present invention can be significantly obtained by making the amount ratio with component (A) within the above range.
[0100] The amount ratio of component (A) to component (B) and component (E) is preferably in the range of 1:0.01 to 1:10, more preferably 1:0.3 to 1:5, and further preferably 1:0.4 to 1:4, in terms of the ratio of [the total number of epoxy groups of component (A)]:[the total number of active groups of component (B) and component (E)]. Here, "the total number of active groups of component (B) and component (E)" refers to the value obtained by adding up all the values obtained by dividing the mass of the non-volatile components of component (B) and component (E) present in the resin composition by the active group equivalent. By making the amount ratio of component (A) to component (B) and component (E) within the above range, the effect of the present invention can be significantly obtained.
[0101] From the viewpoint of significantly obtaining the desired effect of the present invention, when the non-volatile component in the resin combination is set to 100 mass %, the content of (E) component is preferably more than 0.1 mass %, more preferably more than 0.3 mass %, and further more preferably more than 0.5 mass %. The upper limit is preferably below 8 mass %, more preferably below 5 mass %, and further more preferably below 3 mass %.
[0102] From the viewpoint of significantly obtaining the desired effect of the present invention, when the resin component in the resin composition is set to 100% by mass, the content of the component (E) is preferably 1% by mass or more, more preferably 3% by mass or more, further preferably 5% by mass or more, preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 10% by mass or less.
[0103] <(F) Curing accelerator> In addition to the above-mentioned components, the resin composition may further contain a curing accelerator as a component (F) as an arbitrary component. The (F) curing accelerator as the component (F) does not include substances belonging to the above-mentioned components (A) to (E). By making it contain the (F) component, the curing of the (A) component can be further accelerated. The (F) component can be used alone or in combination of two or more.
[0104] As the component (F), for example, phosphorus curing accelerators, urea curing accelerators, guanidine curing accelerators, imidazole curing accelerators, metal curing accelerators, amine curing accelerators, etc. Among them, preferably, a curing accelerator selected from amine curing accelerators and metal curing accelerators is used, and particularly preferably, an amine curing accelerator is used.
[0105] Phosphorus curing accelerators include, for example, tetrabutylphosphonium bromide, tetrabutylphosphonium chloride, tetrabutylphosphonium acetate, tetrabutylphosphonium decanoate, tetrabutylphosphonium laurate, bis(tetrabutylphosphonium)pyromellitic acid salt, tetrabutylphosphonium hexahydrophthalate, tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, di-tert-butyldimethylphosphonium tetraphenylborate and other aliphatic phosphonium salts; methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide, butyltriphenylphosphonium bromide, benzyltriphenylphosphonium chloride, tetraphenylphosphonium bromide, para- Aromatic phosphonium salts such as tolyltriphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, etc.; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone addition reactants such as triphenylphosphine-p-benzoquinone addition reactants; tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butylphosphine aliphatic phosphines such as (2-butenyl)phosphine, di-tert-butyl (3-methyl-2-butenyl)phosphine, tricyclohexylphosphine, dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tri(4-ethylphenyl)phosphine, tri(4-propylphenyl)phosphine, tri(4-isopropylphenyl)phosphine, tri(4-butylphenyl)phosphine, tri(4-tert-butylphenyl)phosphine, tri(2,4-dimethylphenyl)phosphine, tri(2,5-dimethylphenyl)phosphine, tri(2,6-dimethylphenyl)phosphine The present invention also includes aromatic phosphines such as tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether.
[0106] Examples of the urea curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, 3-(3,4-dimethylphenyl)-1, Aromatic dimethylureas such as 1-dimethylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluenebisdimethylurea], and the like.
[0107] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanidine, 1-ethylbiguanidine, 1-n-butylbiguanidine, 1-n-octadecylbiguanidine, 1,1-dimethylbiguanidine, 1,1-diethylbiguanidine, 1-cyclohexylbiguanidine, 1-allylbiguanidine, 1-phenylbiguanidine, and 1-(o-tolyl)biguanidine.
[0108] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1') imidazole compounds such as 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, and adducts of imidazole compounds with epoxy resins.
[0109] As the imidazole curing accelerator, a commercially available product can be used, and examples thereof include "1B2PZ", "2MZA-PW", "2PHZ-PW", and "C11Z-A" manufactured by Shikoku Chemical Industry Co., Ltd. and "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0110] As metal curing accelerators, organic metal complexes or organic metal salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin can be cited. As specific examples of organic metal complexes, organic cobalt complexes such as cobalt acetylacetonate (II), cobalt acetylacetonate (III), organic copper complexes such as copper acetylacetonate (II), organic zinc complexes such as zinc acetylacetonate (II), organic iron complexes such as iron acetylacetonate (III), organic nickel complexes such as nickel acetylacetonate (II), and organic manganese complexes such as manganese acetylacetonate (II) can be cited. As organic metal salts, for example, zinc octoate, tin octoate, zinc naphthenate, cobalt naphthenate, tin stearate, zinc stearate, etc. can be cited.
[0111] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene.
[0112] As the amine curing accelerator, a commercially available product may be used, and examples thereof include "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd. and the like.
[0113] From the viewpoint of significantly obtaining the desired effect of the present invention, when the non-volatile component in the resin composition is set to 100% by mass, the content of the component (F) is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, further preferably 0.05% by mass or more, preferably 1% by mass or less, more preferably 0.8% by mass or less, further preferably 0.5% by mass or less.
[0114] From the viewpoint of significantly obtaining the desired effect of the present invention, when the resin component in the resin composition is set to 100% by mass, the content of the component (F) is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, further preferably 0.1% by mass or more, preferably 1.5% by mass or less, more preferably 1% by mass or less, further preferably 0.5% by mass or less.
[0115] <(G) Thermoplastic resin> In addition to the above-mentioned components, the resin composition may further contain (G) a thermoplastic resin as an optional component. The (G) thermoplastic resin as the (G) component does not include those belonging to the above-mentioned (A) to (F) components.
[0116] As (G) thermoplastic resin, for example, polyimide resin, phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyamide-imide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, etc. can be mentioned. In one embodiment, (G) thermoplastic resin preferably comprises a thermoplastic resin selected from polyimide resin and phenoxy resin, and more preferably comprises phenoxy resin. In addition, thermoplastic resin can be used alone or in combination of two or more.
[0117] Specific examples of the polyimide resin include "SLK-6100" manufactured by Shin-Etsu Chemical Co., Ltd., and "RIKACOAT SN20" and "RIKACOAT PN20" manufactured by Shin Nippon Rika Co., Ltd.
[0118] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenol acetophenone skeleton, phenolic skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group.
[0119] Specific examples of phenoxy resins include "1256" and "4250" manufactured by Mitsubishi Chemical Corporation (both are phenoxy resins containing a bisphenol A skeleton), "YX8100" manufactured by Mitsubishi Chemical Corporation (a phenoxy resin containing a bisphenol S skeleton), "YX6954" manufactured by Mitsubishi Chemical Corporation (a phenoxy resin containing a bisphenol acetophenone skeleton), "FX280" and "FX293" manufactured by Nippon Steel & Sumitomo Metal Chemical Corporation, "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", "YL7482" and "YL7891BH30" manufactured by Mitsubishi Chemical Corporation, etc.
[0120] As the polyvinyl acetal resin, for example, polyvinyl formal resin and polyvinyl butyral resin can be mentioned, and polyvinyl butyral resin is preferred. As specific examples of the polyvinyl acetal resin, S-LEC BH series, BX series (for example, BX-5Z), KS series (for example, KS-1), BL series, BM series, etc. manufactured by Sekisui Chemical Co., Ltd. can be mentioned.
[0121] Examples of the polyolefin resin include low-density polyethylene, ultra-low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymers, ethylene-ethyl acrylate copolymers, ethylene-methyl acrylate copolymers and other ethylene copolymer resins; polyolefin polymers such as polypropylene and ethylene-propylene block copolymers; and the like.
[0122] Examples of the polybutadiene resin include resins containing a hydrogenated polybutadiene skeleton, hydroxyl-containing polybutadiene resins, phenolic hydroxyl-containing polybutadiene resins, carboxyl-containing polybutadiene resins, acid anhydride-containing polybutadiene resins, epoxy-containing polybutadiene resins, isocyanate-containing polybutadiene resins, urethane-containing polybutadiene resins, and polyphenylene ether-polybutadiene resins.
[0123] Specific examples of polyamideimide resins include "VYLOMAX HR11NN" and "VYLOMAX HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamideimide resins include modified polyamideimides such as "KS9100" and "KS9300" (polyamideimide containing a polysiloxane skeleton) manufactured by Hitachi Chemical Co., Ltd.
[0124] Specific examples of the polyethersulfone resin include "PES5003P" manufactured by Sumitomo Chemical Co., Ltd. and the like.
[0125] Specific examples of the polysulfone resin include polysulfone "P1700" and "P3500" manufactured by Solvay High Performance Polymers.
[0126] Specific examples of the polyphenylene ether resin include "NORYL SA90" manufactured by SABIC Innovative Plastics, etc. Specific examples of the polyetherimide resin include "ULTEM" manufactured by GE, etc.
[0127] Examples of polycarbonate resins include hydroxyl-containing carbonate resins, phenolic hydroxyl-containing carbonate resins, carboxyl-containing carbonate resins, anhydride-containing carbonate resins, isocyanate-containing carbonate resins, and urethane-containing carbonate resins. Specific examples of polycarbonate resins include "FPC0220" manufactured by Mitsubishi Gas Chemical Co., Ltd., "T6002" and "T6001" (polycarbonate diols) manufactured by Asahi Kasei Corporation, and "C-1090", "C-2090", and "C-3090" (polycarbonate diols) manufactured by Kuraray Co., Ltd. Specific examples of polyetheretherketone resins include "SUMIPLOY K" manufactured by Sumitomo Chemical Co., Ltd.
[0128] Examples of the polyester resin include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, and polycyclohexane dimethyl terephthalate resin.
[0129] From the viewpoint of significantly achieving the effects of the present invention, the weight average molecular weight (Mw) of the (G) thermoplastic resin is preferably 5,000 or more, more preferably 8,000 or more, further preferably 10,000 or more, particularly preferably 20,000 or more, preferably 100,000 or less, more preferably 70,000 or less, further preferably 60,000 or less, particularly preferably 50,000 or less.
[0130] From the viewpoint of significantly obtaining the desired effect of the present invention, when the non-volatile component in the resin composition is set to 100 mass %, the content of the (G) thermoplastic resin is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, further preferably 1 mass % or more, preferably 5 mass % or less, more preferably 3 mass % or less, further preferably 2 mass % or less.
[0131] From the viewpoint of significantly obtaining the desired effect of the present invention, when the resin component in the resin composition is set to 100 mass %, the content of the (G) thermoplastic resin is preferably 1 mass % or more, more preferably 1.5 mass % or more, further preferably 2 mass % or more, and is preferably 10 mass % or less, more preferably 8 mass % or less, further preferably 5 mass % or less.
[0132] <(H) Other additives> In addition to the above-mentioned components, the resin composition may further contain other additives as arbitrary components. Examples of (H) other additives include free radical polymerizable compounds, elastomers, polymerization initiators, organic metal compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds, colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black, polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine, leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents, thickeners such as Benton and montmorillonite, defoamers such as silicone-based defoamers, acrylic-based defoamers, fluorine-based defoamers, and vinyl resin-based defoamers, ultraviolet light absorbers such as benzotriazole-based ultraviolet light absorbers, adhesion enhancers such as urea silane, adhesion enhancers such as triazole-based adhesion enhancers, tetrazole-based adhesion enhancers, and triazine-based adhesion enhancers, and hindered phenol-based antioxidants. Antioxidants such as phthalates, fluorescent whitening agents such as stilbene derivatives, surfactants such as fluorine-based surfactants and silicone-based surfactants, flame retardants such as phosphorus-based flame retardants (such as phosphate compounds, phosphazene compounds, phosphinic acid compounds, and red phosphorus), nitrogen-based flame retardants (such as melamine sulfate), halogen-based flame retardants, inorganic flame retardants (such as antimony trioxide), etc., dispersants such as phosphate-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants, stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers, tertiary amine-based photopolymerization initiation aids, and photosensitizers such as pyrazolines, anthracenes, coumarins, xanthones, and thioxanthones. (H) Other additives may be used alone or in combination of two or more.
[0133] <(I) Solvent> In addition to the above-mentioned non-volatile components, the resin composition may further contain any solvent as a volatile component. As (I) solvent, a known solvent may be appropriately used, and its type is not particularly limited, preferably an organic solvent. As (I) solvent, for example: ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone; ester solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone; ether solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, anisole; alcohol solvents such as methanol, ethanol, propanol, butanol, ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, carbitol acetate (ethyl diglycol Ether ester solvents such as acetate, γ-butyrolactone, and methyl methoxypropionate; ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. (I) The solvent may be used alone or in combination of two or more in any ratio.
[0134] In resin combination, from the viewpoint of significantly obtaining the effect of the present invention, relative to the total components 100 mass % of resin combination, it is better to include more than 0.5 mass % and less than 6 mass % (I) solvent. Specifically, relative to the total components 100 mass % of resin combination, the content of (I) solvent is preferably less than 5 mass %, more preferably less than 4 mass %, preferably more than 0.5 mass %, more preferably more than 0.8 mass %, further more preferably more than 1 mass %.
[0135] The method for preparing the resin composition of the present invention is not particularly limited, and examples thereof include a method in which a solvent or the like is added to the compounding components as necessary, and the mixture is mixed and dispersed using a rotary mixer or the like.
[0136] <Physical properties and uses of resin composition> By curing the resin composition of the present invention, an insulating layer formed of a cured product of the resin composition can be obtained. When a through hole is formed in the insulating layer and a roughening treatment is performed, a halo phenomenon can be suppressed. The above-mentioned effect is described below with reference to the accompanying drawings.
[0137] Figure 11 is a cross-sectional view schematically showing an insulating layer 100 obtained by curing the resin composition according to the first embodiment of the present invention into a sheet form together with an inner layer substrate 200. Figure 1 2 shows a cross section of the insulating layer 100 cut along a plane passing through the center 120C of the bottom 120 of the through hole 110 and parallel to the thickness direction of the insulating layer 100 .
[0138] like Figure 1 As shown, the insulating layer 100 involved in the first embodiment of the present invention is a layer obtained by curing a resin composition layer formed on an inner substrate 200 including a conductor layer 210, and is formed by a cured product of the resin composition layer. In addition, the insulating layer 100 is formed with a through hole 110. The through hole 110 is generally formed in a shape such that the diameter is larger as the surface 100U of the insulating layer 100 on the side opposite to the conductor layer 210 is closer, and the diameter is smaller as the surface 100U is closer to the conductor layer 210. It is ideally formed in a columnar shape having a constant diameter in the thickness direction of the insulating layer 100. The through hole 110 is generally formed by irradiating a laser to the surface 100U of the insulating layer 100 on the side opposite to the conductor layer 210 and removing a portion of the insulating layer 100.
[0139] The bottom of the through hole 110 on the conductor layer 210 side is appropriately referred to as the "through hole bottom" and is indicated by the symbol 120. Therefore, the diameter of the through hole bottom 120 is called the bottom diameter Lb. In addition, the opening of the through hole 110 formed on the side opposite to the conductor layer 210 is appropriately referred to as the "through hole top" and is indicated by the symbol 130. Therefore, the diameter of the through hole top 130 is called the top diameter Lt. Usually, the through hole bottom 120 and the through hole top 130 are formed so that the planar shape observed from the thickness direction of the insulating layer 100 is circular, but they can also be elliptical. In the case where the planar shape of the through hole bottom 120 and the through hole top 130 is an ellipse, the bottom diameter Lb and the top diameter Lt respectively represent the major diameter of the ellipse.
[0140] At this time, the closer the taper ratio Lb / Lt (%) obtained by dividing the bottom diameter Lb by the top diameter Lt is to 100%, the better the shape of the through hole 110. If the resin composition layer of the present invention is used, the shape of the through hole 110 can be easily controlled, so the through hole 110 with a taper ratio Lb / Lt close to 100% can be realized.
[0141] For example, for the insulating layer 100 obtained by heating the resin composition at 100°C for 30 minutes and then heating it at 180°C for 30 minutes to cure it, when a through hole 110 with a top diameter Lt of about 70 μm is formed by irradiating it with a CO2 laser under the conditions of a mask diameter of 1 mm, a pulse width of 16 μs, an energy of 0.2 mJ / shot, 2 irradiations, and a burst mode (10 kHz), the taper ratio Lb / Lt of the through hole 110 can be preferably 75% to 100%, more preferably 80% to 100%, and particularly preferably 85% to 100%.
[0142] The taper ratio Lb / Lt of the through hole 110 can be calculated from the bottom diameter Lb and the top diameter Lt of the through hole 110. In addition, the bottom diameter Lb and the top diameter Lt of the through hole 110 can be measured as follows: using FIB (focused ion beam), the insulating layer 100 is cut to reveal a cross section parallel to the thickness direction of the insulating layer 100 and passing through the center 120C of the through hole bottom 120, and then the cross section is observed with an electron microscope.
[0143] Figure 2 The insulating layer 100 and the conductive layer 210 ( Figure 2 A top view of the surface 100U on the opposite side (not shown).
[0144] like Figure 2 As shown, if the insulating layer 100 having the through hole 110 is observed, a discolored portion 140 of the insulating layer 100 may be observed around the through hole 110. The discolored portion 140 may be formed due to resin degradation when the through hole 110 is formed, and is usually formed continuously from the through hole 110. In addition, the discolored portion 140 is a whitened portion in most cases.
[0145] Figure 3 1 is a cross-sectional view schematically showing an insulating layer 100 obtained by curing the resin composition according to the first embodiment of the present invention into a sheet shape and subjected to a roughening treatment together with an inner substrate 200. Figure 3 2 shows a cross section of the insulating layer 100 cut along a plane passing through the center 120C of the through-hole bottom 120 of the through-hole 110 and parallel to the thickness direction of the insulating layer 100 .
[0146] like Figure 3 As shown, if the insulating layer 100 having the through hole 110 is subjected to a roughening process, a halo phenomenon occurs, and the insulating layer 100 of the discolored portion 140 is sometimes peeled off from the conductive layer 210, forming a gap portion 160 continuous from the edge 150 of the through hole bottom 120. The gap portion 160 is usually formed by the discolored portion 140 being eroded during the roughening process.
[0147] By using the resin composition of the present invention, the above-mentioned halo phenomenon can be suppressed. Therefore, the insulation layer 100 can be suppressed from peeling off from the conductive layer 210, so the size of the gap 160 can be reduced.
[0148] The edge 150 of the through-hole bottom 120 is equivalent to the edge portion of the inner peripheral side of the gap portion 160. Therefore, the distance Wb from the edge 150 of the through-hole bottom 120 to the end 170 of the outer peripheral side of the gap portion 160 (that is, the end on the side farther from the center 120C of the through-hole bottom 120) is equivalent to the dimension of the gap portion 160 in the in-plane direction. Here, the in-plane direction refers to the direction perpendicular to the thickness direction of the insulating layer 100. In addition, in the following description, the distance Wb is sometimes referred to as the halo distance Wb of the through-hole 110 from the edge 150 of the through-hole bottom 120. The degree of suppression of the halo phenomenon can be evaluated by the halo distance Wb from the edge 150 of the through-hole bottom 120. Specifically, the smaller the halo distance Wb from the edge 150 of the through-hole bottom 120, the more effectively the halo phenomenon can be suppressed.
[0149] For example, the insulating layer 100 obtained by curing the resin composition layer containing the resin composition by heating at 100°C for 30 minutes and then heating at 180°C for 30 minutes is irradiated with a CO2 laser under the conditions of a mask diameter of 1 mm, a pulse width of 16 μs, an energy of 0.2 mJ / time, irradiation times of 2, and a burst mode (10 kHz) to form a through hole 110 with a top diameter Lt of about 70 μm. Then, it is immersed in a swelling liquid at 60°C for 5 minutes, then immersed in an oxidant solution at 80°C for 10 minutes, then immersed in a neutralizing solution at 40°C for 5 minutes, and then dried at 80°C for 15 minutes.
[0150] The halo distance Wb from the edge 150 of the through-hole bottom 120 can be measured by using FIB (focused ion beam) to cut the insulating layer 100 to reveal a cross section parallel to the thickness direction of the insulating layer 100 and passing through the center 120C of the through-hole bottom 120, and then observing the cross section with an electron microscope.
[0151] Furthermore, by using the resin composition of the present invention, the shape of the through hole 110 of the insulating layer 100 before the roughening treatment can be easily controlled, so generally, even in the insulating layer 100 after the roughening treatment, the shape of the through hole 110 can be easily controlled. Therefore, even after the roughening treatment, the shape of the through hole 110 can be made good as before the roughening treatment. Therefore, if the resin composition of the present invention is used, in the insulating layer after the roughening treatment, the through hole 110 having a taper ratio Lb / Lt close to 100% can be realized.
[0152] For example, the insulating layer 100 obtained by curing the resin composition layer by heating it at 100°C for 30 minutes and then heating it at 180°C for 30 minutes is irradiated with a CO2 laser under the conditions of a mask diameter of 1 mm, a pulse width of 16 μs, an energy of 0.2 mJ / time, irradiation times of 2, and a burst mode (10 kHz) to form a through hole 110 with a top diameter Lt of about 70 μm. Then, it is immersed in a swelling liquid at 60°C for 5 minutes, then immersed in an oxidizing agent solution at 80°C for 10 minutes, then immersed in a neutralizing liquid at 40°C for 5 minutes, and then dried at 80°C for 15 minutes. If the resin composition of the present invention is used, the taper ratio Lb / Lt of the through hole 110 formed in the insulating layer 100 thus obtained can be preferably 76% to 100%, more preferably 80% to 100%, and particularly preferably 85% to 100%.
[0153] The taper ratio Lb / Lt of the through hole 110 can be calculated from the bottom diameter Lb and the top diameter Lt of the through hole 110. In addition, the bottom diameter Lb and the top diameter Lt of the through hole 110 can be measured by cutting the insulating layer 100 using a FIB (focused ion beam) to reveal a cross section parallel to the thickness direction of the insulating layer 100 and passing through the center 120C of the bottom 120 of the through hole, and then observing the cross section using an electron microscope.
[0154] Furthermore, according to the research of the present inventors, it is found that generally, the larger the diameter of the through hole 110, the easier it is for the size of the discoloration portion 140 to become larger, so the size of the gap portion 160 tends to become larger. Therefore, the ratio of the size of the gap portion 160 to the diameter of the through hole 110 can be used to evaluate the degree of suppression of the halo phenomenon. For example, the halo ratio Hb of the through hole 110 relative to the bottom radius Lb / 2 can be used for evaluation. Here, the bottom radius Lb / 2 of the through hole 110 refers to the radius of the through hole bottom 120 of the through hole 110. In addition, the halo ratio Hb of the through hole 110 relative to the bottom radius Lb / 2 refers to the ratio obtained by dividing the halo distance Wb from the edge 150 of the through hole bottom 120 by the bottom radius Lb / 2 of the through hole 110. The smaller the halo ratio Hb of the through hole 110 relative to the bottom radius Lb / 2, the more effectively the halo phenomenon can be suppressed.
[0155] For example, the insulating layer 100 obtained by heating the resin composition at 100°C for 30 minutes and then heating it at 180°C for 30 minutes to cure it is irradiated with a CO2 laser under the conditions of a mask diameter of 1 mm, a pulse width of 16 μs, an energy of 0.2 mJ / time, irradiation times of 2, and a burst mode (10 kHz) to form a through hole 110 with a top diameter Lt of 30 μm±2 μm. Then, it is immersed in a swelling liquid at 60°C for 5 minutes, then immersed in an oxidizing agent solution at 80°C for 10 minutes, then immersed in a neutralizing solution at 40°C for 5 minutes, and then dried at 80°C for 15 minutes. If the resin composition of the present invention is used, the halo ratio Hb of the through hole 110 formed in the insulating layer 100 thus obtained relative to the bottom radius Lb / 2 can be preferably 35% or less, more preferably 30% or less, and further preferably 25% or less.
[0156] The halo ratio Hb of the through hole 110 relative to the bottom radius Lb / 2 may be calculated from the bottom diameter Lb of the through hole 110 and the halo distance Wb of the through hole 110 from the edge 150 of the through hole bottom 120 .
[0157] Furthermore, by using the resin composition of the present invention, the formation of the discolored portion 140 when the through hole 110 is formed can be suppressed. Figure 2 As shown, the size of the discoloration portion 140 can be reduced, and ideally can be eliminated. The size of the discoloration portion 140 can be evaluated using the halo distance Wt of the through hole 110 from the edge 180 of the through hole top 130.
[0158] The edge 180 of the through-hole top 130 corresponds to the edge portion of the inner peripheral side of the discoloration portion 140. The halo distance Wt from the edge 180 of the through-hole top 130 represents the distance from the edge 180 of the through-hole top 130 to the edge portion 190 of the outer peripheral side of the discoloration portion 140. The smaller the halo distance Wt from the edge 180 of the through-hole top 130, the more effectively the formation of the discoloration portion 140 can be evaluated.
[0159] The halo distance Wt from the edge 180 of the via top 130 may be measured by observation using an optical microscope.
[0160] Furthermore, according to the research conducted by the present inventors, it is found that generally, the larger the diameter of the through hole 110, the easier it is for the size of the discoloration portion 140 to become larger. Therefore, the ratio of the size of the discoloration portion 140 to the diameter of the through hole 110 can be used to evaluate the degree of suppression of the formation of the discoloration portion 140. For example, the halo ratio Ht of the through hole 110 relative to the top radius Lt / 2 can be used for evaluation. Here, the top radius Lt / 2 of the through hole 110 refers to the radius of the through hole top 130 of the through hole 110. In addition, the halo ratio Ht of the through hole 110 relative to the top radius Lt / 2 refers to the ratio obtained by dividing the halo distance Wt from the edge 180 of the through hole top 130 by the top radius Lt / 2 of the through hole 110. The smaller the halo ratio Ht of the through hole 110 relative to the top radius Lt / 2, the more effectively the formation of the discoloration portion 140 can be suppressed.
[0161] For example, for the insulating layer 100 obtained by heating the resin composition layer at 100°C for 30 minutes and then heating it at 180°C for 30 minutes to cure it, when a through hole 110 with a top diameter Lt of about 70 μm is formed by irradiating it with a CO2 laser under the conditions of a mask diameter of 1 mm, a pulse width of 16 μs, an energy of 0.2 mJ / time, irradiation times of 2, and a burst mode (10 kHz), the halo ratio Ht of the through hole 110 relative to the top radius Lt / 2 can be preferably less than 45%, more preferably less than 40%, and further preferably less than 35%.
[0162] The halo ratio Ht of the via 110 relative to the top radius Lt / 2 may be calculated from the top diameter Lt of the via 110 and the halo distance Wt of the via 110 from the edge 180 of the via top 130 .
[0163] During the manufacturing process of the printed wiring board, the through hole 110 is usually formed in a state where no other conductor layer (not shown) is provided on the surface 100U of the insulating layer 100 on the side opposite to the conductor layer 210. Therefore, if the manufacturing process of the printed wiring board is known, it can be clearly recognized that there is a structure in which the through hole bottom 120 exists on the conductor layer 210 side and the through hole top 130 is opened on the side opposite to the conductor layer 210. However, in the completed printed wiring board, the conductor layer may be provided on both sides of the insulating layer 100. In this case, it may be difficult to distinguish the through hole bottom 120 and the through hole top 130 by the positional relationship with the conductor layer. However, usually, the top diameter Lt of the through hole top 130 is larger than the bottom diameter Lb of the through hole bottom 120. Therefore, in the above-mentioned case, the through hole bottom 120 and the through hole top 130 can be distinguished by the size of the diameter.
[0164] The resin composition of the present invention can suppress the halo phenomenon and can also obtain a cured product with low dielectric properties. In addition, by curing the resin composition of the present invention, an insulating layer with excellent elongation at break can usually be obtained.
[0165] The cured product obtained by heat curing the resin composition at 200° C. for 90 minutes shows the property of low dielectric loss tangent. Therefore, the cured product brings an insulating layer with low dielectric loss tangent. The dielectric loss tangent is preferably less than 0.008, more preferably less than 0.005, and further preferably less than 0.004. The lower limit of the dielectric loss tangent can be set to 0.0001 or more. The determination of the dielectric loss tangent can be measured according to the method described in the embodiments described later.
[0166] The cured product obtained by heat curing the resin composition at 200° C. for 90 minutes shows the characteristic of low relative dielectric constant. Therefore, the cured product brings an insulating layer with low relative dielectric constant. The relative dielectric constant is preferably less than 4, more preferably less than 3.5, and further preferably less than 3. The lower limit of the relative dielectric constant can be set to more than 1, etc. The determination of the relative dielectric constant can be measured according to the method described in the embodiments described later.
[0167] The cured product obtained by heat curing the resin composition at 200° C. for 90 minutes generally shows the property of high elongation at break. Therefore, the cured product brings an insulating layer with high elongation at break. The elongation at break is carried out by a tensile test based on JIS K7127. The elongation at break is preferably 1% or more, more preferably 1.3% or more, and further preferably 1.7% or more. The upper limit of the elongation at break can be set to 10% or less, etc. The determination of the elongation at break can be measured according to the method described in the embodiments described later.
[0168] The resin composition of the present invention can obtain a cured product with low dielectric properties and the ability to suppress the halo phenomenon. Furthermore, a cured product with excellent elongation at break can be obtained. Therefore, the resin composition of the present invention can be suitably used as a resin composition for insulating purposes. Specifically, it can be suitably used as: a resin composition for forming an insulating layer for forming a conductor layer (including a rewiring layer) (a resin composition for forming an insulating layer for forming a conductor layer), wherein the conductor layer is formed on the insulating layer.
[0169] Furthermore, in the multilayer printed wiring board described later, it can be suitably used as: a resin composition for forming an insulating layer of a multilayer printed wiring board (resin composition for forming an insulating layer of a multilayer printed wiring board), and a resin composition for forming an interlayer insulating layer of a printed wiring board (resin composition for forming an interlayer insulating layer of a printed wiring board).
[0170] In addition, for example, when a semiconductor chip package is manufactured through the following steps (1) to (6), the resin composition of the present invention can also be suitably used as a resin composition for a rewiring forming layer as an insulating layer for forming a rewiring layer (resin composition for forming a rewiring forming layer), and a resin composition for sealing a semiconductor chip (resin composition for sealing a semiconductor chip). When manufacturing a semiconductor chip package, a rewiring layer can be further formed on the sealing layer. (1) A step of laminating a temporary fixing film on a substrate; (2) A step of temporarily fixing the semiconductor chip on a temporary fixing film; (3) a step of forming a sealing layer on a semiconductor chip; (4) a step of peeling the substrate and the temporary fixing film from the semiconductor chip; (5) forming a rewiring forming layer as an insulating layer on the surface of the semiconductor chip from which the substrate and the temporary fixing film have been peeled off; and (6) A step of forming a rewiring layer as a conductor layer on the rewiring formation layer.
[0171] [Adhesive film] The adhesive film of the present invention includes a support and a resin composition layer formed from the resin composition of the present invention and provided on the support.
[0172] From the viewpoint of thinning of the printed wiring board and providing a cured product of the resin composition with excellent insulation even as a thin film, the thickness of the resin composition layer is preferably 100 μm or less, more preferably 80 μm or less, and further preferably 50 μm or less. The lower limit of the thickness of the resin composition layer is not particularly limited, and can usually be set to 5 μm or more.
[0173] Examples of the support include films formed of a plastic material, metal foil and release paper, and films formed of a plastic material and metal foil are preferred.
[0174] When a film formed of a plastic material is used as a support, the plastic material includes polyesters such as polyethylene terephthalate (hereinafter sometimes referred to as "PET") and polyethylene naphthalate (hereinafter sometimes referred to as "PEN"), polycarbonate (hereinafter sometimes referred to as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among them, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0175] When a metal foil is used as a support, examples of the metal foil include copper foil and aluminum foil, preferably copper foil. As the copper foil, a foil formed of a single metal of copper can be used, or a foil formed of an alloy of copper and other metals (such as tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) can be used.
[0176] The surface of the support to be in contact with the resin composition layer may be subjected to matte treatment, corona discharge treatment, or antistatic treatment.
[0177] In addition, as a support, a support with a release layer having a release layer on the surface bonded to the resin composition layer can be used. As a release agent for the release layer of the support with a release layer, for example, one or more release agents selected from alkyd resins, polyolefin resins, polyurethane resins and silicone resins can be cited. The support with a release layer can use commercial products, for example, "SK-1", "AL-5", "AL-7" made by Lintec Co., Ltd., which is a PET film having a release layer with an alkyd resin release agent as the main component, "LUMIRROR T60" made by Toray Industries, Ltd., "Purex" made by Teijin Limited, "Unipeel" made by Unitika Co., Ltd., etc. can be cited.
[0178] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, the entire thickness of the support with a release layer is preferably within the above range.
[0179] In one embodiment, the adhesive film may further include other layers as needed. As the other layers, for example, a protective film selected according to the support body and disposed on the surface of the resin composition layer that is not bonded to the support body (i.e., the surface on the side opposite to the support body) can be cited. The thickness of the protective film is not particularly limited, for example, 1 μm to 40 μm. By laminating the protective film, it is possible to suppress the adhesion of garbage or the formation of damage on the surface of the resin composition layer.
[0180] The adhesive film can be produced, for example, by preparing a resin varnish by dissolving the resin composition in a solvent, applying the resin varnish on a support using a die coater or the like, and drying to form a resin composition layer. The solvent is as described above.
[0181] Drying can be carried out by known methods such as heating and hot air blowing. The drying conditions are not particularly limited, and the drying is carried out under the condition that the content of the solvent in the resin composition layer is 10% by mass or less, preferably 5% by mass or less. It varies depending on the boiling point of the solvent in the resin varnish. For example, in the case of using a resin varnish containing 30% by mass to 60% by mass of a solvent, the resin composition layer can be formed by drying at 50° C. to 150° C. for 3 minutes to 10 minutes.
[0182] The adhesive film can be stored in a roll shape. When the adhesive film has a protective film, it can be used by peeling off the protective film.
[0183] [Printed wiring board] The printed wiring board of the present invention includes an insulating layer formed from a cured product of the resin composition of the present invention.
[0184] The printed wiring board can be produced, for example, by using the above-mentioned adhesive film through a method including the following steps (I) and (II): (I) laminating the adhesive film on the inner substrate so that the resin composition layer is bonded to the inner substrate; (II) A step of thermally curing the resin composition layer to form an insulating layer.
[0185] The "inner substrate" used in step (I) refers to a component that becomes a substrate of a printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, a thermosetting polyphenylene ether substrate, and the like. In addition, the substrate may have a conductor layer on one or both sides thereof, and the conductor layer may be patterned. An inner substrate having a conductor layer (circuit) formed on one or both sides of a substrate is sometimes referred to as an "inner circuit substrate". In addition, an intermediate product that requires further formation of an insulating layer and / or a conductor layer when manufacturing a printed wiring board is also included in the "inner substrate" referred to in the present invention. In the case where the printed wiring board is a circuit board with built-in components, an inner substrate with built-in components can be used.
[0186] The inner substrate and the adhesive film can be laminated, for example, by heat-pressing the adhesive film to the inner substrate from the support body side. As a member for heat-pressing the adhesive film to the inner substrate (hereinafter also referred to as "heat-pressing member"), for example, a heated metal plate (SUS end plate, etc.) or a metal roller (SUS roller) etc. can be cited. It should be noted that it is better not to press the heat-pressing member directly on the adhesive film, but to press it with an elastic material such as heat-resistant rubber so that the adhesive film fully conforms to the surface unevenness of the inner substrate.
[0187] The lamination of the inner substrate and the adhesive film can be implemented by vacuum lamination. In the vacuum lamination method, the heating and pressing temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the heating and pressing pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the heating and pressing time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. Lamination is preferably implemented under reduced pressure conditions of 26.7hPa or less.
[0188] Lamination can be performed by a commercially available vacuum laminator. Examples of the commercially available vacuum laminator include a vacuum pressure laminator manufactured by Meiki Mfg. Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., and a batch vacuum pressure laminator.
[0189] After lamination, the laminated adhesive film may be smoothed by, for example, pressing a heat-pressing member from the support body side under normal pressure (atmospheric pressure). The pressing conditions for the smoothing treatment may be the same as the heat-pressing conditions for the above-mentioned lamination. The smoothing treatment may be performed by a commercially available laminator. It should be noted that the lamination and smoothing treatment may be performed continuously using the above-mentioned commercially available vacuum laminator.
[0190] The support may be removed between step (I) and step (II), or may be removed after step (II).
[0191] In step (II), the resin composition layer is thermally cured to form an insulating layer. The thermal curing conditions of the resin composition layer are not particularly limited, and conditions generally used when forming an insulating layer of a printed wiring board can be used.
[0192] For example, the heat curing conditions of the resin composition layer vary depending on the type of the resin composition, and the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and further preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and further preferably 15 minutes to 100 minutes.
[0193] The resin composition layer may be preheated at a temperature lower than the curing temperature before the resin composition layer is thermally cured. For example, the resin composition layer may be preheated at a temperature of 50°C or more and less than 120°C (preferably 60°C or more and 115°C or less, more preferably 70°C or more and 110°C or less) for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and further preferably 15 minutes to 100 minutes) before the resin composition layer is thermally cured.
[0194] When manufacturing a printed wiring board, the step of (III) opening holes in the insulating layer, the step of (IV) roughening the insulating layer, and the step of (V) forming a conductor layer can be further implemented. These steps (III) to (V) can be implemented according to various methods known to those skilled in the art used in the manufacture of printed wiring boards. It should be noted that when the support body is removed after step (II), the removal of the support body can be implemented between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). In addition, the formation of the insulating layer and the conductor layer of steps (II) to (V) can be repeatedly implemented as needed to form a multilayer wiring board.
[0195] Step (III) is a step of drilling holes in the insulating layer, thereby forming holes such as through holes and vias in the insulating layer. Step (III) can be performed using, for example, a drill, laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The size and shape of the hole can be appropriately determined according to the design of the printed wiring board.
[0196] Step (IV) is a step of roughening the insulating layer. Usually, in step (IV), contamination is also removed. The steps and conditions of the roughening treatment are not particularly limited, and the known steps and conditions commonly used when forming the insulating layer of the printed wiring board can be adopted. For example, the insulating layer can be roughened by swelling treatment using a swelling liquid, roughening treatment using an oxidant, and neutralization treatment using a neutralizing liquid in sequence. The swelling liquid used in the roughening treatment is not particularly limited, and exemplified are alkaline solutions, surfactant solutions, etc., preferably alkaline solutions, and more preferably sodium hydroxide solutions and potassium hydroxide solutions as the alkaline solution. Examples of commercially available swelling liquids include "Swelling Dip Securiganth P", "Swelling Dip Securiganth SBU", and "Swelling Dip Securiganth P" manufactured by Atotech Japan Co., Ltd. The swelling treatment using the swelling liquid is not particularly limited, and can be performed, for example, by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 minute to 20 minutes. From the viewpoint of controlling the swelling of the resin of the insulating layer to an appropriate level, it is preferred to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 minutes to 15 minutes. As the oxidant used in the roughening treatment, there is no particular limitation, and an alkaline permanganate solution obtained by dissolving potassium permanganate or sodium permanganate in an aqueous solution of sodium hydroxide can be cited. The roughening treatment using an oxidant such as an alkaline permanganate solution is preferably carried out by immersing the insulating layer in an oxidant solution heated to 60°C to 100°C for 10 minutes to 30 minutes. In addition, the concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. As commercially available oxidants, alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing solution Securiganth P" manufactured by Atotech Japan Co., Ltd. can be cited. In addition, as a neutralizing solution used in the roughening treatment, an acidic aqueous solution is preferred, and as a commercially available product, for example, "Reduction solution Securiganth P" manufactured by Atotech Japan Co., Ltd. can be cited. The treatment with a neutralizing solution can be performed by immersing the treated surface subjected to the roughening treatment with an oxidizing agent in a neutralizing solution at 30° C. to 80° C. for 1 to 30 minutes. From the viewpoint of operability, etc., a method in which the object subjected to the roughening treatment with an oxidizing agent is immersed in a neutralizing solution at 40° C. to 70° C. for 5 to 20 minutes is preferred.
[0197] In one embodiment, the arithmetic mean roughness (Ra) of the insulating layer surface after roughening treatment is preferably less than 300nm, more preferably less than 250nm, and further preferably less than 200nm. There is no particular limitation on the lower limit, but it is preferably more than 30nm, more preferably more than 40nm, and further preferably more than 50nm. The arithmetic mean roughness (Ra) of the insulating layer surface can be measured using a non-contact surface roughness meter.
[0198] Step (V) is a step of forming a conductor layer, and a conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer comprises one or more metals selected from gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer. As the alloy layer, for example, a layer formed by an alloy of two or more metals selected from the above metals (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy) may be cited. Among them, from the viewpoints of versatility, cost, ease of pattern formation, etc., of the formation of the conductor layer, preferably, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of nickel-chromium alloy, copper-nickel alloy, or copper-titanium alloy, more preferably, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of nickel-chromium alloy, and further preferably, a single metal layer of copper.
[0199] The conductor layer may be a single layer structure, or a multilayer structure in which two or more single metal layers or alloy layers formed of different types of metals or alloys are stacked. When the conductor layer is a multilayer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.
[0200] The thickness of the conductor layer varies depending on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, preferably 5 μm to 30 μm.
[0201] In one embodiment, the conductor layer can be formed by plating. For example, the conductor layer having a desired wiring pattern can be formed by plating on the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method. From the perspective of manufacturing simplicity, it is preferably formed by a semi-additive method. An example of forming a conductor layer by a semi-additive method is shown below.
[0202] First, a plating seed layer is formed on the surface of the insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a portion of the plating seed layer corresponding to the desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Then, the unnecessary plating seed layer is removed by etching or the like, thereby forming a conductor layer having a desired wiring pattern.
[0203] [Semiconductor devices] The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be produced using the printed wiring board of the present invention.
[0204] Examples of the semiconductor device include various semiconductor devices used in electrical products (such as computers, mobile phones, digital cameras, and televisions) and vehicles (such as motorcycles, automobiles, trains, ships, and aircraft).
[0205] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) at a conductive position of a printed wiring board. "Conductive position" refers to "a position in a printed wiring board where an electrical signal is conducted", and the position may be a surface position or an embedded position. In addition, the semiconductor chip is not particularly limited as long as it is an electrical circuit element made of semiconductor.
[0206] The method for mounting a semiconductor chip when manufacturing a semiconductor device is not particularly limited as long as the semiconductor chip functions effectively. Specifically, there can be cited a wire bonding mounting method, a flip chip mounting method, a mounting method using a solderless build-up layer (BBUL), a mounting method using an anisotropic conductive film (ACF), a mounting method using a non-conductive film (NCF), etc. Here, "a mounting method using a solderless build-up layer (BBUL)" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess of a printed wiring board to connect the semiconductor chip to the wiring on the printed wiring board". Example
[0207] Hereinafter, the present invention will be described in more detail using examples, but the present invention is not limited to these examples. It should be noted that in the following description, "parts" and "%" refer to "parts by mass" and "mass %" respectively, unless otherwise specified.
[0208] <Measurement of average particle size of inorganic filler> 100 mg of inorganic filler and 10 g of methyl ethyl ketone were weighed in a vial and dispersed by ultrasonic wave for 10 minutes. A laser diffraction particle size distribution measuring device (LA-960 manufactured by Horiba, Ltd.) was used, and the wavelength of the light source was set to blue and red, and the particle size distribution of the inorganic filler was measured by flow cell method on a volume basis. Based on the obtained particle size distribution, the average particle size of the inorganic filler was calculated as the median particle size.
[0209] <Measurement of average porosity of inorganic filler> The density of the inorganic filler was measured using a true density measuring device ("ULTRAPYCNOMETER 1000" manufactured by Quantachrome). In this measurement, nitrogen was used as the measuring gas. Then, the measured density (measured value) D M (g / cm 3 ) and the material density (theoretical value) D of the inorganic material (silicon dioxide) forming the inorganic filler T (g / cm 3 ), the average porosity of the inorganic filler was determined according to the above formula (I). In the above formula (I), the material density (theoretical value) of silicon dioxide as an inorganic material is 2.2 g / cm 3 .
[0210] <Synthesis Example 1: Production of Hollow Silica Particles 1> Hollow silica particles 1 were synthesized according to the description of Japanese Patent No. 5864299. The obtained hollow silica particles 1 had an average particle size of 2.0 μm and a porosity of 50% by volume.
[0211] <Example 1> 280 parts of solid silica (average particle size 0.5 μm, "SO-C2" manufactured by Yaduma Co., Ltd.) and 1.68 parts of an aminosilane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed with 100 parts of MEK and 20 parts of solvent naphtha, heated and stirred at 60° C. for 2 hours, and then cooled to room temperature. Thus, a stirred liquid containing solid silica surface-treated with an aminosilane coupling agent was obtained. Into the stirred liquid, 30 parts of bisphenol A epoxy resin ("828US" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent of about 180 g / eq.), 30 parts of biphenyl epoxy resin ("NC3000H" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 269 g / eq.), 14 parts of a phenolic curing agent containing a triazine skeleton ("LA-3018-50P" manufactured by DIC Corporation, hydroxyl equivalent of about 151 g / eq., 2-methoxypropanol solution with a non-volatile content of 50%), and 40 parts of an active esterified A resin varnish was prepared by uniformly dispersing a mixture of 10 parts of a phenoxy resin (“YX6954BH30” manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a non-volatile content of 30% by mass) and 6 parts of a curing accelerator (“DMAP”, 4-dimethylaminopyridine, a MEK solution with a solid content of 5% by mass) in a high-speed rotating mixer.
[0212] As a support, a PET film ("LUMIRROR R80" manufactured by Toray Industries, Ltd., thickness 38 μm) subjected to a release treatment with an alkyd resin release agent ("AL-5" manufactured by Lintec Co., Ltd.) was prepared. The resin varnish was uniformly applied to the release layer of the support using a die coater so that the thickness of the resin composition layer after drying was 40 μm, and dried at 80 to 120° C. (average 100° C.) for 4 minutes to prepare an adhesive film.
[0213] <Example 2> In Example 1, the stirring liquid containing solid silica surface-treated with an aminosilane coupling agent was changed to a stirring liquid containing solid silica surface-treated with an aminosilane coupling agent and hollow silica surface-treated with an aminosilane coupling agent. The same operation as in Example 1 was performed except for the above matters to prepare a resin varnish and an adhesive film.
[0214] A stirred liquid containing solid silica surface-treated with an aminosilane coupling agent and hollow silica surface-treated with an aminosilane coupling agent is obtained by the following method. 140 parts of solid silica (average particle size 0.5 μm, "SO-C2" manufactured by Yaduma Co., Ltd.), 70 parts of hollow silica (average particle size 0.5 μm, porosity 50% by volume, "LHP-208" manufactured by Ube Exsymo Co., Ltd.) and 2.24 parts of aminosilane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) are mixed with 100 parts of MEK and 20 parts of solvent naphtha, heated and stirred at 60°C for 2 hours, and then cooled to room temperature. Thus, a stirred liquid containing solid silica surface-treated with an aminosilane coupling agent and hollow silica surface-treated with an aminosilane coupling agent is obtained.
[0215] <Example 3> In Example 2, 1) 70 parts of hollow silica (average particle size 0.5 μm, porosity 50% by volume, “LHP-208” manufactured by Ube Exsymo Co., Ltd.) were replaced with 70 parts of hollow silica particles 1 (average particle size 2.0 μm, porosity 50% by volume), 2) The amount of the silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 2.24 parts to 3.08 parts; A resin varnish and an adhesive film were prepared in the same manner as in Example 2 except for the above matters.
[0216] <Example 4> In Example 1, 1) 280 parts of solid silica (average particle size 0.5 μm, "SO-C2" manufactured by Yaduma Co., Ltd.) were replaced with 140 parts of hollow silica particles 1 (average particle size 2.0 μm, porosity 50% by volume), 2) The amount of the silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 1.68 parts to 4.48 parts; except for the above matters, the same operation as in Example 1 was carried out to prepare a resin varnish and an adhesive film.
[0217] <Example 5> In Example 1, the amount of the silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 1.68 parts to 0.84 parts. A resin varnish and an adhesive film were prepared in the same manner as in Example 1 except for the above matters.
[0218] <Example 6> In Example 4, the amount of the silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 4.48 parts to 2.24 parts. A resin varnish and an adhesive film were prepared in the same manner as in Example 4 except for the above matters.
[0219] <Comparative Example 1> In Example 1, 1.68 parts of silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was replaced with 1.68 parts of aminosilane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) A resin varnish and an adhesive film were prepared in the same manner as in Example 1 except for the above matters.
[0220] <Comparative Example 2> In Example 4, 4.48 parts of silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was replaced with 4.48 parts of aminosilane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) A resin varnish and an adhesive film were prepared in the same manner as in Example 4 except for the above matters.
[0221] <Comparative Example 3> In Example 4, 4.48 parts of silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was replaced with 8.96 parts of aminosilane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) A resin varnish and an adhesive film were prepared in the same manner as in Example 4 except for the above matters.
[0222] <Comparative Example 4> In Example 1, 1.68 parts of silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was not used. Except for the above matters, the same operation as in Example 1 was carried out to prepare a resin varnish and an adhesive film.
[0223] <Preparation of Cured Material for Evaluation> The adhesive films having a thickness of 40 μm prepared in Examples and Comparative Examples were heated at 200° C. for 90 minutes to thermally cure the resin composition layer, and then the support was peeled off. The obtained cured product was referred to as a “cured product for evaluation”.
[0224] <Measurement of relative dielectric constant and dielectric loss tangent> The cured product for evaluation was cut into a test piece with a width of 2 mm and a length of 80 mm. For the test piece, the relative dielectric constant and dielectric loss tangent were measured by the resonant cavity perturbation method at a measurement frequency of 5.8 GHz and a measurement temperature of 23° C. Two test pieces were measured and the average value was calculated.
[0225] <Determination of elongation at break> The cured product for evaluation was subjected to a tensile test using a Tensilon universal testing machine ("RTC-1250A" manufactured by Orientec Corporation) in accordance with Japanese Industrial Standards (JIS K7127) to measure the elongation at break.
[0226] <Production of samples for halo evaluation> (1) Base treatment of inner layer circuit board Both sides of a glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.4 mm, R1515A manufactured by Panasonic Corporation) with an inner layer circuit formed thereon were etched 1 μm with a microetchant (CZ8101 manufactured by MEC Corporation) to roughen the copper surface.
[0227] (2) Lamination of adhesive film with support The adhesive films were laminated on both sides of the inner layer circuit board using a batch vacuum press laminator (MVLP-500, manufactured by Meiki Seisakusho Co., Ltd.) by reducing the pressure for 30 seconds to 13 hPa or less and then pressing at 100°C and 0.74 MPa for 30 seconds.
[0228] (3) Curing of the resin composition layer The laminated adhesive film was cured under curing conditions of 130° C. for 30 minutes and then 170° C. for 30 minutes to form an insulating layer.
[0229] (4) Formation of through holes A CO2 laser processing machine (manufactured by Hitachi Via Machine Co., Ltd., LC-2E21B / 1C) was used to open holes in the insulating layer under the conditions of mask diameter 1.60 mm, focus offset 0.050, pulse width 25 μs, power 0.66 W, aperture 13, irradiation times 2, and burst mode (10 kHz), and a plurality of through holes were formed under the condition that the top diameter of the through holes in the surface of the insulating layer was about 50 μm. Then, the support was peeled off.
[0230] (5) Roughening treatment The inner layer circuit board with the insulating layer formed thereon was immersed in Swelling Dip Securiganth P (glycol ethers, aqueous solution of sodium hydroxide) containing diethylene glycol monobutyl ether manufactured by Atotech Japan Co., Ltd. as a swelling liquid at 60°C for 10 minutes, then immersed in Concentrate Compact P (aqueous solution of KMnO4: 60 g / L, NaOH: 40 g / L) manufactured by Atotech Japan Co., Ltd. as a roughening liquid at 80°C for 20 minutes, and finally immersed in Reduction Solution Securiganth P (aqueous solution of sulfuric acid) manufactured by Atotech Japan Co., Ltd. as a neutralizing liquid at 40°C for 5 minutes, and then dried at 80°C for 30 minutes. This substrate is referred to as an evaluation substrate.
[0231] <Measurement of through-hole dimensions, halo distance, and halo ratio after roughening> For the evaluation substrate, a cross-section observation was performed using a FIB-SEM composite device (SII Nanotech Co., Ltd. "SMI3050SE"). Specifically, the insulating layer was cut using a FIB (focused ion beam) to reveal a cross section parallel to the thickness direction of the insulating layer and passing through the center of the bottom of the through hole. The cross section was observed by SEM. Based on the observed image, the bottom diameter and top diameter of the through hole were measured.
[0232] In addition, in the image observed by SEM, a gap portion is visible which is continuous from the edge of the through-hole bottom and formed by the insulation layer peeling off from the copper foil layer of the inner substrate. Therefore, based on the observed image, the distance r1 from the center of the through-hole bottom to the edge of the through-hole bottom (equivalent to the inner radius of the gap portion) and the distance r2 from the center of the through-hole bottom to the end of the gap further away (equivalent to the outer radius of the gap portion) are measured, and the difference between these distances r1 and r2 (r2-r1) is calculated as the halo distance from the edge of the through-hole bottom at the measurement location.
[0233] The above measurement was performed on 5 randomly selected through holes. And the average value of the top diameters of the 5 through holes measured was used as the top diameter Lt of the sample after the roughening treatment. In addition, the average value of the bottom diameters of the 5 through holes measured was used as the bottom diameter Lb of the sample after the roughening treatment. Furthermore, the average value of the halo distances of the 5 through holes measured was used as the halo distance Wb from the edge of the bottom of the through hole of the sample.
[0234] Based on the measurement results, the taper rate (the ratio of the bottom diameter Lb to the top diameter Lt of the through hole after roughening treatment "Lb / Lt") and the halo ratio Hb (the ratio of the halo distance Wb from the edge of the bottom of the through hole after roughening treatment to the radius of the bottom of the through hole after roughening treatment (Lb / 2) "Wb / (Lb / 2)") were calculated and evaluated according to the following standards. ○: halo ratio Hb is less than 35%; △: halo ratio Hb is greater than 35% and less than 50%; ×: The halo ratio Hb is greater than 50%.
[0235] [Table 1] * In the table, the content (mass %) of component (C) indicates the content when the non-volatile component in the resin composition is set to 100 mass %, and the content (volume %) of component (C) indicates the content when the non-volatile component in the resin composition is set to 100 volume %. The content of component (D) indicates the content when the resin component in the resin composition is set to 100 mass %.
[0236] Explanation of symbols 100 insulation layer 100U The surface of the insulating layer opposite to the conductor layer 110 Through hole 120 Through hole bottom 120C Center of bottom of through hole 130 Through hole top 140 Color Change Department 150 Edge of bottom of through hole 160 Clearance 170 end 180 Edge of top of through hole 190 End of outer peripheral side 200 Inner substrate 210 conductor layer (first conductor layer) Lb Bottom diameter of through hole Lt Top diameter of through hole Wt is the distance of the halo from the edge of the top of the via Wb is the halo distance from the edge of the bottom of the via.
Claims
1. A resin composition, in, contain: (A) Epoxy resin, (B) Active ester curing agent, (C) Inorganic filler materials, and (D) A silane compound having a silicon atom as a ring-constituting atom.
2. The resin composition according to claim 1, in, The component (C) includes any one of (C-1) a hollow inorganic filler and (C-2) a solid inorganic filler.
3. The resin composition according to claim 1, in, The component (C) contains (C-1) a hollow inorganic filler.
4. The resin composition according to claim 1, in, The component (C) is surface-treated with the component (D).
5. The resin composition according to claim 1, in, When the nonvolatile matter in the resin composition is 100% by mass, the content of the component (C) is 50% by mass or more.
6. The resin composition according to claim 1, in, When the resin component in the resin composition is 100 mass %, content of the component (D) is 0.1 mass % or more and 5 mass % or less.
7. An adhesive film, in, Include: Support body, and A resin composition layer provided on the support and comprising the resin composition according to any one of claims 1 to 6.
8. A printed wiring board, in, An insulating layer comprising a cured product of the resin composition according to any one of claims 1 to 6.
9. A semiconductor device, in, A printed wiring board comprising the method according to claim 8.