Flame-retardant reactive nylon composite material with low candlewick effect and preparation method thereof

By aminating and flame retardant modification of glass fibers and using DOPO-PH flame retardant, the problem of difficult to take into account both the flame retardant properties and mechanical properties caused by the 'candle wick effect' in nylon composite materials is achieved, and the low candlesticks are achieved The preparation of the flame retardant reaction nylon composite material of core effect reduces the amount of flame retardant and improves production efficiency.

CN118994895APending Publication Date: 2024-11-22CHONGQING COPOLYFORCE NEW MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411372694.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In application, nylon composites are difficult to take into account flame retardant performance, production efficiency and mechanical properties due to the ‘wick effect’. The prior art requires increasing the flame retardant dose to improve flame retardancy, but this increases the cost of the material and affects the mechanical properties.

Method used

By aminating and flame retardant modification of glass fibers, DOPO-PH is used as flame retardant to form a carbon layer with high thermal stability, reducing the amount of flame retardant and optimizing the preparation process, reducing the 'wick effect', and improving Production efficiency of flame retardant composite materials.

Benefits of technology

Effectively suppress the 'wick effect', reduce the amount of flame retardant, maintain the mechanical properties of composite materials, improve production efficiency, and achieve both flame retardant and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994895A_ABST
    Figure CN118994895A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of composite material modification, and discloses a flame-retardant reaction nylon composite material with low candlewick effect and a preparation method thereof, the flame-retardant reaction nylon composite material comprises 7.5-8 parts of flame-retardant modified glass fiber and 2-2.5 parts of resin component; the flame-retardant modified glass fiber is obtained by sequentially carrying out amination modification and flame-retardant modification on glass fiber; the resin component comprises 89-96 parts of caprolactam, 0-7 parts of a flame retardant, 2 parts of an initiator and 2 parts of an activator. The preparation method comprises the following steps: 1, treating the glass fibers: carrying out amination modification and flame-retardant modification on the glass fibers to obtain flame-retardant modified glass fibers; step 2, glue injection: mixing the flame-retardant modified glass fiber and a resin component according to a mass ratio of (7.5-8): (2-2.5), wherein the resin component comprises 89-96 parts of caprolactam, 0-7 parts of a flame retardant, 2 parts of an initiator and 2 parts of an activator; and 3, forming, wherein curing forming is conducted through a forming mold. The flame retardance, the production efficiency and the mechanical property of the material can be considered.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite material modification, and in particular to a flame-retardant reactive nylon composite material with low candle wick effect and a preparation method thereof. Background Art

[0002] As a thermoplastic, nylon has good mechanical properties, wear resistance, chemical resistance and low water absorption. By adding different reinforcing materials (such as glass fiber, carbon fiber, etc.), nylon composites can further improve their performance and make them suitable for more demanding working environments. Nylon composites have the advantages of high strength, wear resistance, chemical resistance and light weight, making them widely used in the automotive, aerospace, electrical and electronic and construction industries.

[0003] However, in practical applications, nylon composites also face some challenges. Especially in composite materials, if the distribution of fibers or particles is uneven, or there are differences in the physical properties of the material such as the thermal expansion coefficient and thermal conductivity coefficient, the internal temperature field and heat flow field will show uneven distribution. This unevenness will cause a "candle wick"-shaped channel to form along the axis of the fiber or particle during the process of heat transfer from the high-temperature area to the low-temperature area, which is called the "candle wick effect". The "candle wick effect" will accelerate the transfer of heat, causing the local temperature of the material to rise, increasing the fire hazard of the material.

[0004] In order to meet the flame retardant requirements of nylon composite materials, the commonly used solution is to add flame retardants to the resin during molding. However, due to the existence of the "wick effect", the amount of flame retardant added must be increased to achieve the flame retardancy of the composite material. This not only increases the cost of the material, but also has a significant impact on the mechanical properties, life and production efficiency of the composite material. Summary of the invention

[0005] The present invention aims to provide a flame-retardant reactive nylon composite material with low candle wick effect and a preparation method thereof, so as to achieve a balance between flame retardant properties and mechanical properties of the nylon composite material.

[0006] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a flame-retardant reactive nylon composite material with low wick effect, which comprises, by weight, 7.5-8 parts of flame-retardant modified glass fiber and 2-2.5 parts of resin component; the flame-retardant modified glass fiber is obtained by sequentially subjecting the glass fiber to amino modification and flame-retardant modification; the resin component comprises caprolactam flame-retardant modified glass fiber is obtained by sequentially subjecting the glass fiber to amino modification and flame-retardant modification; the resin component comprises 89-96 parts of caprolactam, 0-7 parts of flame retardant, 2 parts of initiator and 2 parts of activator.

[0007] Preferably, as an improvement, when the glass fiber is modified by amino, the added amount of the amino coupling agent is 1wt%, and the amino coupling agent is at least one of 3-aminopropyltriethoxysilane (KH550), 3-aminopropyltrimethoxysilane (APS), N(2-aminoethyl)3-aminopropylmethoxysilane (AAPS), and N(2-aminoethyl)3-propylaminomethoxymethylsilane (AEAPS).

[0008] Preferably, as an improvement, the structural formula of the amino glass fiber obtained after the amino modification of the glass fiber is as follows:

[0009]

[0010] Preferably, as an improvement, when the glass fiber is flame-retardant modified, the flame retardant is DOPO-PH, and the amount of DOPO-PH added is 1%-10% of the mass of the amination-modified glass fiber.

[0011] Preferably, as an improvement, the structural formula of DOPO-PH is as follows:

[0012]

[0013] Preferably, as an improvement, the preparation method of DOPO-PH comprises the following steps:

[0014] S1, mixing 4-aminophenol, 4-hydroxybenzaldehyde and methanol, and stirring to obtain system I;

[0015] S2, adding methanol to system I and cooling in an ice-water bath to precipitate the product 2-[(phenylimino)methyl]phenol, filtering and separating the solid and washing with cold methanol;

[0016] S3, dissolving 2-[(phenylimino)methyl]phenol and DOPO in THF, heating and stirring the mixture to obtain System II;

[0017] S4. The white precipitate in system II was filtered and washed with cold THF, and then dried under vacuum to obtain white powder DOPO-PH.

[0018] Preferably, as an improvement, the structural formula of the flame retardant modified glass fiber obtained by flame retardant modification of the glass fiber is as follows:

[0019]

[0020] Preferably, as an improvement, a method for preparing a flame-retardant reactive nylon composite material with low wick effect comprises the following steps:

[0021] Step 1: treating the glass fiber: performing amino modification and flame retardant modification on the glass fiber to obtain flame retardant modified glass fiber;

[0022] Step 2, glue injection: inject the resin into the mold through a glue injection machine, and mix it with the flame retardant modified glass fiber. The two are mixed in a mass ratio of 7.5-8:2-2.5. The flame retardant modified glass fiber is obtained by sequentially performing amino modification and flame retardant modification on the glass fiber. The resin component includes 89-96 parts of caprolactam, 0-7 parts of flame retardant, 2 parts of initiator, and 2 parts of activator.

[0023] Step 3: Molding: Use a molding mold to perform curing and molding to obtain a flame-retardant reactive nylon composite material with low "wick effect".

[0024] Preferably, as an improvement, in step 2, the flame retardant is at least one of DDP, TCPP and TCEP; the initiator is sodium hydroxide, sodium bicarbonate or sodium methoxide; and the activator is toluene diisocyanate or hexamethylene diisocyanate.

[0025] The principle and advantage of this solution are: in actual application, in this technical solution, in view of the "wick effect" existing in the prior art when glass fiber is used in composite materials, which leads to the problem that the flame retardant performance, production efficiency and mechanical properties of the composite materials cannot be taken into account, the present invention modifies the surface of the glass fiber, performs amino modification on the glass fiber, and then performs flame retardant modification. In the flame retardant modification stage of the glass fiber, this technical solution applies the flame retardant DOPO-PH to the modification of the glass fiber for the first time. DOPO-PH can self-crosslink to form carbon at a relatively low temperature and pyrolyze small molecules with polymer materials at high temperature to crosslink to form a carbon layer with high thermal stability, so that the glass fiber material modified by this technical solution has a good "wick effect" suppression effect, and can further reduce the amount of flame retardant used in the material and maintain the mechanical properties of the composite material, improve the production efficiency of the flame retardant composite material, and achieve a balance of the three, which has outstanding economic effects and important significance in the industry.

[0026] Moreover, when the flame-retardant modified glass fiber is applied to the preparation of reaction nylon composite materials, the technical scheme comprehensively and systematically optimizes the formula and preparation process of the flame-retardant modified reaction nylon composite materials. First, flame-retardant fiber is used in the composition of raw materials to reduce the amount of flame retardant added to the resin, thereby reducing the influence of the flame retardant on the reaction molding of the resin; in the optimization of the preparation process, the pultrusion speed of the flame-retardant composite material is increased, thereby improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a physical picture of the composite material of Example 1 of the present invention.

[0028] Figure 2It is a structural schematic diagram of a flame retardant reactive nylon composite material processing system with low wick effect in an embodiment of the present invention. DETAILED DESCRIPTION

[0029] The following is further described in detail through specific implementations, but the implementation of the present invention is not limited thereto. Unless otherwise specified, the technical means used in the following implementations are conventional means well known to those skilled in the art; the experimental methods used are all conventional methods; the materials, reagents, etc. used can all be obtained from commercial channels.

[0030] The figure marks in the drawings of the specification include: yarn frame 1, yarn ball 2, first tensioning wheel 3, first yarn dividing plate 4, amino modification pool 5, second yarn dividing plate 6, first reflux tank 7, first oven 8, second tensioning wheel 9, third yarn dividing plate 10, DOPO-PH pool 11, fourth yarn dividing plate 12, second reflux tank 13, second oven 14, third tensioning wheel 15, reaction nylon pool 16, dipping rod 17, fifth yarn dividing plate 18, third reflux tank 19, molding mold 20, mold heating device 21, first traction device 22, second traction device 23, cutting machine 24.

[0031] Program Overview:

[0032] A flame-retardant reactive nylon composite material with low wick effect comprises, by weight, 7.5-8 parts of flame-retardant modified glass fiber and 2-2.5 parts of resin component; the flame-retardant modified glass fiber is glass fiber that is sequentially subjected to amino modification and flame-retardant modification; the flame-retardant modified glass fiber is glass fiber that is sequentially subjected to amino modification and flame-retardant modification; the resin component comprises 89-96 parts of caprolactam, 0-7 parts of flame retardant, 2 parts of initiator and 2 parts of activator.

[0033] The flame retardant is a phosphate flame retardant selected from DDP, TCPP and TCEP, or a mixture of 2 to 3 phosphate flame retardants;

[0034] The initiator is sodium hydroxide, sodium bicarbonate or sodium methoxide;

[0035] The activator is toluene diisocyanate or hexamethylene diisocyanate.

[0036] A method for preparing a flame-retardant reactive nylon composite material with low candle wick effect comprises the following steps:

[0037] Step 1: Processing of glass fiber:

[0038] S1. Amino modification of glass fiber: 100 g of GF (glass fiber) was dispersed in ethanol / water (500 ml, the mass ratio of ethanol to water was 450:50), and 1 wt% of an amino coupling agent (at least one of 3-aminopropyltriethoxysilane (KH550), 3-aminopropyltrimethoxysilane (APS), N(2-aminoethyl)3-aminopropylmethoxysilane (AAPS), and N(2-aminoethyl)3-propylaminomethoxymethylsilane (AEAPS)) was added under high-speed stirring, and the reaction temperature was raised from room temperature to 60-100° C. for 1-2 min. After the reaction was completed, the amino glass fiber GF-NH was obtained by filtering, washing, and drying at 80° C. 2, Its structural formula is as shown in formula (I).

[0039]

[0040] S2. Preparation of DOPO-PH: 4-aminophenol (10.9 g, 0.1 mole), 4-hydroxybenzaldehyde (12.2 g, 0.1 mole) and methanol were placed in a three-necked round-bottom flask equipped with a magnetic stirrer. The resulting mixture was stirred at 50°C for 5 h under a nitrogen atmosphere. The product 2-[(phenylimino)methyl]phenol was precipitated by adding methanol (200 ml) and cooling the resulting solution with an ice-water bath, and then the solid was separated by filtration and washed with cold methanol. Then, 2-[(phenylimino)methyl]phenol (10 g, 0.05 mole) and DOPO (21.6 g, 0.1 mole) were dissolved in THF (100 ml) at room temperature under a nitrogen atmosphere. The mixture was heated to 60°C and stirred for 12 h. The resulting white precipitate was filtered and washed several times with cold THF, and then dried under vacuum. The white powder was marked as DOPO-PH, and the structural formula of DOPO-PH is as shown in Formula (II).

[0041]

[0042] S3. Synthesis of GF@DOPO-PH: GF-NH2 (100 g) was evenly dispersed in ethanol (500 ml, the mass ratio of ethanol to water was 450:50), and the DOPO-PH prepared in step 2 was dissolved in 100 ml of ethanol and slowly dripped into the above solution, wherein the amount of DOPO-PH added was DOPO-PH / GF-NH2 = 1%-10% (mass ratio). After the addition was completed, the reaction was continued for 1-10 minutes. After the reaction was completed, it was filtered, washed, and dried at 80°C to obtain the flame retardant modified glass fiber GF@DOPO-PH, with a structural formula as shown in formula (III).

[0043]

[0044] Step 2: Injecting glue: injecting the resin into the mold through a glue injection machine and mixing it with the flame retardant modified glass fiber in a mass ratio of 7.5-8:2-2.5;

[0045] The resin component includes caprolactam flame-retardant modified glass fiber, which is obtained by sequentially performing amino modification and flame-retardant modification on glass fiber; the resin component includes 89-96 parts of caprolactam, 0-7 parts of flame retardant, 2 parts of initiator and 2 parts of activator.

[0046] The caprolactam is divided into a caprolactam group A and a caprolactam group B; an initiator is added to the caprolactam group A, and the mixture is mixed evenly at 110-130° C. to obtain a mixture A; an activator is added to the caprolactam group B, and the mixture is mixed evenly at 110-130° C. to obtain a mixture B;

[0047] S2: adding a flame retardant to the mixture A, and mixing them uniformly at 110-130° C. to obtain a mixture A′;

[0048] S3: mixing mixture A' and mixture B to obtain a reaction mixture;

[0049] S4: preheating the glass fiber to 100-150° C., and then pulling the glass fiber into an impregnation mold; injecting the reaction mixture into the impregnation mold, maintaining the temperature in the impregnation mold at 170-190° C., reacting for 1-4 minutes, and obtaining a rough profile;

[0050] S5: pulling the rough profile into a forming mold, maintaining the temperature in the forming mold at 150-170° C. for 1-4 minutes, and obtaining a profile.

[0051] In this embodiment, the flame retardant reactive nylon composite material with low wick effect is manufactured by using a flame retardant reactive nylon composite material processing system with low wick effect, such as Figure 2 As shown: The system includes a glass fiber amination modification unit, a DOPO-PH treatment unit, a pultrusion unit and a cutting unit.

[0052] The glass fiber amination modification unit is used for amination modification of glass fiber, and includes a first tension wheel 3, a first yarn separation plate 4, an amination modification pool 5, a second yarn separation plate 6, a first reflux tank 7 and a first oven 8 arranged in sequence, and an amination modification solution (amino coupling agent KH550) is contained in the amination modification pool 5. A yarn rack 1 is fixed to the feed end of the amination modification unit, and a plurality of yarn balls 2 are placed on the yarn rack 1, so that multiple yarn balls 2 can be processed simultaneously, and the system operation efficiency can be ensured.

[0053] The DOPO-PH treatment unit comprises a second tension wheel 9, a third yarn separation plate 10, a DOPO-PH tank 11, a fourth yarn separation plate 12, a second reflux tank 13 and a second oven 14 which are arranged in sequence. The DOPO-PH tank 11 contains a DOPO-PH mixed solution.

[0054] The pultrusion unit includes a third tension wheel 15, a reaction nylon pool 16, a dipping rod 17, a fifth yarn dividing plate 18, a third reflow groove 19 and a forming mold 20, which are arranged in sequence. A first traction device 22 is arranged at the discharge end of the forming mold 20, and a mold heating device 21 for heating the forming mold 20 is arranged between the first traction device 22 and the forming mold 20. A second traction device 23 is arranged on the right side of the first traction device 22, and a cutting unit is arranged on the right side of the second traction device 23. A plurality of dipping rods 17 are arranged, and the plurality of dipping rods 17 are arranged in the reaction nylon pool 16 for full contact between the glass fiber and the nylon.

[0055] The cutting unit is a cutter 24 .

[0056] When the above processing system is used to process the reactive nylon composite material with the main effect of the base, first, the amination modification solution and the DOPO-PH mixed solution are respectively fed into the amination modification pool 5 and the DOPO-PH pool 11. Then, the glass fibers fixed on the creel 1 pass through the first tension wheel 3 and the first yarn dividing plate 4 and are immersed in the amination modification solution for amination modification, and then dried in the first oven 8.

[0057] The dried glass fiber is further pulled, flame-retardant modified by the DOPO-PH mixed solution and further dried by the second oven 14. The flame-retardant modified glass fiber is mixed with the resin material in the reaction nylon pool 16 to form a mixed system, which enters the molding die 20 and is heated and cured by the mold heating device 21 to obtain a low "wick effect" flame-retardant composite material profile. The low "wick effect" flame-retardant composite material profile enters the cutting unit under the traction of the first and second traction devices 23 and is cut to a fixed length by the cutting machine 24.

[0058] Example 1

[0059] A flame retardant reactive nylon composite material with low wick effect, comprising, by weight, 8 parts of flame retardant modified glass fiber and 2 parts of resin component; the flame retardant modified glass fiber is obtained by sequentially undergoing amino modification and flame retardant modification; the resin component comprises 96 parts of caprolactam, 0 parts of flame retardant, 2 parts of initiator, and 2 parts of activator. After testing, the flame retardant reactive nylon composite material meets the standard of flame retardant grade V1.

[0060] The flame retardant is one phosphate flame retardant selected from DDP, TCPP and TCEP or a mixture of 2-3 phosphate flame retardants;

[0061] The initiator is sodium hydroxide, sodium bicarbonate or sodium methoxide;

[0062] The activator is toluene diisocyanate or hexamethylene diisocyanate.

[0063] A method for preparing a flame-retardant reactive nylon composite material with low candle wick effect comprises the following steps:

[0064] Step 1: Processing of glass fiber:

[0065] S1. Amination modification of glass fiber: 100 g of GF (glass fiber) was dispersed in ethanol / water (500 ml, the mass ratio of ethanol to water was 450:50), and 1 wt% of amino coupling agent (3-aminopropyltriethoxysilane (KH550)) was added under high-speed stirring, and the reaction temperature was raised from room temperature to 60-100° C. for 1-2 min. After the reaction was completed, the amino glass fiber GF-NH was obtained by filtering, washing, and drying at 80° C. 2, Its structural formula is as shown in formula (I).

[0066]

[0067] S2. Preparation of DOPO-PH: 4-aminophenol (10.9 g, 0.1 mole), 4-hydroxybenzaldehyde (12.2 g, 0.1 mole) and methanol were placed in a three-necked round-bottom flask equipped with a magnetic stirrer. The resulting mixture was stirred at 50°C for 5 h under a nitrogen atmosphere. The product 2-[(phenylimino)methyl]phenol was precipitated by adding methanol (200 ml) and cooling the resulting solution with an ice-water bath, and then the solid was separated by filtration and washed with cold methanol. Then, 2-[(phenylimino)methyl]phenol (10 g, 0.05 mole) and DOPO (21.6 g, 0.1 mole) were dissolved in THF (100 ml) at room temperature under a nitrogen atmosphere. The mixture was heated to 60°C and stirred for 12 h. The resulting white precipitate was filtered and washed several times with cold THF, and then dried under vacuum. The white powder was marked as DOPO-PH, and the structural formula of DOPO-PH is as shown in Formula (II).

[0068]

[0069] S3. Synthesis of GF@DOPO-PH: GF-NH2 (100 g) was evenly dispersed in ethanol (500 ml, the mass ratio of ethanol to water was 450:50), and salicylaldehyde or 2,4-dihydroxybenzaldehyde was added; then a diamine (ethylenediamine or m-phenylenediamine) of equal molar mass to salicylaldehyde or 2,4-dihydroxybenzaldehyde was dissolved in 100 ml of ethanol and slowly dripped into the above solution. After the dripping was completed, the reaction was continued for 1-10 minutes. After the reaction was completed, it was filtered, washed, and dried at 80°C to obtain a flame-retardant modified glass fiber with a structural formula as shown in Formula (III).

[0070]

[0071] Step 2: Injecting the resin into the mold through a glue injection machine and mixing it with the flame retardant modified glass fiber in a mass ratio of 8:2.

[0072] The resin component includes 96 parts of caprolactam, 0 parts of flame retardant, 2 parts of initiator and 2 parts of activator.

[0073] The caprolactam is divided into a caprolactam group A and a caprolactam group B; an initiator is added to the caprolactam group A, and the mixture is mixed evenly at 110-130° C. to obtain a mixture A; an activator is added to the caprolactam group B, and the mixture is mixed evenly at 110-130° C. to obtain a mixture B;

[0074] S2: adding a flame retardant to the mixture A, and mixing them uniformly at 110-130° C. to obtain a mixture A′;

[0075] S3: mixing mixture A' and mixture B to obtain a reaction mixture;

[0076] S4: preheating the glass fiber to 100-150° C., and then pulling the glass fiber into an impregnation mold; injecting the reaction mixture into the impregnation mold, maintaining the temperature in the impregnation mold at 170-190° C., reacting for 1-4 minutes, and obtaining a rough profile;

[0077] S5: pulling the rough profile into a forming mold, maintaining the temperature in the forming mold at 150-170° C. for 1-4 minutes, and obtaining a profile.

[0078] Example 2

[0079] The difference between this embodiment and embodiment 1 is that: in this embodiment, a flame-retardant reactive nylon composite material with low wick effect comprises, by mass, 8 parts of flame-retardant modified glass fiber and 2 parts of resin component; the flame-retardant modified glass fiber is obtained by amino modification and flame-retardant modification in sequence; the resin component comprises 92 parts of caprolactam, 4 parts of flame retardant, 2 parts of initiator and 2 parts of activator. After testing, the flame-retardant reactive nylon composite material meets the standard of flame retardant grade V0.

[0080] Example 3

[0081] The difference between this embodiment and embodiment 1 is that: in this embodiment, a flame-retardant reactive nylon composite material with low wick effect includes, by weight, 8 parts of flame-retardant modified glass fiber and 2 parts of resin component; the flame-retardant modified glass fiber is obtained by amino modification and flame-retardant modification in sequence; the resin component includes 89 parts of caprolactam, 7 parts of flame retardant, 2 parts of initiator, and 2 parts of activator. After testing, the flame-retardant reactive nylon composite material meets the MT113 standard.

[0082] Comparative Example 1

[0083] The difference between this comparative example and Example 1 is that in this comparative example, the amount of the flame retardant is 3%.

[0084] Comparative Example 2

[0085] The difference between this comparative example and Example 1 is that in this comparative example, the flame-retardant modified glass fiber is replaced by ordinary glass fiber that has not been modified.

[0086] Comparative Example 3

[0087] The difference between this comparative example and Example 1 is that in this comparative example, only the glass fiber is subjected to amino modification, and no flame retardant modification is performed.

[0088] Comparative Example 4

[0089] The difference between this comparative example and Example 1 is that in this comparative example, only the glass fiber is flame-retardantly modified, and no amino modification is performed.

[0090] Comparative Example 5

[0091] The difference between this comparative example and Example 1 is that in this comparative example, the glass fiber is treated with a conventional flame retardant BDP when undergoing flame retardant modification.

[0092] Comparative Example 6

[0093] The difference between this comparative example and Example 1 is that in this comparative example, when the glass fiber is subjected to amino modification, the coupling agent used is isopropyl tri(dioctyl pyrophosphate) titanate.

[0094] Comparative Example 7

[0095] The difference between this comparative example and Example 1 is that in this comparative example, the flame-retardant modified glass fiber is replaced by ordinary glass fiber that has not been modified, and the amount of the flame retardant is 35%.

[0096] Comparative Example 8

[0097] The difference between this comparative example and Example 1 is that in this comparative example, the flame-retardant modified glass fiber is replaced by ordinary glass fiber without modification, the amount of flame retardant is 35%, and the pultrusion speed is 0.1 m / min.

[0098] Experimental Example 1 Mechanical Properties Test

[0099] The flame retardant modified polyurethane composite materials prepared in the above embodiments and comparative examples were subjected to mechanical property tests, wherein the mechanical property test method was based on GB / T 3354. The results are shown in Table 1.

[0100] Experimental Example 2 Flame retardant performance test

[0101] The flame retardant modified polyurethane composite materials prepared in the above embodiments and comparative examples were subjected to flame retardant performance tests, wherein: the flame retardant performance test method refers to GB / T 2408-2008, ASTM D2863 and MT113; each group was subjected to three repeated experiments, and the results are shown in Table 1:

[0102] The results show that the use of modified glass fiber can effectively reduce the amount of flame retardant used in composite materials, improve production efficiency, and take into account both the mechanical properties and flame retardant properties of composite materials. Figure 1 Shown is a physical picture of the composite material prepared in Example 1 of the present invention.

[0103] Table 1

[0104]

[0105] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A flame retardant reactive nylon composite material with low candle wick effect, Features: Calculated by mass, it includes 7.5-8 parts of flame retardant modified glass fiber and 2-2.5 parts of resin component; the flame retardant modified glass fiber is obtained by sequentially subjecting the glass fiber to amino modification and flame retardant modification; the flame retardant modified glass fiber is obtained by sequentially subjecting the glass fiber to amino modification and flame retardant modification; the resin component includes 89-96 parts of caprolactam, 0-7 parts of flame retardant, 2 parts of initiator and 2 parts of activator.

2. A flame retardant reactive nylon composite material with low wick effect according to claim 1, Features: When the glass fiber is modified by amino modification, the added amount of the amino coupling agent is 1wt%, and the amino coupling agent is at least one of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N(2-aminoethyl)3-aminopropylmethoxysilane, and N(2-aminoethyl)3-propylaminomethoxymethylsilane.

3. A flame retardant reactive nylon composite material with low wick effect according to claim 2, Features: The structural formula of the amino glass fiber obtained after the amino modification of the glass fiber is as shown in formula (I):

4. A flame retardant reactive nylon composite material with low wick effect according to claim 3, Features: When the glass fiber is flame-retardant modified, the flame retardant is DOPO-PH, and the added amount of DOPO-PH is 1%-10% of the mass of the amino-modified glass fiber.

5. A flame retardant reactive nylon composite material with low wick effect according to claim 4, Features: The structural formula of the DOPO-PH is as follows:

6. A flame retardant reactive nylon composite material with low wick effect according to claim 5, Features: The preparation method of DOPO-PH comprises the following steps: S1, mixing 4-aminophenol, 4-hydroxybenzaldehyde and methanol, and stirring to obtain system I; S2, adding methanol to system I and cooling in an ice-water bath to precipitate the product 2-[(phenylimino)methyl]phenol, filtering and separating the solid and washing with cold methanol; S3, dissolving 2-[(phenylimino)methyl]phenol and DOPO in THF, heating and stirring the mixture to obtain System II; S4. The white precipitate in system II was filtered and washed with cold THF, and then dried under vacuum to obtain white powder DOPO-PH.

7. A flame retardant reactive nylon composite material with low wick effect according to claim 6, Features: The structural formula of the flame retardant modified glass fiber obtained by flame retardant modification of glass fiber is as follows:

8. A method for preparing a flame-retardant reactive nylon composite material with low wick effect according to any one of claims 1 to 7, It is characterized in that The steps include: Step 1: treating the glass fiber: performing amino modification and flame retardant modification on the glass fiber to obtain flame retardant modified glass fiber; Step 2, glue injection: inject the resin into the mold through a glue injection machine, and mix it with the flame retardant modified glass fiber. The two are mixed in a mass ratio of 7.5-8:2-2.

5. The flame retardant modified glass fiber is obtained by sequentially performing amino modification and flame retardant modification on the glass fiber. The resin component includes 89-96 parts of caprolactam, 0-7 parts of flame retardant, 2 parts of initiator, and 2 parts of activator. Step 3: Molding: Use a molding mold to perform curing and molding to obtain a flame-retardant reactive nylon composite material with low "wick effect".

9. The method for preparing a flame-retardant reactive nylon composite material with low wick effect according to claim 8, Features: In step 2, the flame retardant is at least one of DDP, TCPP and TCEP; the initiator is sodium hydroxide, sodium bicarbonate or sodium methoxide; and the activator is toluene diisocyanate or hexamethylene diisocyanate.