Fluororubber formula for coating and fluororubber adhesive tape
By doping EPDM rubber and nano-sized molybdenum disulfide into fluororubber, the problems of molecular chain breakage and porosity caused by excessive cohesive energy during the high-temperature vulcanization of fluororubber have been solved, resulting in the production of thin and dense protective rubber sheets that significantly improve the protective effect against toxic chemicals.
Patent Information
- Application Number
- CN202411226847.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
AI Technical Summary
During the high-temperature vulcanization process, excessive cohesive energy in fluororubber can cause molecular chain breakage, resulting in cracks or delamination. Additionally, the volatilization of plasticizers creates pores, reducing protective performance and making it unable to effectively block toxic chemicals.
The material is made of highly elastic EPDM rubber and nano-sized molybdenum disulfide and fluororubber. The cohesive energy is reduced by coating and embedding, and the voids and pores in the vulcanization process are filled to maintain the density of the protective layer.
The production of thin, dense fluororubber cloth significantly improves the protection against non-polar toxic chemicals, solves defects such as cracks, pinholes and bubbles, and enhances protective performance.
Smart Images

Figure CN118994975A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of anti-toxic materials, and in particular to a fluororubber formula and a fluororubber adhesive tape for coating. Background Art
[0002] Fluororubber has become the preferred material for protective clothing, protective gloves and other protective products due to its strong resistance to penetration and flame retardancy to non-polar toxic chemicals. For example, the fabrics of high-end airtight protective clothing in the United States, France and other countries currently on the market all achieve broad-spectrum protection against toxic chemicals of different properties through the lamination of rubbers of different properties, among which fluororubber is an indispensable protective layer in the lamination composite fabrics.
[0003] The preparation methods of fluororubber tape include calendering and coating processes. The coating process is to coat the rubber paste made from the mixed rubber on the fabric, and then undergo a high-temperature vulcanization process to make a tape with protective function. The fabric in the tape provides the necessary mechanical strength for the protective product, and the rubber material provides it with protective function. The coated tape is light, thin and dense, and in particular, it can realize the lamination of heterogeneous rubbers, becoming an irreplaceable processing method for the production of high-end airtight protective fabrics.
[0004] During the high temperature vulcanization process of fluororubber, its great cohesive energy causes the free radicals broken in the previous processing process to recombine and restore to the initial molecular chain or produce partial aggregation, thereby producing a large shrinkage deformation (shrinkage force). Due to the restraint of the fabric, it cannot be in a free state, the molecular chain breaks, and cracks or delamination are formed ( Figure 1 For cracks, Figure 2 The adhesive tape has no protective capability and has no practical use value.
[0005] In order to solve the coagulation phenomenon of fluororubber itself, low molecular weight plasticizers are usually added to improve the fluidity of fluororubber. However, the pores formed by the volatilization of plasticizers under high temperature conditions are more conducive to the shrinkage of fluororubber, resulting in defects such as pinholes and bubbles. Figure 3 For the eye of the needle, Figure 4 The plasticizers remaining inside are similar to toxic chemicals and are easily miscible, which accelerates the penetration of toxic chemicals and is extremely detrimental to the protective performance of fluororubber. After testing, its protection against toluene and xylene is only a few minutes. Summary of the invention
[0006] The invention provides a fluororubber formula for coating in order to solve the technical problems of coagulation phenomenon and poor protective performance of fluororubber itself.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a fluororubber formula for coating, comprising the following raw materials in weight proportions: 100 parts of fluororubber; 5-20 parts of EPDM; 0.1-0.5 parts of sulfur; 0.4-2.0 parts of zinc oxide; 0.1-0.5 parts of accelerator TT; 0.4-2.0 parts of accelerator M; 0.5-1.0 parts of accelerator BPP; 2-7 parts of magnesium oxide; 1-5 parts of bisphenol AF; 5-10 parts of calcium hydroxide and 4-10 parts of molybdenum disulfide.
[0008] The present invention modifies fluororubber by doping EPDM rubber with high elasticity and large effective volume, and the fluororubber is present in the molecular interface or between molecules of the fluororubber in a wrapped and embedded manner, thereby reducing the cohesive energy of the fluororubber. At the same time, nano-scale molybdenum disulfide with excellent lubricity is added to compensate for the loss of the protective ability of the fluororubber against non-polar toxic chemicals due to the large difference in physical properties between the EPDM rubber and the fluororubber, and the holes and pores formed by the vulcanization of the solvent are filled in time to ensure the density of the protective layer.
[0009] The present invention also provides a method for preparing a fluororubber adhesive tape, using the fluororubber formula as described above, comprising the following steps: A. Weighing: weigh all raw materials according to the proportion; B. Mixing: B1, add fluororubber, plasticize, roller distance 0.5mm, B2, add EPDM rubber, plasticize, roller distance 0.6mm, B3, fluororubber and EPDM are mixed evenly, the roller distance is 1mm, B4, add magnesium oxide, zinc oxide, calcium hydroxide and molybdenum disulfide for mixing, the roller distance is 1.5mm, B5. Add sulfur, accelerator TT, accelerator DM, accelerator BPP, and bisphenol AF and mix evenly. Roller distance 2mm. B6, thin pass, roller distance 1.0mm, B7, film output; C. Preparation of mixed glue mortar: Mix the mixed glue obtained in step B7 with the polar solvent ethyl acetate-gasoline mixed solution in a stirring tank; D. Preparation of adhesive tape: D1. First, let the polyester-cotton cloth run in the glue coating machine for one circle. The glue coating temperature is between 40℃ and 60℃. D2. Apply the mixed glue paste on the polyester-cotton cloth by scraping. The amount of mixed glue dry glue on each layer is controlled according to the protection requirements of the product. D3. After gluing, evenly apply a layer of release agent talcum powder on the surface of the tape; E. Vulcanization of adhesive tape: The adhesive tape obtained in step D3 is vulcanized in an electrically heated vulcanizing tank to complete the preparation.
[0010] As a further limitation of the technical solution of the present invention, the stirring time in step C is 4h-6h.
[0011] As a further limitation of the technical solution of the present invention, the vulcanization parameters in step E are temperature 130° C., vulcanization time 1.5 h, and pressure 0.4 MPa.
[0012] In addition, the present invention also provides the use of the above fluororubber formula in the preparation of protective clothing and protective gloves.
[0013] Compared with the prior art, the present invention has the following beneficial effects: The present invention selects EPDM rubber with high elasticity and large effective volume as a plasticizer to replace the low molecular plasticizer used in the traditional production process, and increases the spatial distance between fluororubber molecules in a coating and embedding manner, reduces the cohesive energy of fluororubber, effectively blocks the shrinkage and aggregation of fluororubber itself, and maintains the excellent protective ability of fluororubber itself.
[0014] The invention adds nano-scale molybdenum disulfide with excellent lubricity in the formula design to compensate for the loss of the protective ability of fluororubber against non-polar toxic chemicals due to the large difference in physical properties between EPDM rubber and fluororubber, and at the same time timely fills the holes and pores formed by solvent volatilization during the vulcanization process to ensure the compactness of the protective layer. The protective ability of fluororubber tape against toxic chemicals is ensured through the synergistic effect of the two. The problem of cracks, pinholes, extremely poor protective ability and lack of practical use value in fluororubber coated tape is solved.
[0015] The fluororubber tape produced by the present invention is thin, dense and has strong protective capability, and the fluororubber formula can be applied to products such as protective clothing and protective gloves. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a picture of cracks in existing fluororubber tape.
[0017] Figure 2 Image of delamination produced for existing fluoro rubber tape.
[0018] Figure 3 Image of pinholes produced for existing Viton tape.
[0019] Figure 4 Picture of bubbles generated in existing fluororubber tape.
[0020] Figure 5 This is a picture of the fluororubber tape prepared according to the present invention. DETAILED DESCRIPTION
[0021] The present invention is further described below in conjunction with specific embodiments.
[0022] A fluororubber formula for coating comprises the following raw materials in proportion by weight: 100 parts of fluororubber; 5-20 parts of EPDM; 0.1-0.5 parts of sulfur; 0.4-2.0 parts of zinc oxide; 0.1-0.5 parts of accelerator TT; 0.4-2.0 parts of accelerator M; 0.5-1.0 parts of accelerator BPP; 2-7 parts of magnesium oxide; 1-5 parts of bisphenol AF; 5-10 parts of calcium hydroxide and 4-10 parts of molybdenum disulfide.
[0023] The present invention provides a fluororubber formula for coating technology, which reduces the cohesive energy of fluororubber by doping EPDM rubber and nanomaterials with excellent slip properties, and maintains the excellent protective ability of fluororubber. The fluororubber tape produced by the invention has a smooth surface, no defects such as cracks and bubbles, and a dense protective layer with strong protective ability.
[0024] The fluororubber formulations of Examples 1-3 are shown in Table 1.
[0025] Example 1-3 Fluororubber formulation
[0026] The fluororubber formulations of the above-mentioned embodiments 1-3 are used to prepare adhesive tapes, and the preparation method is as follows: A. Weighing: weigh all raw materials according to the proportion; B. Mixing: B1, add fluororubber, plasticize, roller distance 0.5mm, B2, add EPDM rubber, plasticize, roller distance 0.6mm, B3, fluororubber and EPDM are mixed evenly, the roller distance is 1mm, B4, add magnesium oxide, zinc oxide, calcium hydroxide and molybdenum disulfide for mixing, the roller distance is 1.5mm, B5. Add sulfur, accelerator TT, accelerator DM, accelerator BPP, and bisphenol AF and mix evenly. Roller distance 2mm. B6, thin pass, roller distance 1.0mm, B7, film output; C. Preparation of mixed glue mortar: Mix the mixed glue obtained in step B7 with the polar solvent ethyl acetate-gasoline mixed solution in a stirring tank for 4-6 hours; wherein the volume ratio of ethyl acetate to gasoline is 1.5:3; and the mass ratio of the mixed glue to the ethyl acetate-gasoline mixed solution is 1:4.5; D. Preparation of adhesive tape: D1. First, let the polyester-cotton cloth run in the glue coating machine for one circle. The glue coating temperature is between 40℃ and 60℃. D2. Apply the mixed glue paste on the polyester-cotton cloth by scraping. The amount of mixed glue dry glue on each layer is controlled according to the protection requirements of the product. D3. After gluing, evenly apply a layer of release agent talcum powder on the surface of the tape; E. Vulcanization of adhesive tape: The adhesive tape obtained in step D3 is vulcanized in an electrically heated vulcanizing tank at a temperature of 130° C., a vulcanization time of 1.5 h, and a pressure of 0.4 MPa to complete the preparation.
[0027] The adhesive tapes prepared with the fluororubber formulations of Examples 1-3 above were tested, and the results are shown in Table 2.
[0028] Table 2 Test results of Examples 1-3 Example 4
[0029] A fluororubber formula for coating comprises the following raw materials in proportion by weight: 100 parts of fluororubber; 5 parts of EPDM; 0.5 parts of sulfur; 0.4 parts of zinc oxide; 0.5 parts of accelerator TT; 0.4 parts of accelerator M; 1.0 parts of accelerator BPP; 2 parts of magnesium oxide; 5 parts of bisphenol AF; 5 parts of calcium hydroxide and 10 parts of molybdenum disulfide. Example 5
[0030] A fluororubber formula for coating comprises the following raw materials in proportion by weight: 100 parts of fluororubber; 20 parts of EPDM; 0.1 parts of sulfur; 2.0 parts of zinc oxide; 0.1 parts of accelerator TT; 2.0 parts of accelerator M; 0.5 parts of accelerator BPP; 7 parts of magnesium oxide; 1 part of bisphenol AF; 10 parts of calcium hydroxide and 4 parts of molybdenum disulfide.
Claims
1. A fluororubber formulation for coating, It is characterized in that The invention comprises the following raw materials in proportions by weight: 100 parts of fluororubber; 5-20 parts of EPDM rubber; 0.1-0.5 parts of sulfur; 0.4-2.0 parts of zinc oxide; 0.1-0.5 parts of accelerator TT; 0.4-2.0 parts of accelerator M; 0.5-1.0 parts of accelerator BPP; 2-7 parts of magnesium oxide; 1-5 parts of bisphenol AF; 5-10 parts of calcium hydroxide and 4-10 parts of molybdenum disulfide.
2. A method for preparing a fluororubber tape, using the fluororubber formula as claimed in claim 1, It is characterized in that The following steps are involved: A. Weighing: weigh all raw materials according to the proportion; B. Mixing: B1, add fluororubber, plasticize, roller distance 0.5mm, B2, add EPDM rubber, plasticize, roller distance 0.6mm, B3, fluororubber and EPDM are mixed evenly, the roller distance is 1mm, B4, add magnesium oxide, zinc oxide, calcium hydroxide and molybdenum disulfide for mixing, the roller distance is 1.5mm, B5. Add sulfur, accelerator TT, accelerator DM, accelerator BPP, and bisphenol AF and mix evenly. Roller distance 2mm. B6, thin pass, roller distance 1.0mm, B7, film output; C. Preparation of mixed glue mortar: Mix the mixed glue obtained in step B7 with the polar solvent ethyl acetate-gasoline mixed solution in a stirring tank; D. Preparation of adhesive tape: D1 First, let the polyester-cotton cloth run in the glue coating machine for one circle, and the glue coating temperature is between 40℃ and 60℃. D2 uses scraping to apply the mixed glue paste on the polyester-cotton cloth. The amount of mixed glue dry glue in each layer is controlled according to the protection requirements of the product. D3 After the glue is applied, evenly apply a layer of release agent talcum powder on the surface of the tape; E. Vulcanization of adhesive tape: The adhesive tape obtained in step D3 is vulcanized in an electrically heated vulcanizing tank to complete the preparation.
3. A method for preparing a fluororubber tape according to claim 2, It is characterized in that The stirring time in step C is 4h-6h.
4. The method for preparing a fluororubber tape according to claim 2, It is characterized in that The vulcanization parameters in step E are temperature 130° C., vulcanization time 1.5 h, and pressure 0.4 MPa.
5. Use of the fluororubber formulation as claimed in claim 1 in the preparation of protective clothing and protective gloves.
Citation Information
Patent Citations
Coating on surface of cylinder ring and manufacturing method thereof
CN103694810A
Nano silver modified fluororubber composite material
CN105367957A
Adhesive tape material of multi-component blended rubber coated fabric
CN109401138A
Fuororubber-chlorinated butyl rubber composite rubberized fabric prepared by adopting two layers of cloth and three layers of rubber, and method
CN110776838A