Flame-retardant wave-absorbing patch and preparation method thereof
By using a multi-layer structure design and an intumescent flame retardant, the problem of non-recyclability of coated microwave absorbing materials after combustion has been solved, achieving simplified preparation and reduced costs for both flame retardant and microwave absorbing properties.
Patent Information
- Application Number
- CN202411062148.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
AI Technical Summary
Existing technologies struggle to prepare coating-type microwave absorbing materials that simultaneously possess flame-retardant and microwave-absorbing properties. The process is complex and costly, and the products are rendered unusable after combustion, making recycling impossible.
It adopts a multi-layer structure design consisting of a flame-retardant layer, a microwave-absorbing layer, a conductive layer, and a release layer. It utilizes an intumescent flame retardant to form a dense protective layer during combustion, and combines it with pressure-sensitive adhesive to achieve detachable bonding of each layer, thus enabling the material to be recycled.
This technology enables the peelable and recyclable flame-retardant layer of the material after combustion, reducing usage costs. It also possesses excellent microwave absorption and flame-retardant properties, simplifying the preparation process.
Smart Images

Figure CN118995068A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer material preparation, in particular to a flame retardant wave absorbing patch and a preparation method thereof. Background Art
[0002] With the rapid development of modern guidance and detection technologies, how to enhance the survivability and combat capability of aircraft has become the research focus of major military powers around the world. As a radar stealth technology, absorbing materials have developed rapidly in the fields of military equipment and defense systems; commonly used absorbing materials are mainly divided into structural and coated types. Among them, the preparation process of coated absorbing materials is relatively simple, the construction is convenient, and the requirements for the shape of the workpiece are relatively low, making it one of the key development targets of modern radar stealth technology. Among coated absorbing materials, absorbing patches have been widely used in radar stealth weapon systems due to their advantages such as good flexibility, prefabrication, adjustable thickness, and easy mounting and disassembly.
[0003] With the iteration and upgrade of military equipment, light-weight and high-strength fiber-reinforced composite materials have gradually replaced traditional metal materials. This type of fiber-reinforced composite material uses polymer materials such as epoxy resin, phenolic resin, polyethylene, and nylon as a matrix, which makes these materials easy to burn, and once ignited, the flame spreads rapidly, accompanied by the release of huge amounts of heat, smoke, and toxic gases, causing great casualties and property losses. Therefore, in the design and preparation of military equipment, it is usually necessary to add flame retardants to the materials, or apply a flame retardant layer to the surface of the equipment to reduce its fire risk.
[0004] Under the dual requirements of radar stealth performance and fire safety performance, the application of flame retardant and radar absorbing products is imminent. However, in order to prepare products that are both flame retardant and radar absorbing, it usually requires cumbersome process flow and higher manufacturing difficulty, and the product will be scrapped once it burns, further increasing its use cost. Therefore, it is urgent to develop a flame retardant and radar absorbing product with simple process and multiple uses. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a flame retardant absorbing patch and a preparation method thereof. The material preparation process is simple and can give the adhered material good absorbing and flame retardant properties. At the same time, the patch can be recycled after burning, reducing the use cost of the product.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] A flame retardant absorbing patch comprises a flame retardant layer, an absorbing layer, a conductive layer and a release layer, wherein the flame retardant layer is bonded to the surface of the absorbing layer through an adhesive layer, the bottom surface of the absorbing layer is bonded to the surface of the conductive layer through an adhesive layer, and the release layer is bonded to the bottom surface of the conductive layer through an adhesive layer.
[0008] Furthermore, the flame retardant layer is made of an intumescent flame retardant and a resin matrix.
[0009] Furthermore, the intumescent flame retardant includes a charring agent, a dehydrating agent and a foaming agent.
[0010] Furthermore, the carbon-forming agent is one or more of pentaerythritol, dipentaerythritol, sorbitol, starch, triazine carbon-forming agent, and polyimide carbon-forming agent.
[0011] Furthermore, the dehydrating agent is one or more of ammonium phosphate, ammonium polyphosphate, triphenyl phosphate, melamine phosphate, aluminum hypophosphite, and dimethyl methyl phosphate.
[0012] Furthermore, the foaming agent is one or more of melamine, dicyandiamide, chlorinated paraffin and urea.
[0013] Furthermore, the resin matrix is one of polyurethane, acrylate, and epoxy resin.
[0014] Furthermore, the adhesive layer is a pressure-sensitive adhesive.
[0015] Furthermore, the thickness of the adhesive layer is 1 to 100 μm.
[0016] A method for preparing a flame retardant wave absorbing patch comprises the following steps:
[0017] S1: preparing a flame retardant layer; wherein the method for preparing the flame retardant layer is specifically: adding a flame retardant to a resin matrix, stirring with a magnetic stirrer for 30 minutes, vacuum degassing for 10 minutes, then coating, and baking in an oven at 80° C. for 12 hours to obtain a flame retardant layer;
[0018] S2: preparing an absorbing layer and a conductive layer;
[0019] S3: Multi-layer assembly of the patch: Use adhesive layers to bond the flame retardant layer, the absorbing layer and the conductive layer together in sequence. Use a silicone roller to roll from the bonding end to the non-bonding end to make them fit. After they are fully bonded, roll them back and forth 4-6 times with a rolling force of 0.8-1.2kg / cm 2 ;
[0020] S4: bonding the release layer to the bottom surface of the conductive layer via an adhesive layer.
[0021] The present invention has the following advantages:
[0022] 1. When the material burns, a series of chemical reactions occur in the flame retardant layer, which promotes the dehydration, expansion and carbonization of the resin matrix, thereby forming a dense protective layer on the surface, isolating the transfer of heat and oxygen, making it difficult for the flame to spread to the absorbing layer and the conductive layer below. Since the structures such as the absorbing layer and the conductive layer are not destroyed by the flame, the flame retardant layer that has failed after burning is peeled off, and the original absorbing layer and the conductive layer and adhesive layer below can be re-pasted with a new flame retardant layer, thereby realizing the recycling of the absorbing layer and the conductive layer.
[0023] 2. The flame retardant and wave absorbing patch of the present invention sequentially bonds the flame retardant layer, the wave absorbing layer, the conductive layer and the release layer together through a pressure sensitive adhesive, and the process is simple. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a structural schematic diagram of the present invention;
[0025] In the figure: 1-flame retardant layer, 2-wave absorbing layer, 3-conductive layer, 4-release layer, 5-adhesive layer. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following description.
[0027] like Figure 1 As shown, a flame retardant absorbing patch comprises a flame retardant layer 1, an absorbing layer 2, a conductive layer 3 and a release layer 4, wherein the flame retardant layer 1 is bonded to the surface of the absorbing layer 2 through an adhesive layer 5, the bottom surface of the absorbing layer 2 is bonded to the surface of the conductive layer 3 through an adhesive layer 5, and the release layer 4 is bonded to the bottom surface of the conductive layer 3 through an adhesive layer 5.
[0028] In this embodiment, the flame retardant layer 1 is made of an intumescent flame retardant and a resin matrix. When the material burns, a series of chemical reactions occur in the flame retardant layer 1, which promotes the dehydration and expansion and carbonization of the resin matrix, thereby forming a dense protective layer on the surface, isolating the transfer of heat and oxygen, and making it difficult for the flame to spread to the absorbing layer 2 and the conductive layer 3 below. Since the structures such as the absorbing layer 2 and the conductive layer 3 are not destroyed by the flame, the flame retardant layer 1 that has failed after burning is peeled off, and the original absorbing layer 2 and the conductive layer 3 below and the adhesive layer 5 can be re-pasted with a new flame retardant layer 1, thereby realizing the recycling of the absorbing layer 2 and the conductive layer 3.
[0029] The intumescent flame retardant includes a carbonizing agent, a dehydrating agent and a foaming agent. The carbonizing agent is one or more of pentaerythritol, dipentaerythritol, sorbitol, starch, triazine carbonizing agent, and polyimide carbonizing agent. The dehydrating agent is one or more of ammonium phosphate, ammonium polyphosphate, triphenyl phosphate, melamine phosphate, aluminum hypophosphite, and dimethyl methyl phosphate. The foaming agent is one or more of melamine, dicyandiamide, chlorinated paraffin, and urea. The resin matrix is one of polyurethane, acrylate, and epoxy resin.
[0030] In this embodiment, the adhesive layer 5 is a pressure-sensitive adhesive, which has good self-adhesiveness and does not contaminate the adherend after peeling, facilitating correction after misapplication and replacement of each functional layer. The pressure-sensitive adhesive may include one or more of silicone pressure-sensitive adhesive, acrylic pressure-sensitive adhesive, and polyurethane pressure-sensitive adhesive. Preferably, the thickness of the adhesive layer 5 is 1 to 100 μm.
[0031] The wave absorbing layer 2 is used to absorb electromagnetic waves. It is mainly composed of magnetic medium type absorbent and resin, and has a thickness of 100 to 1000 μm. The absorbent is the key to achieving the radar stealth performance of the material. The magnetic medium type absorbent attenuates the electromagnetic waves through resonance and hysteresis loss, which can effectively reduce the reflection and propagation of electromagnetic waves. The magnetic medium type absorbent is a magnetic metal alloy particle with a particle size of 10 to 100 μm, which can include Fe3O4 powder, NiFe2O4 powder, BaFe 12 O 19 Powder, SeFe 12 O 19 The resin may include one or more of polyurethane, acrylate, and epoxy resin.
[0032] The conductive layer 3 is also called the electromagnetic shielding layer, which is used to reflect and absorb the residual electromagnetic waves that pass through the absorbing layer, and has a thickness of 10 to 500 μm. When the electromagnetic wave is incident on the surface of the conductive layer 3, it is reflected due to the impedance discontinuity, so that the electromagnetic wave returns to the absorbing layer 2 to be consumed and absorbed again; part of the electromagnetic wave enters the conductive layer 2, and is absorbed and lost by the conductive material during the propagation process and multiple interface reflections. The conductive layer 3 is made of conductive fiber cloth, which can include one of gold-plated conductive cloth, silver-plated conductive cloth, nickel-plated conductive cloth, nickel-plated copper conductive cloth, and silver / polyester blended conductive cloth.
[0033] A method for preparing a flame retardant wave absorbing patch comprises the following steps:
[0034] S1. Prepare flame retardant layer 1: prepare flame retardant according to the following weight parts: 3.4-5.2 parts of carbonizing agent, 5.0-6.3 parts of dehydrating agent, 4.3-5.0 parts of foaming agent, put each component in a clean mortar, grind for 10-15 minutes, mix them evenly, and obtain flame retardant; add the above flame retardant to 100 parts of resin matrix, stir for 30 minutes with magnetic stirrer, vacuum degas for 10 minutes, then apply, the feeler gauge height is 0.4-0.45mm, and then bake in an oven at 80℃ for 12 hours to obtain flame retardant layer;
[0035] S2, preparing the wave absorbing layer 2 and the conductive layer 3;
[0036] The wave absorbing layer 2 is composed of the following materials in parts by weight: 80 parts of resin, 200-300 parts of magnetic medium absorbent, 8-15 parts of deionized water, 0.4 parts of defoamer, 4 parts of crosslinking aid, 0.3 parts of orientation agent and 0-1.2 parts of thickener. The above materials are stirred for 30 minutes with a mechanical stirrer, then filtered and vacuum degassed for 10 minutes to obtain a slurry, which is placed on a coating machine with a feeler gauge height of 0.42-0.54 mm. After coating, it is placed in an oven at 80°C and baked for 12 hours to obtain the wave absorbing layer 2.
[0037] The conductive layer 3 is a commercially available material, and its preparation process is not described in detail in this application.
[0038] S3. Multi-layer assembly of the patch: Use adhesive layer 5 to bond flame retardant layer 1, wave absorbing layer 2 and conductive layer 3 together in sequence. Use silicone roller to roll from bonding end to non-bonding end to make them fit. After they are fully bonded, roll them back and forth 4-6 times with a rolling force of 0.8-1.2kg / cm 2 ;
[0039] S4 , bonding the release layer 4 to the bottom surface of the conductive layer 3 via the adhesive layer 5 .
[0040] The following examples further illustrate the preparation method of the flame retardant wave absorbing patch:
[0041] [Example 1]
[0042] A method for preparing a flame retardant wave absorbing patch comprises the following steps:
[0043] 1. Preparation of flame retardant layer
[0044] Weigh 3.4g of pentaerythritol, 6.3g of ammonium polyphosphate and 5.0g of melamine, put them in a clean mortar, grind for 10min to mix them evenly to obtain a flame retardant. Add the flame retardant to 100g of acrylic emulsion, and also add 0.1g of dispersant and 0.5g of defoamer, stir with a magnetic stirrer for 30min; vacuum degassing for 10min before coating (feeler gauge height 0.4mm), and then place in an oven at 80℃ for 12h to obtain a flame retardant layer with a thickness of 280μm.
[0045] 2. Preparation of absorbing layer
[0046] 80g polyurethane emulsion, 240g magnetic metal alloy particles, 10g deionized water, 0.4g defoamer, 4g crosslinking aid, 0.3g orientation agent, 1.2g thickener were mixed, stirred with a mechanical stirrer for 30min, then filtered and vacuum degassed for 10min. The slurry was placed on a coater with a feeler gauge height of 0.5mm; after coating, it was placed in an oven at 80℃ and baked for 12h to obtain a wave absorbing layer with a thickness of 350μm.
[0047] 3. Multi-layer assembly of patches
[0048] The prepared 280μm flame retardant layer, 350μm wave absorbing layer and 200μm silver-plated conductive fabric were bonded together using double-sided acrylic pressure-sensitive adhesive (30μm). During the bonding process, a silicone roller was used to roll from the bonding end to the non-bonding end to make them fit together. After they were fully bonded, they were rolled back and forth for 5 times with a rolling force of 0.8kg / cm 2 When a functional layer is damaged or has abnormal quality, it can be directly peeled off with the pressure-sensitive adhesive and replaced.
[0049] [Example 2]
[0050] A method for preparing a flame retardant wave absorbing patch comprises the following steps:
[0051] 1. Preparation of flame retardant layer
[0052] Weigh 5.2g of pentaerythritol, 5.6g of ammonium polyphosphate and 4.3g of melamine, put them in a clean mortar, grind for 15min to mix them evenly to obtain a flame retardant. Add the flame retardant to 100g of acrylic emulsion, and also add 0.1g of dispersant and 0.5g of defoamer, stir with a magnetic stirrer for 30min; vacuum degassing for 10min before coating (feeler gauge height 0.4mm), and then place in an oven at 80℃ for 12h to obtain a flame retardant layer with a thickness of 280μm.
[0053] 2. Preparation of absorbing layer
[0054] 80g polyurethane emulsion, 200g magnetic metal alloy particles, 8g deionized water, 0.4g defoamer, 4g crosslinking aid, 0.3g orientation agent, 1.2g thickener were mixed, stirred with a mechanical stirrer for 30min, then filtered and vacuum degassed for 10min. The slurry was placed on a coater with a feeler gauge height of 0.42mm; after coating, it was placed in an oven at 80℃ and baked for 12h to obtain a wave absorbing layer with a thickness of 350μm.
[0055] 3. Multi-layer assembly of patches
[0056] The prepared 280μm flame retardant layer, 350μm wave absorbing layer and 200μm nickel-plated copper conductive cloth were bonded together using double-sided polyurethane pressure-sensitive adhesive (30μm). During the bonding process, a silicone roller was used to roll from the bonding end to the non-bonding end to make them fit. After they were fully bonded, they were rolled back and forth for 5 times with a rolling force of 1kg / cm 2 When a functional layer is damaged or has abnormal quality, it can be directly peeled off with the pressure-sensitive adhesive and replaced.
[0057] [Example 3]
[0058] A method for preparing a flame retardant wave absorbing patch comprises the following steps:
[0059] 1. Preparation of flame retardant layer
[0060] Weigh 4.8g of triazine carbonizing agent, 5.0g of triphenyl phosphate and 4.3g of melamine, put them in a clean mortar, grind for 10min to mix them evenly to obtain a flame retardant. Add the flame retardant to 100g of acrylic emulsion, and also add 0.1g of dispersant and 0.5g of defoaming agent, stir with a magnetic stirrer for 30min; vacuum degassing for 10min before coating (feeler gauge height 0.45mm), and then place in an oven at 80℃ for 12h to obtain a flame retardant layer with a thickness of 280μm.
[0061] 2. Preparation of absorbing layer
[0062] 80g polyurethane emulsion, 280g magnetic metal alloy particles, 15g deionized water, 0.4g defoamer, 4g crosslinking aid, 0.3g orientation agent were mixed, stirred with a mechanical stirrer for 30min, then filtered and vacuum degassed for 10min. The slurry was placed on a coater with a feeler gauge height of 0.50mm; after coating, it was placed in an oven at 80℃ and baked for 12h to obtain a wave absorbing layer with a thickness of 350μm.
[0063] 3. Multi-layer assembly of patches
[0064] The prepared 280μm flame retardant layer, 350μm wave absorbing layer and 200μm nickel-plated copper conductive cloth were bonded together using double-sided acrylic pressure-sensitive adhesive (30μm). During the bonding process, a silicone roller was used to roll from the bonding end to the non-bonding end to make them fit. After they were fully bonded, they were rolled back and forth for 5 times with a rolling force of 0.9kg / cm 2 When a functional layer is damaged or has abnormal quality, it can be directly peeled off with the pressure-sensitive adhesive and replaced.
[0065] [Example 4]
[0066] A method for preparing a flame retardant wave absorbing patch comprises the following steps:
[0067] 1. Preparation of flame retardant layer
[0068] Weigh 4.5g of triazine carbon former, 3.2g of aluminum hypophosphite, 3.0g of ammonium polyphosphate and 5.0g of melamine, put them in a clean mortar, grind for 15min to mix them evenly to obtain a flame retardant. Add the flame retardant to 100g of acrylic emulsion, and also add 0.1g of dispersant and 0.5g of defoamer, stir with a magnetic stirrer for 30min; vacuum degassing for 10min before coating (feeler gauge height 0.42mm), and then place in an oven at 80℃ for 12h to obtain a flame retardant layer with a thickness of 280μm.
[0069] 2. Preparation of absorbing layer
[0070] 80g polyurethane emulsion, 300g magnetic metal alloy particles, 15g deionized water, 0.4g defoamer, 4g crosslinking aid, 0.3g orientation agent were mixed, stirred with a mechanical stirrer for 30min, then filtered and vacuum degassed for 10min. The slurry was placed on a coater with a feeler gauge height of 0.54mm; after coating, it was placed in an oven at 80℃ and baked for 12h to obtain a wave absorbing layer with a thickness of 350μm.
[0071] 3. Multi-layer assembly of patches
[0072] according to Figure 1 The prepared 280μm flame retardant layer, 350μm wave absorbing layer and 200μm silver / polyester blended conductive fabric were bonded together using double-sided acrylic pressure-sensitive adhesive (30μm). During the bonding process, a silicone roller was used to roll from the bonding end to the non-bonding end to make them fit. After they were fully bonded, they were rolled back and forth for 5 times with a rolling force of 1.2kg / cm 2 When a functional layer is damaged or has abnormal quality, it can be directly peeled off with the pressure-sensitive adhesive and replaced.
[0073] [Comparative Example 1]
[0074] A method for preparing a comparison patch comprises the following steps:
[0075] 1. Preparation of flame retardant layer
[0076] 14.7 g of tetrabromobisphenol A was weighed and added to 100 g of acrylic emulsion. 0.1 g of dispersant and 0.5 g of defoaming agent could also be added. The mixture was stirred for 30 min using a magnetic stirrer. After vacuum degassing for 10 min, the mixture was coated (feeler gauge height 0.46 mm). The mixture was then placed in an oven at 80° C. for 12 h to obtain a flame retardant layer with a thickness of 280 μm.
[0077] 2. Preparation of absorbing layer
[0078] 80g polyurethane emulsion, 240g magnetic metal alloy particles, 10g deionized water, 0.4g defoamer, 4g crosslinking aid, 0.3g orientation agent, 1.2g thickener were mixed, stirred with a mechanical stirrer for 30min, then filtered and vacuum degassed for 10min. The slurry was placed on a coater with a feeler gauge height of 0.5mm; after coating, it was placed in an oven at 80℃ and baked for 12h to obtain a wave absorbing layer with a thickness of 350μm.
[0079] 3. Multi-layer assembly of patches
[0080] The prepared 280μm flame retardant layer, 350μm wave absorbing layer and 200μm silver-plated conductive fabric were bonded together using double-sided acrylic pressure-sensitive adhesive (30μm). During the bonding process, a silicone roller was used to roll from the bonding end to the non-bonding end to make them fit together. After they were fully bonded, they were rolled back and forth for 5 times with a rolling force of 0.8kg / cm 2 When a functional layer is damaged or has abnormal quality, it can be directly peeled off with the pressure-sensitive adhesive and replaced.
[0081] [Comparative Example 2]
[0082] A method for preparing a comparison patch comprises the following steps:
[0083] 1. Preparation of flame retardant layer
[0084] 14.1 g of decabromodiphenyl ether was weighed and added to 100 g of acrylic emulsion. 0.1 g of dispersant and 0.5 g of defoaming agent could also be added. The mixture was stirred for 30 min using a magnetic stirrer. After vacuum degassing for 10 min, the mixture was coated (feeler gauge height 0.42 mm). The mixture was then placed in an oven at 80° C. for 12 h to obtain a flame retardant layer with a thickness of 280 μm.
[0085] 2. Preparation of absorbing layer
[0086] 80g polyurethane emulsion, 280g magnetic metal alloy particles, 15g deionized water, 0.4g defoamer, 4g crosslinking aid, 0.3g orientation agent were mixed, stirred with a mechanical stirrer for 30min, then filtered and vacuum degassed for 10min. The slurry was placed on a coater with a feeler gauge height of 0.50mm; after coating, it was placed in an oven at 80℃ and baked for 12h to obtain a wave absorbing layer with a thickness of 350μm.
[0087] 3. Multi-layer assembly of patches
[0088] The prepared 280μm flame retardant layer, 350μm wave absorbing layer and 200μm nickel-plated copper conductive cloth were bonded together using double-sided acrylic pressure-sensitive adhesive (30μm). During the bonding process, a silicone roller was used to roll from the bonding end to the non-bonding end to make them fit. After they were fully bonded, they were rolled back and forth for 5 times with a rolling force of 0.9kg / cm 2 When a functional layer is damaged or has abnormal quality, it can be directly peeled off with the pressure-sensitive adhesive and replaced.
[0089] The flame retardant absorbing patches of Examples 1-4 and Comparative Examples 1-2 of the present invention were tested for performance. The vertical reflectivity was measured according to the GJB 2038A radar absorbing material reflectivity test method, with an aluminum plate as the substrate; the peeling force was measured according to the GB / T2792 adhesive tape peeling strength test method, with an aluminum plate as the substrate; the fire resistance time was measured according to the GB / T 15442.2 fire resistance performance classification and test method for decorative fire retardant coatings, with a wooden board as the substrate; the heat release rate was tested directly on the fire-resistant fiber layer according to the GB / T 16172-2007 building material heat release test method. The test results are shown in the following table:
[0090]
[0091]
[0092] It can be seen from the above table that the above embodiments of the present invention achieve the following technical effects:
[0093] The composite of the multilayer structure of the flame retardant layer, the wave absorbing layer and the conductive layer is realized through a simple bonding process, which can simultaneously give the bonded material good radar stealth performance and fireproof performance. In order to achieve a better flame retardant effect and realize the recyclability of the patch after burning, the present invention designs an intumescent flame retardant layer on the surface of the patch, so that the embodiment has a longer fire resistance time and a lower heat release rate, and the wave absorbing layer and the conductive layer of the patch after burning are not damaged and can be used multiple times, reducing the manufacturing and use costs of the patch.
[0094] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A flame retardant microwave absorbing patch, characterized in that: The invention comprises a flame retardant layer (1), an absorbing layer (2), a conductive layer (3) and a release layer (4), wherein the flame retardant layer (1) is bonded to the surface of the absorbing layer (2) via an adhesive layer (5), the bottom surface of the absorbing layer (2) is bonded to the surface of the conductive layer (3) via an adhesive layer (5), and the release layer (4) is bonded to the bottom surface of the conductive layer (3) via an adhesive layer (5).
2. The flame retardant absorbing patch according to claim 1, characterized in that: The flame retardant layer (1) is made of an intumescent flame retardant and a resin matrix.
3. The flame retardant absorbing patch according to claim 2, characterized in that: The intumescent flame retardant comprises a charring agent, a dehydrating agent and a foaming agent.
4. The flame retardant absorbing patch according to claim 3, characterized in that: The carbon-forming agent is one or more of pentaerythritol, dipentaerythritol, sorbitol, starch, triazine carbon-forming agent, and polyimide carbon-forming agent.
5. The flame retardant absorbing patch according to claim 3, characterized in that: The dehydrating agent is one or more of ammonium phosphate, ammonium polyphosphate, triphenyl phosphate, melamine phosphate, aluminum hypophosphite, and dimethyl methyl phosphate.
6. The flame retardant absorbing patch according to claim 3, characterized in that: The foaming agent is one or more of melamine, dicyandiamide, chlorinated paraffin and urea.
7. The flame retardant absorbing patch according to claim 2, characterized in that: The resin matrix is one of polyurethane, acrylate and epoxy resin.
8. The flame retardant and microwave absorbing patch according to claim 1, characterized in that: The adhesive layer (5) is a pressure-sensitive adhesive.
9. The flame retardant absorbing patch according to claim 8, characterized in that: The thickness of the adhesive layer (5) is 1 to 100 μm.
10. A method for preparing a flame retardant and microwave absorbing patch according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1: preparing a flame retardant layer (1); wherein the method for preparing the flame retardant layer (1) is specifically: adding a flame retardant to a resin matrix, stirring with a magnetic stirrer for 30 minutes, vacuum degassing for 10 minutes, then coating, and baking in an oven at 80° C. for 12 hours to obtain a flame retardant layer; S2: preparing an absorbing layer (2) and a conductive layer (3); S3: Multi-layer assembly of the patch: the flame retardant layer (1), the wave absorbing layer (2) and the conductive layer (3) are sequentially bonded together using an adhesive layer (5). During the bonding process, a silicone roller is used to roll from the bonded end to the unbonded end to make them bonded. After they are fully bonded, they are rolled back and forth for 4 to 6 times with a rolling force of 0.8 to 1.2 kg / cm². S4: bonding the release layer (4) to the bottom surface of the conductive layer (3) via the adhesive layer (5).