Double-lap-joint polymeric membrane-based waterproof coiled material with capillary crystallization function
By adding silicone waterproofing agent and mineral sand to the waterproof roll, silicate crystallization is promoted, and 3-trifluoroacetoxypropyltrimethoxysilane and epoxysulfuron are used, the waterproof roll is easily permeable. and aging problems achieve self-healing function, improve water retardancy and impermeability, and reduce maintenance costs.
Patent Information
- Application Number
- CN202411193665.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-22
AI Technical Summary
The double-layer polymer membrane-based waterproof coil is easy to permeate during long-term use, and aging accelerates, resulting in reduced performance and inability to heal itself, increasing maintenance costs and waterproof hidden dangers.
Add silicone waterproofing agent and mineral sand to the bonding layer of the waterproof coil to promote the crystallization of silicate minerals, fill in tiny cracks and pores, and use 3-trifluoroacetoxypropyltrimethoxysilane and ring As a dispersant, oxazuron enhances compatibility and bonding strength and achieves self-healing function.
It improves the water-repellent resistance and impermeability of the waterproof coil, extends the service life, reduces maintenance costs, and realizes the self-healing function when micro-cracks appear, ensuring the waterproof effect.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof coiled materials, and in particular to a double-lapped polymer membrane-based waterproof coiled material with a penetration crystallization function. Background Art
[0002] Double-lap polymer membrane-based waterproofing membrane is a new type of building waterproofing material. It is widely used in various building waterproofing projects because of its convenient construction, environmental protection and safety, and good flexibility. For example, it is used in the exterior or interior structure of a building to form a waterproof barrier to prevent moisture from penetrating from the outside to the inside. However, with the long-term use of this material, some problems have also been exposed. The membrane is exposed to harsh environments such as moisture, ultraviolet rays and chemicals for a long time, which accelerates the aging and degradation of the waterproof membrane, resulting in performance degradation, thereby shortening its service life. Once a leak occurs, the repair work will be more complicated and expensive, and more frequent inspections and maintenance will be required in the later stage, increasing the overall maintenance cost. When microcracks appear, self-healing cannot be achieved, resulting in long-term waterproofing risks. Therefore, the development of a double-lap polymer membrane-based waterproofing membrane with penetration crystallization function is an urgent problem to be solved. Summary of the invention
[0003] The invention provides a double-lapped polymer membrane-based waterproofing coiled material with a penetration crystallization function, which solves the problem of easy water permeability of the waterproofing coiled material in the related art.
[0004] The technical scheme of the present invention is as follows: The present invention provides a double-lapped polymer membrane-based waterproofing coiled material with a permeation crystallization function, which comprises, from top to bottom, an anti-adhesion protective layer, a first permeation reaction adhesive layer, a first polymer membrane base layer, a second permeation reaction adhesive layer, a second polymer membrane base layer, a third permeation reaction adhesive layer, and an isolation film, wherein the anti-adhesion protective layer comprises the following components in parts by weight: 10 to 20 parts of mineral sand, 30 to 50 parts of hydroxyl acrylic resin, 20 to 30 parts of silicone waterproofing agent, 0.3 to 0.5 parts of dispersant, 0.3 to 0.5 parts of antifreeze agent, 0.5 to 1 parts of defoaming agent, and 20 to 30 parts of water; The dispersant includes 3-trifluoroacetoxypropyltrimethoxysilane and / or oxasulfuron-methyl.
[0005] As a further technical solution, when the dispersant is composed of 3-trifluoroacetoxypropyltrimethoxysilane and oxasulfuron-methyl, the mass ratio of 3-trifluoroacetoxypropyltrimethoxysilane to oxasulfuron-methyl is 2-4:1.
[0006] As a further technical solution, the mass ratio of 3-trifluoroacetoxypropyltrimethoxysilane to oxasulfuron is 3:1.
[0007] As a further technical solution, the mineral sand includes one or more of quartz sand, mullite sand, and sintered sand.
[0008] As a further technical solution, the hydroxylated acrylic emulsion consists of a first hydroxylated acrylic emulsion and a second hydroxylated acrylic emulsion.
[0009] As a further technical solution, the first hydroxyl acrylic emulsion and the second hydroxyl acrylic emulsion have different hydroxyl values, and the hydroxyl value of the first hydroxyl acrylic emulsion is smaller than the hydroxyl value of the second hydroxyl acrylic emulsion.
[0010] As a further technical solution, the hydroxyl value of the first hydroxylated acrylic emulsion is 60 mgKOH / g, and the hydroxyl value of the second hydroxylated acrylic emulsion is 94 mgKOH / g.
[0011] As a further technical solution, the mass ratio of the first hydroxylated acrylic emulsion to the second hydroxylated acrylic emulsion is 1-2:3.
[0012] As a further technical solution, the mass ratio of the first hydroxylated acrylic emulsion to the second hydroxylated acrylic emulsion is 1:2.
[0013] As a further technical solution, the isolation film is a PE film.
[0014] As a further technical solution, the defoaming agent includes one or more of emulsified silicone oil, high carbon alcohol fatty acid ester complex, and polyoxyethylene polyoxypropylene pentaerythritol ether.
[0015] As a further technical solution, the antifreeze agent includes one or more of glycerol, ethylene glycol, and propylene glycol.
[0016] The present invention also proposes a method for preparing a double-lapped polymer membrane-based waterproofing coiled material with a penetration crystallization function. The specific preparation method is: S1, weighing the raw materials, and mixing them evenly to obtain the anti-sticking protective layer raw materials; S2, preparing a 0.3 mm thick polyethylene terephthalate film as the first polymer film base layer, a 0.3 mm thick polyethylene terephthalate film as the second polymer film base layer, and a 0.15 mm thick PE film as a separator; S3. Heat 35 parts of 90# asphalt to 185°C, mix evenly with 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS 4452, 3.5 parts of petroleum resin C9, 5 parts of dibutyl phthalate, 0.6 parts of antioxidant 1010, 40 parts of talcum powder and 3 parts of 2-cyanoaniline, cool to 145°C, introduce into between calendering rollers through a pump, cover between the first polymer film base and the second polymer film base, between the second polymer film base and the isolation film respectively, calender, and coat the surface with the raw material of the anti-sticking protective layer to obtain the double-lap polymer film-based waterproof membrane.
[0017] The working principle and beneficial effects of the present invention are: In the present invention, an organosilicon waterproofing agent and mineral sand are added to the bonding layer of the waterproofing coiled material. The organosilicon waterproofing agent, as a silicon source, can undergo a hydration reaction in the pores of the mineral sand to promote the crystallization of silicate minerals. These crystals can fill the tiny cracks and pores in the substrate, thereby improving the waterproofness. In the application process, if tiny cracks appear, the infiltrated crystallization material can react with the components in the water to automatically generate crystals to fill the cracks, thereby achieving a "self-healing" function and ensuring the waterproofing effect. 3-Trifluoroacetoxypropyltrimethoxysilane and oxasulfuron are added as dispersants to enhance the compatibility and bonding strength between the components and improve the impermeability of the waterproofing coiled material. DETAILED DESCRIPTION
[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] In the following examples and comparative examples: The first hydroxyl acrylic resin: the hydroxyl value is 60mgKOH / g, the model is FX-9460, and the manufacturer is Jiangsu Saixin Resin Co., Ltd.; The second hydroxy acrylic resin: the hydroxyl value is 94 mgKOH / g, the model is Joncryl 910, and the manufacturer is Guangzhou Yangsong Technology Co., Ltd.; Silicone waterproofing agent: Model 011, manufacturer: Shandong Xinxiangda Chemical Co., Ltd. High carbon alcohol fatty acid ester complex: industrial grade, model CI-314, manufacturer: Guangdong Nanhui New Materials Co., Ltd. Emulsified silicone oil: Model 3002, manufacturer: Dezhou Decheng District Binshengjing Cleaning Products Factory; Polyoxyethylene polyoxypropylene pentaerythritol ether: model number is SPO-10, the manufacturer is Jiangsu Hai'an Petrochemical Plant; Polyethylene terephthalate film: thickness 0.3 mm, manufacturer Shanghai Fuzhong Industrial Co., Ltd.; Carboxylated styrene butadiene rubber: Ultrafine powder carboxylated styrene butadiene rubber, brand name NarpowVP201, manufactured by Beijing Beihua Research Institute of China Petrochemical Corporation; PE film: thickness is 0.15mm, the manufacturer is Wenzhou Zhenglin Plastic Technology Co., Ltd.
[0020] Example 1 S1, weigh 10 parts of quartz sand, 30 parts of the first hydroxy acrylic resin, 20 parts of the silicone waterproofing agent, 0.3 parts of 3-trifluoroacetoxypropyltrimethoxysilane, 0.3 parts of glycerol, 0.5 parts of emulsified silicone oil, and 20 parts of water, and stir evenly to obtain the anti-sticking protective layer raw material; S2, preparing a 0.3 mm thick polyethylene terephthalate film as the first polymer film base layer, a 0.3 mm thick polyethylene terephthalate film as the second polymer film base layer, and a 0.15 mm thick PE film as a separator; S3. Heat 35 parts of 90# asphalt to 185°C, mix evenly with 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS 4452, 3.5 parts of petroleum resin C9, 5 parts of dibutyl phthalate, 0.6 parts of antioxidant 1010, 40 parts of talcum powder and 3 parts of 2-cyanoaniline, cool to 145°C, introduce into between calendering rollers through a pump, and coat between the first polymer film base and the second polymer film base, and between the second polymer film base and the isolation film respectively, calender, and coat the surface with an anti-sticking protective layer to obtain a double-lap polymer film-based waterproof membrane.
[0021] Example 2 Compared with Example 1, the difference of Example 2 lies in the raw materials of the anti-sticking protective layer. The preparation method of the raw materials of the anti-sticking protective layer in Example 2 is: weigh 15 parts of mullite sand, 40 parts of the first hydroxy acrylic resin, 25 parts of silicone waterproofing agent, 0.4 parts of 3-trifluoroacetoxypropyltrimethoxysilane, 0.4 parts of ethylene glycol, 0.5 parts of high-carbon alcohol fatty acid ester complex, and 25 parts of water, stir well to obtain the anti-sticking protective layer.
[0022] Example 3 Compared with Example 1, the difference of Example 3 lies in the raw materials of the anti-sticking protective layer. The preparation method of the raw materials of the anti-sticking protective layer in Example 3 is: weigh 20 parts of sintered sand, 50 parts of the first hydroxy acrylic resin, 30 parts of silicone waterproofing agent, 0.5 parts of 3-trifluoroacetoxypropyltrimethoxysilane, 0.5 parts of propylene glycol, 0.5 parts of polyoxyethylene polyoxypropylene pentaerythritol ether, and 30 parts of water, stir well to obtain the anti-sticking protective layer.
[0023] Example 4 Compared with Example 1, Example 4 is different in that 0.3 parts of 3-trifluoroacetoxypropyltrimethoxysilane is replaced by an equal amount of oxasulfuron-methyl.
[0024] Example 5 Compared with Example 1, Example 5 is different in that 0.3 parts of 3-trifluoroacetoxypropyltrimethoxysilane is replaced by 0.15 parts of 3-trifluoroacetoxypropyltrimethoxysilane and 0.15 parts of oxasulfuron-methyl.
[0025] Example 6 Compared with Example 1, Example 6 is different in that 0.3 parts of 3-trifluoroacetoxypropyltrimethoxysilane is replaced by 0.2 parts of 3-trifluoroacetoxypropyltrimethoxysilane and 0.1 parts of oxasulfuron-methyl.
[0026] Example 7 Compared with Example 1, Example 7 is different in that 0.3 parts of 3-trifluoroacetoxypropyltrimethoxysilane is replaced by 0.225 parts of 3-trifluoroacetoxypropyltrimethoxysilane and 0.075 parts of oxasulfuron-methyl.
[0027] Example 8 Compared with Example 1, Example 8 is different in that 0.3 parts of 3-trifluoroacetoxypropyltrimethoxysilane is replaced by 0.24 parts of 3-trifluoroacetoxypropyltrimethoxysilane and 0.06 parts of oxasulfuron-methyl.
[0028] Example 9 Compared with Example 1, Example 9 is different in that 0.3 parts of 3-trifluoroacetoxypropyltrimethoxysilane is replaced by 0.25 parts of 3-trifluoroacetoxypropyltrimethoxysilane and 0.05 parts of oxasulfuron-methyl.
[0029] Example 10 Compared with Example 7, the difference in Example 10 is that 30 parts of the first hydroxy acrylic resin are replaced by an equal amount of the second hydroxy acrylic resin.
[0030] Embodiment 11 Compared with Example 7, Example 11 is different in that 30 parts of the first hydroxy acrylic resin are replaced with 15 parts of the first hydroxy acrylic resin and 15 parts of the second hydroxy acrylic resin.
[0031] Example 12 Compared with Example 7, the difference of Example 12 is that 30 parts of the first hydroxy acrylic resin is replaced by 12 parts of the first hydroxy acrylic resin and 18 parts of the second hydroxy acrylic resin.
[0032] Embodiment 13 Compared with Example 7, Example 13 is different in that 30 parts of the first hydroxy acrylic resin are replaced with 10 parts of the first hydroxy acrylic resin and 20 parts of the second hydroxy acrylic resin.
[0033] Embodiment 14 Compared with Example 7, Example 14 is different in that 30 parts of the first hydroxy acrylic resin is replaced by 7.5 parts of the first hydroxy acrylic resin and 22.5 parts of the second hydroxy acrylic resin.
[0034] Embodiment 15 Compared with Example 7, Example 15 is different in that 30 parts of the first hydroxy acrylic resin are replaced with 8 parts of the first hydroxy acrylic resin and 24 parts of the second hydroxy acrylic resin.
[0035] Comparative Example 1 Compared with Example 1, Comparative Example 1 is different in that 3-trifluoroacetoxypropyltrimethoxysilane is not added.
[0036] The waterproof membranes prepared in Examples 1 to 15 and Comparative Example 1 were tested according to the following method: 1. Water penetration resistance (hydraulic gradient MPa): According to the test method specified in GB / T 23457-2017 "Pre-laid waterproof membrane", the water penetration resistance of the sample is tested. The sample size is: 110mm×110mm×0.3mm. The test time is 4h. The maximum pressure that the mortar test block can withstand without water seepage on the surrounding surface is recorded.
[0037] 2. Waterproofness: According to the P-type product test method specified in GB / T 35467-2017 "Wet-laid waterproof membrane", the water-impermeability of the sample is tested. The anti-sticking protective layer is retained during the test. The sample size is: 110mm×110mm×0.3mm, the test condition is 0.6MPa, and the time when water permeability occurs is recorded.
[0038] The test results are shown in the following table: Table 1 Performance test results of waterproof membranes prepared in Examples 1 to 15 and Comparative Example 1
[0039] Compared with Comparative Example 1, Example 1 adds 3-trifluoroacetoxypropyltrimethoxysilane. As a result, the water resistance and water impermeability of Example 1 are better than those of Comparative Example 1, indicating that the addition of 3-trifluoroacetoxypropyltrimethoxysilane can improve the water resistance and water impermeability of the coiled material.
[0040] Compared with Examples 1 and 4, Examples 5 to 9 simultaneously added 3-trifluoroacetoxypropyltrimethoxysilane and oxasulfuron-methyl. As a result, the water resistance and water impermeability of Examples 5 to 9 were better than those of Examples 1 and 4, indicating that 3-trifluoroacetoxypropyltrimethoxysilane and oxasulfuron-methyl played a synergistic role, which could further improve the water resistance and water impermeability of the waterproof membrane.
[0041] Compared with Example 5, Examples 6 to 9 added 3-trifluoroacetoxypropyltrimethoxysilane and oxasulfuron in different mass ratios. As a result, the water resistance and water impermeability of Examples 6 to 8 were better than those of Examples 5 and 9, indicating that when the mass ratio of 3-trifluoroacetoxypropyltrimethoxysilane and oxasulfuron is 2 to 4:1, and the preferred ratio is 3:1, the obtained waterproof membrane has better water resistance and water impermeability.
[0042] Compared with Examples 7 and 10, Examples 11 to 15 simultaneously added the first hydroxyl acrylic emulsion and the second hydroxyl acrylic emulsion. As a result, the water resistance and water impermeability of Examples 11 to 15 were better than those of Examples 7 and 10, indicating that the first hydroxyl acrylic emulsion and the second hydroxyl acrylic emulsion play a synergistic role and can further improve the water resistance and water impermeability of the waterproof membrane.
[0043] Compared with Example 11, Examples 12 to 15 added the first hydroxyl acrylic emulsion and the second hydroxyl acrylic emulsion in different mass ratios. As a result, the water resistance and water impermeability of Examples 12 to 14 were better than those of Examples 11 and 15, indicating that when the mass ratio of the first hydroxyl acrylic emulsion and the second hydroxyl acrylic emulsion is 1 to 2:3, and the preferred ratio is 1:2, the obtained waterproof membrane has the best water resistance and water impermeability.
[0044] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A double-lapped polymer membrane-based waterproofing membrane with a permeation crystallization function, which comprises, from top to bottom, an anti-adhesion protective layer, a first permeation reaction adhesive layer, a first polymer membrane base layer, a second permeation reaction adhesive layer, a second polymer membrane base layer, a third permeation reaction adhesive layer, and a separator, characterized in that: The anti-sticking protective layer comprises the following components in parts by weight: 10-20 parts of mineral sand, 30-50 parts of hydroxy acrylic resin, 20-30 parts of silicone waterproofing agent, 0.3-0.5 parts of dispersant, 0.3-0.5 parts of antifreeze agent, 0.5-1 parts of defoaming agent, and 20-30 parts of water; the dispersant comprises 3-trifluoroacetoxypropyltrimethoxysilane and / or oxasulfuron-methyl.
2. The double-lapped polymer membrane-based waterproofing coiled material with penetration crystallization function according to claim 1, characterized in that: When the dispersant is composed of 3-trifluoroacetoxypropyl trimethoxysilane and oxasulfuron-methyl, the mass ratio of 3-trifluoroacetoxypropyl trimethoxysilane to oxasulfuron-methyl is 2-4:
1.
3. The double-lapped polymer membrane-based waterproofing coiled material with penetration crystallization function according to claim 1, characterized in that: The mineral sand includes one or more of quartz sand, mullite sand and sintered sand.
4. The double-lapped polymer membrane-based waterproofing coiled material with penetration crystallization function according to claim 1, characterized in that: The hydroxy acrylic resin consists of a first hydroxy acrylic resin and a second hydroxy acrylic resin.
5. The double-lapped polymer membrane-based waterproofing coiled material with penetration crystallization function according to claim 4, characterized in that: The first hydroxy acrylic resin and the second hydroxy acrylic resin have different hydroxy values, and the hydroxy value of the first hydroxy acrylic resin is smaller than the hydroxy value of the second hydroxy acrylic resin.
6. The double-lapped polymer membrane-based waterproofing coiled material with penetration crystallization function according to claim 4, characterized in that: The hydroxyl value of the first hydroxy acrylic resin is 60 mgKOH / g, and the hydroxyl value of the second hydroxy acrylic resin is 94 mgKOH / g.
7. The double-lapped polymer membrane-based waterproofing coiled material with penetration crystallization function according to claim 4, characterized in that: The mass ratio of the first hydroxy acrylic resin to the second hydroxy acrylic resin is 1-2:
3.
8. The double-lapped polymer membrane-based waterproofing coiled material with penetration crystallization function according to claim 1, characterized in that: The isolation film is a PE film.
9. The double-lapped polymer membrane-based waterproofing coiled material with penetration crystallization function according to claim 1, characterized in that: The defoaming agent includes one or more of emulsified silicone oil, high carbon alcohol fatty acid ester complex, and polyoxyethylene polyoxypropylene pentaerythritol ether.
10. The double-lapped polymer membrane-based waterproofing coiled material with penetration crystallization function according to claim 1, characterized in that: The antifreeze agent includes one or more of glycerol, ethylene glycol, and propylene glycol.