Preparation process of stable gum diaphragm

By using transparent PET film and high-solids-content polyurethane adhesive, combined with precise preparation process and quality control, the problems of uniformity, curing and compatibility in the preparation of adhesive-backed films have been solved, achieving the production of high-quality and stable adhesive-backed films.

CN118995073APending Publication Date: 2024-11-22ANHUI BOX FILM TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410813991.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing adhesive-backed films suffer from issues such as adhesive uniformity, drying and curing control, substrate compatibility, environmental pollution, and impurities during the preparation process, which affect their adhesion performance and stability.

Method used

Using transparent PET film and high-solids-content polyurethane adhesive as raw materials, combined with ultrasonic cleaning, plasma treatment, precise formulation of the adhesive backing, high-precision coating machine and constant temperature and humidity system to ensure a clean and stable environment, gradual heating and drying curing, and strict quality testing and packaging.

Benefits of technology

It improves the adhesion, weather resistance and stability of the adhesive film, ensures the uniformity and complete curing of the adhesive layer, expands the application range, reduces production costs and defect rate, and improves product quality and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995073A_ABST
    Figure CN118995073A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of gum membrane processing, and discloses a stable gum membrane preparation technology. The method comprises the steps that S1, raw materials are selected, a base material is selected, a transparent PET (polyethylene glycol terephthalate) film is adopted as the base material, a back adhesive material is selected, and a high-solid-content polyurethane (PU) adhesive is selected as the back adhesive material; and S2, pretreatment and base material cleaning are conducted, specifically, the PET film is cleaned through an ultrasonic cleaning machine, surface activation is conducted on the PET film, and plasma treatment equipment is used for conducting surface activation treatment on the cleaned PET film. According to the invention, by selecting the gum material with good compatibility, the uniformity and complete curing of the gum layer are ensured, and the possible defects in the preparation and use processes of the gum membrane are effectively prevented. Due to the improvement of the stability, the gum diaphragm can be better applied to the fields of circuit board protection, electronic component protection and the like, the service life of the gum diaphragm is prolonged, the reliability of the gum diaphragm is improved, and more stable protection is provided for electronic products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesive-backed film processing, and in particular relates to a process for preparing a stable adhesive-backed film. Background Art

[0002] In the field of electronics, adhesive-backed films are widely used. Among them, TPU film with adhesive backing is an important application example. TPU film with adhesive backing has been widely used in the electronics industry, mainly due to its excellent electrical insulation performance and weather resistance. These characteristics give it significant advantages in the protection of circuit boards and electronic components. By using TPU film with adhesive backing, the stability and reliability of electronic products have been effectively improved, and it also helps to extend the service life of the product. In addition, adhesive-backed films can also be used for surface protection and decoration of electronic equipment. They can be pasted on the screen, casing and other parts of the device to prevent scratches, dirt and fingerprints, and enhance the appearance and user experience of the device. At the same time, some specially designed adhesive-backed films also have functions such as electrical conductivity and thermal conductivity, which can meet the special needs of electronic equipment in complex environments.

[0003] There are still some problems in the preparation of adhesive films commonly used in the electronics field, such as the uniformity of the adhesive. During the adhesive coating process, if the accuracy of the coating machine is not high enough or the operation is improper, the thickness of the adhesive layer may be uneven, which will affect the adhesion performance of the film. Problems in the drying and curing process. Drying and curing are key steps in the preparation of adhesive films. If the temperature, humidity or time are not properly controlled, the adhesive layer may not be fully cured or over-cured, thereby affecting its adhesion and stability. There are compatibility issues between the adhesive and the substrate. There may be compatibility issues between different substrates and adhesive materials, which may lead to insufficient adhesion between the adhesive layer and the substrate or easy falling off. Environmental pollution and impurity problems. During the preparation process, if the production environment is not clean enough or there are impurities, it may cause defects such as stains and bubbles on the surface of the adhesive film, affecting its appearance and performance. Problems during storage and transportation. During storage and transportation, the adhesive film may be affected by environmental factors such as temperature and humidity, resulting in changes in the performance of the adhesive layer. Summary of the invention

[0004] The purpose of the present invention is to provide a stable adhesive-backed film preparation process to solve the problems raised in the above background technology.

[0005] In order to achieve the above-mentioned object, the present invention provides the following technical solution: a process for preparing a stable adhesive-backed film, comprising the following steps;

[0006] S1: Raw material selection: base material, transparent PET (polyethylene terephthalate) film is used as base material, adhesive material, high solid content polyurethane (PU) adhesive is used as adhesive material;

[0007] S2: pretreatment, substrate cleaning, cleaning the PET film with an ultrasonic cleaner, surface activation, and surface activation treatment of the cleaned PET film with a plasma treatment device;

[0008] S3: Preparation of adhesive formula, which includes polyurethane adhesive, thickener, antioxidant and solvent;

[0009] S4: Preparation of adhesive: In a clean mixing tank, add polyurethane adhesive, thickener, antioxidant and solvent in order according to the formula ratio, and start the mixing equipment. The prepared adhesive liquid needs to be filtered through a filter to remove possible impurities to ensure the coating quality;

[0010] S5: Coating: Use a high-precision coating machine to evenly coat the prepared adhesive liquid on the pre-treated PET film. During the coating process, the environment must be kept clean to prevent dust and other impurities from falling in;

[0011] S6: Drying and curing, sending the coated film into the drying room to remove the solvent and ensure that the adhesive layer is completely cured;

[0012] S7: Environmental control. The production workshop is equipped with a constant temperature and humidity system to ensure a stable production environment. The air quality in the workshop is regularly tested to ensure that it is dust-free and odor-free.

[0013] S8: Clean production. Regularly clean production equipment thoroughly, use special cleaning agents and dust-free cloths to ensure that there is no dust, oil or impurities on the equipment surface. Operators must wear anti-static work clothes and gloves, and must go through an air shower room for dust removal before entering the production workshop.

[0014] S9: Quality inspection and packaging.

[0015] By selecting transparent PET film and high-solid content polyurethane adhesive as raw materials, the transparency of the substrate and the adhesion performance of the adhesive are ensured. The cleaning and surface activation treatment of the substrate further improves the adhesion effect between the adhesive layer and the substrate, thereby enhancing the overall stability of the diaphragm. The preparation of the adhesive formula includes the precise ratio of polyurethane adhesive, thickener, antioxidant and solvent. This ratio ensures the stability and uniformity of the adhesive liquid, which helps to improve the adhesion and weather resistance of the diaphragm. The use of a high-precision coating machine for coating the adhesive liquid ensures the uniformity and thickness consistency of the adhesive layer. At the same time, the environment is kept clean during the coating process to avoid the mixing of impurities such as dust, thereby improving the quality of the diaphragm. Through the drying and curing process with gradually increasing temperature, the adhesive layer is completely cured, avoiding the performance degradation caused by insufficient curing. The constant temperature and humidity system of the production workshop and regular air quality testing ensure the stability of the production environment and dust-free and odor-free. At the same time, thorough cleaning of production equipment and anti-static measures for operators avoid the impact of impurities and static electricity on the quality of the diaphragm. Quality testing methods such as adhesion test, weather resistance test and temperature resistance test ensure that the performance of the diaphragm meets the standard requirements. The use of anti-static packaging bags for packaging ensures the stability and safety of the diaphragm during transportation and storage.

[0016] As a further technical solution of the present invention, when the substrate is selected, the specification of the PET film is 0.1mm×1200mm, and it is required to have high light transmittance, good tensile strength and wear resistance. The high solid content polyurethane (PU) adhesive is required to have high adhesion, low volatile organic compound (VOC) content and good weather resistance.

[0017] The PET film has excellent visual transparency due to its high light transmittance. At the same time, its good tensile strength and wear resistance enhance the durability and service life of the film, ensuring stable performance in various application scenarios. The high adhesion of the high-solid content polyurethane adhesive ensures a strong bond between the backing layer and the substrate, improving the overall stability and reliability of the film. The low volatile organic compound (VOC) content meets environmental protection requirements and reduces potential harm to the environment and human body. The good weather resistance of the polyurethane adhesive enables the film to resist the influence of natural factors and maintain stable performance, which is particularly suitable for outdoor application scenarios.

[0018] As a further technical solution of the present invention, when cleaning the substrate, pure water is used as a cleaning medium, and the cleaning time is 5 minutes. During the activation treatment, the treatment time is 30 seconds to increase its surface energy and enhance the adhesion performance with the back adhesive layer.

[0019] Substrate cleaning uses pure water as the cleaning medium and thoroughly removes dust, oil and other impurities on the surface of the substrate within a specified time to ensure the cleanliness of the substrate surface. This step is the basis for ensuring good adhesion between the back adhesive layer and the substrate, avoiding poor adhesion caused by impurities. The activation treatment uses a specific process, such as using plasma treatment equipment to activate the surface of the cleaned substrate to increase the surface energy of the substrate. This process enhances the activity and wettability of the substrate surface, allowing the back adhesive layer to better bond with the substrate and improve the adhesion performance. This not only ensures a close bond between the back adhesive layer and the substrate, but also enhances the overall stability and durability of the diaphragm.

[0020] As a further technical solution of the present invention, the mass ratio of the polyurethane adhesive is 60%, the mass ratio of the thickener, i.e., hydroxyethyl cellulose, is 5%, the mass ratio of the antioxidant, i.e., the mass ratio of the antioxidant, is 2%, the mass ratio of the solvent is 33%, and a mixed solvent of ethyl acetate and ethanol is used in a ratio of 2:1.

[0021] The high content of polyurethane adhesive ensures that the adhesive layer has excellent adhesion properties, enabling it to adhere firmly to various substrates. The addition of thickener adjusts the viscosity of the adhesive liquid, ensuring the uniformity of coating and the consistency of the thickness of the adhesive layer. The addition of antioxidant effectively prevents the oxidative degradation of the adhesive layer and extends the service life of the film. The use of a mixed solvent of ethyl acetate and ethanol not only ensures the full dissolution of the adhesive and additives, but also achieves rapid drying and curing of the adhesive liquid by adjusting the volatilization rate, avoiding defects in the drying process. In summary, this formula selection ensures the high quality, high performance and stability of the adhesive film.

[0022] As a further technical solution of the present invention, when preparing the back glue, the initial stirring speed of the stirring equipment is 500 rpm, and gradually increased to 1000 rpm, and the stirring time is a total of 40 minutes to ensure that the components are mixed evenly without particles and bubbles.

[0023] It ensures that the various components in the adhesive formula can be fully mixed and evenly formed to form a uniform adhesive liquid; secondly, long-term stirring and gradually increasing stirring speed help to eliminate particles and bubbles in the adhesive liquid, making the adhesive liquid more delicate and defect-free; finally, the adhesive liquid prepared in this way has better performance and can improve the overall quality of the adhesive film, including adhesion, appearance quality and usage experience.

[0024] As a further technical solution of the present invention, during the coating, the coating speed of the coater is 5m / min, and the coating thickness is controlled to be 20±2μm by adjusting the scraper gap of the coater. During the drying and curing, the initial temperature of the drying chamber is 40°C, which is gradually increased to 60°C and maintained for 20 minutes to remove the solvent. Then, the curing stage is entered, and the temperature is gradually increased to 100°C and maintained for 30 minutes, and then increased to 120°C and maintained for 40 minutes. Air circulation must be maintained during the curing process to avoid excessive humidity affecting the curing effect.

[0025] The coater works at an appropriate coating speed, which not only ensures production efficiency, but also ensures the uniformity and stability of the coating; by accurately adjusting the scraper gap, the coating thickness is effectively controlled, further improving product quality. Temperature control is key in the drying and curing stages. The initial low temperature helps the solvent evaporate smoothly and avoid coating defects; the subsequent gradual increase in temperature promotes the curing of the coating, improving its hardness and wear resistance. Throughout the process, air circulation is maintained to avoid the influence of humidity on the curing effect. These steps together ensure the coating quality, physical properties and chemical stability of the adhesive-backed film, thereby producing high-performance adhesive-backed film products.

[0026] As a further technical solution of the present invention, during the environmental control, the temperature of the production workshop is controlled at 25±1°C, and the humidity is controlled at 50±3%RH.

[0027] First, it ensures the stability of product quality. By maintaining a stable physical and chemical environment, it avoids fluctuations in product quality caused by environmental changes. Secondly, such environmental control helps improve production efficiency, reduce equipment failures and operator fatigue. In addition, suitable temperature and humidity conditions can ensure operational safety and reduce potential safety risks. Finally, it also helps to extend the service life of production equipment and reduce equipment wear and aging caused by environmental factors.

[0028] As a further technical solution of the present invention, during the quality inspection, the prepared adhesive-backed film is subjected to an adhesion test, a peeling test is performed using a standard tape to ensure that the adhesion meets the requirements, and a weather resistance test is performed. The film is placed in a constant temperature and humidity chamber to simulate different climatic conditions and its performance changes are observed. At the same time, the surface of the film is observed using a microscope to ensure that there are no bubbles, impurities, or scratches.

[0029] Adhesion test, weather resistance test and microscope observation during the quality inspection process jointly ensure the excellent performance and quality of the adhesive film. Adhesion test ensures the film's stable adhesion to the target object, weather resistance test ensures the film's stable performance under various climatic conditions, and microscope observation ensures that the film surface is flawless, free of defects such as bubbles, impurities and scratches. These measures jointly improve the overall quality of the adhesive film and ensure its excellent performance in practical applications.

[0030] As a further technical solution of the present invention, during the packaging, the qualified adhesive-backed film sheets need to be cut according to specifications to ensure accurate size, and be packaged in anti-static packaging bags to ensure good sealing and avoid moisture and contamination. The product name, specifications, production date, and batch number must be marked on the packaging for easy traceability and management.

[0031] First, cutting according to specifications ensures the accuracy of product size and meets customer needs. Secondly, using anti-static packaging bags and ensuring good sealing effectively prevents static damage and moisture contamination, protecting the quality and performance of the product. Finally, marking detailed information on the packaging facilitates product traceability and management, improving the company's production efficiency and customer satisfaction. These measures jointly ensure the safety and integrity of the self-adhesive film during packaging, transportation and storage, providing companies with reliable product guarantees.

[0032] The beneficial effects of the present invention are as follows:

[0033] 1. The present invention ensures the uniformity and complete curing of the adhesive layer by precisely controlling the coating process, optimizing the drying and curing conditions, and selecting adhesive materials with good compatibility, effectively preventing defects that may occur during the preparation and use of the adhesive film. This improvement in stability not only enables the adhesive film to be better applied to circuit boards, electronic component protection and other fields, but also improves its service life and reliability, providing more stable protection for electronic products.

[0034] 2. The present invention solves the compatibility problem between the adhesive and the substrate, so that the adhesive film can be closely combined with various substrates, thereby expanding its application scenarios in the electronic field. Whether it is used for screen protection, shell decoration, or special functional requirements such as electrical conductivity and thermal conductivity, the adhesive film can show excellent performance. This widening of the application scope not only provides more choices and possibilities for electronic products, but also promotes the further development of the adhesive film market.

[0035] 3. The present invention improves the manufacturing efficiency of adhesive-backed diaphragms and reduces production costs by optimizing the production process and reducing defects and rework rates. At the same time, by selecting cost-effective adhesive materials and using efficient coating and curing equipment, the production cost is further reduced, making the adhesive-backed diaphragms more competitive in the market. This improvement in production efficiency and optimization of cost control will help promote the sustainable development of the adhesive-backed diaphragm industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a schematic diagram of the overall process of the present invention. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] like Figure 1 As shown, in an embodiment of the present invention, a process for preparing a stable adhesive-backed film comprises the following steps:

[0039] S1: Raw material selection: base material, transparent PET (polyethylene terephthalate) film is used as base material, adhesive material, high solid content polyurethane (PU) adhesive is used as adhesive material;

[0040] S2: pretreatment, substrate cleaning, cleaning the PET film with an ultrasonic cleaner, surface activation, and surface activation treatment of the cleaned PET film with a plasma treatment device;

[0041] S3: Preparation of adhesive formula, which includes polyurethane adhesive, thickener, antioxidant and solvent;

[0042] S4: Preparation of adhesive: In a clean mixing tank, add polyurethane adhesive, thickener, antioxidant and solvent in order according to the formula ratio, and start the mixing equipment. The prepared adhesive liquid needs to be filtered through a filter to remove possible impurities to ensure the coating quality;

[0043] S5: Coating: Use a high-precision coating machine to evenly coat the prepared adhesive liquid on the pre-treated PET film. During the coating process, the environment must be kept clean to prevent dust and other impurities from falling in;

[0044] S6: Drying and curing, sending the coated film into the drying room to remove the solvent and ensure that the adhesive layer is completely cured;

[0045] S7: Environmental control. The production workshop is equipped with a constant temperature and humidity system to ensure a stable production environment. The air quality in the workshop is regularly tested to ensure that it is dust-free and odor-free.

[0046] S8: Clean production. Regularly clean production equipment thoroughly, use special cleaning agents and dust-free cloths to ensure that there is no dust, oil or impurities on the equipment surface. Operators must wear anti-static work clothes and gloves, and must go through an air shower room for dust removal before entering the production workshop.

[0047] S9: Quality inspection and packaging.

[0048] By selecting transparent PET film and high-solid content polyurethane adhesive as raw materials, the transparency of the substrate and the adhesion performance of the adhesive are ensured. The cleaning and surface activation treatment of the substrate further improves the adhesion effect between the adhesive layer and the substrate, thereby enhancing the overall stability of the diaphragm. The preparation of the adhesive formula includes the precise ratio of polyurethane adhesive, thickener, antioxidant and solvent. This ratio ensures the stability and uniformity of the adhesive liquid, which helps to improve the adhesion and weather resistance of the diaphragm. The use of a high-precision coating machine for coating the adhesive liquid ensures the uniformity and thickness consistency of the adhesive layer. At the same time, the environment is kept clean during the coating process to avoid the mixing of impurities such as dust, thereby improving the quality of the diaphragm. Through the drying and curing process with gradually increasing temperature, the adhesive layer is completely cured, avoiding the performance degradation caused by insufficient curing. The constant temperature and humidity system of the production workshop and regular air quality testing ensure the stability of the production environment and dust-free and odor-free. At the same time, thorough cleaning of production equipment and anti-static measures for operators avoid the impact of impurities and static electricity on the quality of the diaphragm. Quality testing methods such as adhesion test, weather resistance test and temperature resistance test ensure that the performance of the diaphragm meets the standard requirements. The use of anti-static packaging bags for packaging ensures the stability and safety of the diaphragm during transportation and storage.

[0049] Among them, when selecting the substrate, the specification of the PET film is 0.1mm×1200mm, and it needs to have high light transmittance, good tensile strength and wear resistance. The high solid content polyurethane (PU) adhesive needs to have high adhesion, low volatile organic compound (VOC) content and good weather resistance.

[0050] The PET film has excellent visual transparency due to its high light transmittance. At the same time, its good tensile strength and wear resistance enhance the durability and service life of the film, ensuring stable performance in various application scenarios. The high adhesion of the high-solid content polyurethane adhesive ensures a strong bond between the backing layer and the substrate, improving the overall stability and reliability of the film. The low volatile organic compound (VOC) content meets environmental protection requirements and reduces potential harm to the environment and human body. The good weather resistance of the polyurethane adhesive enables the film to resist the influence of natural factors and maintain stable performance, which is particularly suitable for outdoor application scenarios.

[0051] Among them, when cleaning the substrate, pure water is used as the cleaning medium, and the cleaning time is 5 minutes. During the activation treatment, the treatment time is 30 seconds to increase its surface energy and enhance the adhesion performance with the backing layer.

[0052] Substrate cleaning uses pure water as the cleaning medium and thoroughly removes dust, oil and other impurities on the surface of the substrate within a specified time to ensure the cleanliness of the substrate surface. This step is the basis for ensuring good adhesion between the back adhesive layer and the substrate, avoiding poor adhesion caused by impurities. The activation treatment uses a specific process, such as using plasma treatment equipment to activate the surface of the cleaned substrate to increase the surface energy of the substrate. This process enhances the activity and wettability of the substrate surface, allowing the back adhesive layer to better bond with the substrate and improve the adhesion performance. This not only ensures a close bond between the back adhesive layer and the substrate, but also enhances the overall stability and durability of the diaphragm.

[0053] Among them, the mass ratio of polyurethane adhesive is 60%, the mass ratio of thickener, namely hydroxyethyl cellulose, is 5%, the mass ratio of antioxidant, namely antioxidant, is 2%, the mass ratio of solvent is 33%, and a mixed solvent of ethyl acetate and ethanol is used in a ratio of 2:1.

[0054] The high content of polyurethane adhesive ensures that the adhesive layer has excellent adhesion properties, enabling it to adhere firmly to various substrates. The addition of thickener adjusts the viscosity of the adhesive liquid, ensuring the uniformity of coating and the consistency of the thickness of the adhesive layer. The addition of antioxidant effectively prevents the oxidative degradation of the adhesive layer and extends the service life of the film. The use of a mixed solvent of ethyl acetate and ethanol not only ensures the full dissolution of the adhesive and additives, but also achieves rapid drying and curing of the adhesive liquid by adjusting the volatilization rate, avoiding defects in the drying process. In summary, this formula selection ensures the high quality, high performance and stability of the adhesive film.

[0055] When preparing the backing adhesive, the initial stirring speed of the stirring equipment is 500 rpm, and gradually increases to 1000 rpm, and the stirring time is a total of 40 minutes to ensure that the components are mixed evenly without particles and bubbles.

[0056] It ensures that the various components in the adhesive formula can be fully mixed and evenly formed to form a uniform adhesive liquid; secondly, long-term stirring and gradually increasing stirring speed help to eliminate particles and bubbles in the adhesive liquid, making the adhesive liquid more delicate and defect-free; finally, the adhesive liquid prepared in this way has better performance and can improve the overall quality of the adhesive film, including adhesion, appearance quality and usage experience.

[0057] During coating, the coating speed of the coater is 5m / min, and the coating thickness is controlled to be 20±2μm by adjusting the scraper gap of the coater. During drying and curing, the initial temperature of the drying chamber is 40°C, which is gradually increased to 60°C and maintained for 20 minutes to remove the solvent. Then, the curing stage is entered, and the temperature is gradually increased to 100°C and maintained for 30 minutes, and then increased to 120°C and maintained for 40 minutes. During the curing process, air circulation must be maintained to avoid excessive humidity affecting the curing effect.

[0058] The coater works at an appropriate coating speed, which not only ensures production efficiency, but also ensures the uniformity and stability of the coating; by accurately adjusting the scraper gap, the coating thickness is effectively controlled, further improving product quality. Temperature control is key in the drying and curing stages. The initial low temperature helps the solvent evaporate smoothly and avoid coating defects; the subsequent gradual increase in temperature promotes the curing of the coating, improving its hardness and wear resistance. Throughout the process, air circulation is maintained to avoid the influence of humidity on the curing effect. These steps together ensure the coating quality, physical properties and chemical stability of the adhesive-backed film, thereby producing high-performance adhesive-backed film products.

[0059] Among them, during environmental control, the temperature of the production workshop is controlled at 25±1℃ and the humidity is controlled at 50±3%RH.

[0060] First, it ensures the stability of product quality. By maintaining a stable physical and chemical environment, it avoids fluctuations in product quality caused by environmental changes. Secondly, such environmental control helps improve production efficiency, reduce equipment failures and operator fatigue. In addition, suitable temperature and humidity conditions can ensure operational safety and reduce potential safety risks. Finally, it also helps to extend the service life of production equipment and reduce equipment wear and aging caused by environmental factors.

[0061] During quality inspection, the prepared self-adhesive film is tested for adhesion, and a peeling test is performed using a standard tape to ensure that the adhesion meets the requirements. A weather resistance test is also performed, and the film is placed in a constant temperature and humidity chamber to simulate different climatic conditions and observe its performance changes. At the same time, a microscope is used to observe the surface of the film to ensure that there are no bubbles, impurities, or scratches.

[0062] Adhesion test, weather resistance test and microscope observation during the quality inspection process jointly ensure the excellent performance and quality of the adhesive film. Adhesion test ensures the film's stable adhesion to the target object, weather resistance test ensures the film's stable performance under various climatic conditions, and microscope observation ensures that the film surface is flawless, free of defects such as bubbles, impurities and scratches. These measures jointly improve the overall quality of the adhesive film and ensure its excellent performance in practical applications.

[0063] Among them, when packaging, qualified self-adhesive film sheets need to be cut according to specifications to ensure accurate size, and use anti-static packaging bags for packaging to ensure good sealing and avoid moisture and contamination. The product name, specifications, production date, and batch number must be marked on the packaging for easy traceability and management.

[0064] First, cutting according to specifications ensures the accuracy of product size and meets customer needs. Secondly, using anti-static packaging bags and ensuring good sealing effectively prevents static damage and moisture contamination, protecting the quality and performance of the product. Finally, marking detailed information on the packaging facilitates product traceability and management, improving the company's production efficiency and customer satisfaction. These measures jointly ensure the safety and integrity of the self-adhesive film during packaging, transportation and storage, providing companies with reliable product guarantees.

[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for preparing a stable adhesive-backed film, characterized in that: The steps include: S1: Raw material selection: base material, transparent PET (polyethylene terephthalate) film is used as base material, adhesive material, high solid content polyurethane (PU) adhesive is used as adhesive material; S2: pretreatment, substrate cleaning, cleaning the PET film with an ultrasonic cleaner, surface activation, and surface activation treatment of the cleaned PET film with a plasma treatment device; S3: Preparation of adhesive formula, which includes polyurethane adhesive, thickener, antioxidant and solvent; S4: Preparation of adhesive: In a clean mixing tank, add polyurethane adhesive, thickener, antioxidant and solvent in order according to the formula ratio, and start the mixing equipment. The prepared adhesive liquid needs to be filtered through a filter to remove possible impurities to ensure the coating quality; S5: Coating: Use a high-precision coating machine to evenly coat the prepared adhesive liquid on the pre-treated PET film. During the coating process, the environment must be kept clean to prevent dust and other impurities from falling in; S6: Drying and curing, sending the coated film into the drying room to remove the solvent and ensure that the adhesive layer is completely cured; S7: Environmental control. The production workshop is equipped with a constant temperature and humidity system to ensure a stable production environment. The air quality in the workshop is regularly tested to ensure that it is dust-free and odor-free. S8: Clean production. Regularly clean production equipment thoroughly, use special cleaning agents and dust-free cloths to ensure that there is no dust, oil or impurities on the equipment surface. Operators must wear anti-static work clothes and gloves, and must go through an air shower room for dust removal before entering the production workshop. S9: Quality inspection and packaging.

2. The process for preparing a stable adhesive-backed film according to claim 1, characterized in that: When the substrate is selected, the specification of the PET film is 0.1mm×1200mm, and it needs to have high light transmittance, good tensile strength and wear resistance. The high solid content polyurethane (PU) adhesive needs to have high adhesion, low volatile organic compound (VOC) content and good weather resistance.

3. The process for preparing a stable adhesive-backed film according to claim 1, characterized in that: When the substrate is cleaned, pure water is used as the cleaning medium, and the cleaning time is 5 minutes. During the activation treatment, the treatment time is 30 seconds to increase its surface energy and enhance the adhesion performance with the back adhesive layer.

4. The process for preparing a stable adhesive-backed film according to claim 1, characterized in that: The mass ratio of the polyurethane adhesive is 60%, the mass ratio of the thickener, namely hydroxyethyl cellulose, is 5%, the mass ratio of the antioxidant, namely the antioxidant, is 2%, the mass ratio of the solvent is 33%, and a mixed solvent of ethyl acetate and ethanol is used in a ratio of 2:

1.

5. The process for preparing a stable adhesive-backed film according to claim 1, characterized in that: When preparing the back adhesive, the initial stirring speed of the stirring device is 500 rpm, and is gradually increased to 1000 rpm, and the stirring time is 40 minutes in total to ensure that the components are mixed evenly without particles and bubbles.

6. The process for preparing a stable adhesive-backed film according to claim 1, characterized in that: During the coating, the coating speed of the coater is 5m / min, and the coating thickness is controlled to be 20±2μm by adjusting the scraper gap of the coater. During the drying and curing, the initial temperature of the drying chamber is 40°C, which is gradually increased to 60°C and maintained for 20 minutes to remove the solvent. Then, the curing stage is entered, and the temperature is gradually increased to 100°C and maintained for 30 minutes, and then increased to 120°C and maintained for 40 minutes. Air circulation must be maintained during the curing process to avoid excessive humidity affecting the curing effect.

7. The process for preparing a stable adhesive-backed film according to claim 1, characterized in that: During the environmental control, the temperature of the production workshop is controlled at 25±1°C, and the humidity is controlled at 50±3%RH.

8. The process for preparing a stable adhesive-backed film according to claim 1, characterized in that: During the quality inspection, the prepared adhesive-backed film is subjected to an adhesion test, a peeling test is performed using a standard tape to ensure that the adhesion meets the requirements, and a weather resistance test is performed. The film is placed in a constant temperature and humidity chamber to simulate different climatic conditions and its performance changes are observed. At the same time, the surface of the film is observed using a microscope to ensure that there are no bubbles, impurities, or scratches.

9. The process for preparing a stable adhesive-backed film according to claim 1, characterized in that: When packaging, the qualified self-adhesive film sheets must be cut according to specifications to ensure accurate size, and packaged in anti-static packaging bags to ensure good sealing and avoid moisture and contamination. The product name, specifications, production date, and batch number must be marked on the packaging for easy traceability and management.

Citation Information

Cited By

  • Preparation method of reticulated protective film

    CN121131209A