Composite binder, solid electrolyte film, electrode plate, solid-state battery and preparation method of solid-state battery

Through the composite binder modified by the double-layer polymer, the problem of difficulty in preparing thin films of inorganic solid electrolytes is solved, and an all-solid state battery with high energy density and high safety is realized, which simplifies the preparation process and reduces costs.

CN118995085APending Publication Date: 2024-11-22JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411097089.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Commercial inorganic solid electrolytes are difficult to prepare thin electrolyte membranes with thicknesses less than 200μm, resulting in huge challenges in large-scale production. The energy density and safety of existing solid-state batteries are insufficient, making it difficult to meet new energy needs.

Method used

Compound adhesives modified with double-layer polymers, including polytetrafluoroethylene and surface double-layer polymers, inner polydopamine enhances bonding capacity, outer polyethylene oxide expands Li+ transport channels, connected by hydrogen bonds Improves bonding performance and is used to prepare solid electrolytes and electrode sheets to achieve high stability and high energy density all-solid state batteries.

Benefits of technology

It improves the ionic conductivity and flexibility of solid electrolytes, simplifies the preparation process, reduces costs, is suitable for large-scale production, and improves the cycling performance and energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995085A_ABST
    Figure CN118995085A_ABST
Patent Text Reader

Abstract

The invention provides a double-layer polymer modified composite binder, a solid electrolyte film, an electrode plate, a solid-state battery and a preparation method thereof. The composite binder provided by the invention is a double-layer polymer modified polytetrafluoroethylene binder, and the inner-layer polydopamine contains polar groups such as amido, hydroxyl and the like, so that the binding capacity of polytetrafluoroethylene is improved; after the flexible polyethylene oxide on the outer layer is in contact with the high-hardness inorganic solid electrolyte, the flexibility and the machinability of the electrolyte are improved. The two layers of polymers are connected through hydrogen bonds and are in close contact, so that the intermolecular acting force is enhanced, and the adhesive property of polytetrafluoroethylene in the dry-method solid electrolyte can be improved. The composite binder can be used for preparing a solid electrolyte and an electrode plate, so that the stability of the device is improved, the preparation process is simplified, the preparation cost is reduced, and large-scale production is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid electrolytes, and in particular to a double-layer polymer-modified composite binder, a solid electrolyte film, an electrode sheet, a solid-state battery and a preparation method thereof. Background Art

[0002] In recent years, people have an increasing demand for new energy power supply devices represented by lithium batteries, and their performance requirements are also getting higher and higher.

[0003] Solid-state batteries can provide higher energy and higher safety. However, commercial inorganic solid electrolytes (bulk modulus of about 100 GPa, Young's modulus of about 150 GPa) are difficult to prepare thin electrolyte membranes less than 200 μm thick, and face huge challenges in large-scale production. Therefore, it is urgent to develop new solid electrolytes with excellent processing performance and high Li + The solid electrolyte with high conductivity is combined with a new solid-state battery preparation process (thin electrolyte / thick electrode manufacturing method) to achieve high safety and high energy density (>350wh kg -1 )The preparation of all-solid-state batteries will further accelerate the development and application of new energy around the world. Summary of the invention

[0004] Based on this, the present invention provides a double-layer polymer modified composite binder, solid electrolyte film, electrode sheet, solid-state battery and its preparation method. The composite binder provided by the present invention comprises polytetrafluoroethylene and a double-layer polymer on the surface. The inner layer of polydopamine has a strong adhesion and can improve the bonding ability of polytetrafluoroethylene; the outer layer of branched polyethylene oxide can expand Li + Transmission channel, after polyethylene oxide contacts with high-hardness inorganic solid electrolyte, the flexibility and processability of electrolyte are increased. The two layers of polymer are connected by hydrogen bonds, the two layers of polymer are in close contact, the intermolecular force is enhanced, and the bonding performance of polytetrafluoroethylene in dry solid electrolyte is improved. When the composite binder is used to prepare solid electrolyte and electrode sheet, it can improve the stability of the device.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a double-layer polymer-modified composite adhesive, comprising the following steps:

[0007] A. Preparation of polydopamine-coated polytetrafluoroethylene binder:

[0008] A1. Pre-treating polytetrafluoroethylene with a potassium permanganate / nitric acid mixed solution to form hydrophilic manganese oxide or manganese hydroxide covering polytetrafluoroethylene particles;

[0009] A2, adding dopamine monomer and potassium permanganate in proportion to an alkaline solution with a pH of 8.5, and then slowly adding the polytetrafluoroethylene pretreated in step A1 to carry out a polymerization reaction. After the reaction is completed, the mixture is filtered and ultrasonically washed with deionized water and then vacuum dried to obtain a polydopamine-coated polytetrafluoroethylene binder;

[0010] B. Preparation of double-layer polymer-modified polytetrafluoroethylene binder:

[0011] B1. Add initiator diphenylmethyl potassium, ethylene oxide, 1-ethoxy glycidyl ether monomer and tetrahydrofuran solvent to a dry and clean flask respectively, heat and stir and transfer to a reaction kettle to obtain a hydrophilic polymer Poly (EO-co-EEGE) with polyethylene oxide as the main chain and hydroxyl groups on the side chain;

[0012] B2. Add the polydopamine-coated polytetrafluoroethylene binder obtained in step A into a reaction kettle, and finally add a small amount of anhydrous methanol. After cooling, remove tetrahydrofuran at normal pressure, dissolve the crude product in anhydrous ethanol, wash, filter and spin dry, and vacuum dry to obtain a double-layer polymer-modified polytetrafluoroethylene binder.

[0013] Furthermore, in the step A1, the molar ratio of potassium permanganate to nitric acid is 3:1; in the step A2, the molar ratio of potassium permanganate to dopamine monomer is 6:4; and in the step B1, the molar ratio of ethylene oxide to 1-ethoxyglycidyl ether monomer is 2:1.

[0014] Furthermore, in the step A1, based on the total mass of the single-layer polymer-modified polytetrafluoroethylene binder, the mass proportion of the polydopamine is 1 to 30%.

[0015] Furthermore, in the step A2, the polymerization reaction temperature is 0 to 40° C. and the reaction time is 24 to 48 hours.

[0016] Furthermore, in the step B1, based on the total mass of the double-layer polymer-modified polytetrafluoroethylene binder, the mass proportion of the hydrophilic polymer is 1 to 30%.

[0017] Furthermore, in the step B1, the ratio of the monomers ethylene oxide and 1-ethoxyglycidol is 2:1; the temperature of the anionic polymerization reaction is 0°C to 60°C, and the time is 1h to 48h.

[0018] The second aspect of the present invention provides a double-layer polymer-modified composite adhesive, which is prepared by the method described in the above technical solution. Preferably, the adhesive particles have a size of 10-800 μm.

[0019] The third aspect of the present invention provides a solid electrolyte film, which is prepared by proportioning an inorganic solid electrolyte and a double-layer polymer-modified composite binder; preferably, the inorganic solid electrolyte is lithium lanthanum zirconium oxide.

[0020] In a fourth aspect, the present invention provides a method for preparing a solid electrolyte film, comprising the following steps:

[0021] Step 1, uniformly mixing the lithium lanthanum zirconium oxygen inorganic solid electrolyte and the double-layer polymer-modified polytetrafluoroethylene composite adhesive in a mass ratio of (99-97%): (1-3%);

[0022] Step 2: ball milling the obtained mixture powder for 3 minutes to obtain microfibrillated mixture powder;

[0023] Step 3: The microfibrillated mixture powder is subjected to bidirectional rolling using a double-roller press at a set rolling temperature to fully fiberize the binder to obtain a solid electrolyte film; the rolling temperature is 25 to 80°C.

[0024] In a fifth aspect, the present invention provides an electrode sheet, which includes a current collector and an active layer on the surface of the current collector, wherein the active layer includes electrode active material, conductive carbon and a double-layer polymer-modified composite binder; the double-layer polymer-modified composite binder accounts for 3 to 10% of the mass of the active layer.

[0025] Furthermore, the electrode active material includes a positive electrode active material or a negative electrode active material. Positive electrode active materials include but are not limited to lithium iron phosphate (LiFePO4), lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium nickel cobalt manganese oxide (LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2) at least one; the negative electrode active material includes but is not limited to at least one of lithium metal, carbon-based, and silicon-based negative electrode active materials.

[0026] Furthermore, the silicon-based negative electrode active material includes a silicon-oxygen negative electrode material: the molecular formula is SiOx, and x is any value from 0 to 2. Non-limiting examples include: silicon dioxide and silicon dioxide.

[0027] Furthermore, the carbon-based negative electrode active material can adopt the carbon negative electrode material commonly used in the art, including but not limited to: at least one of mesophase carbon microbeads, natural graphite, artificial graphite, graphene, glassy carbon, carbon nanotubes, carbon fiber, hard carbon, and soft carbon.

[0028] Furthermore, the active layer also includes conductive carbon, and the conductive carbon includes but is not limited to at least one of graphite, carbon nanotubes, nanofibers, carbon black and graphene.

[0029] Furthermore, the thickness of the active layer is 50 μm to 200 μm, for example, 50 μm, 100 μm, 150 μm or 200 μm.

[0030] Furthermore, the current collector adopts a current collector commonly used in the art, such as copper foil, aluminum foil, etc.

[0031] The sixth aspect of the present invention provides a solid-state battery, the battery comprising the solid electrolyte film provided in the third aspect and the electrode sheet described in the fifth aspect.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] 1. The outer layer of the composite binder provided by the present invention is a branched polyethylene oxide, which has polyethylene oxide as the main chain and hydroxyl groups on the side chains, and is in contact with the inorganic solid electrolyte. Compared with the inorganic-inorganic phase, the Li + Transmission channel to improve the ionic conductivity of dry solid electrolytes;

[0034] 2. In the present invention, the KMnO4 / HNO3 mixed solution pre-treats polytetrafluoroethylene to improve the hydrophilicity of PTFE and increase the subsequent coating area of ​​polydopamine. Polydopamine contains polar groups such as amino groups and hydroxyl groups, which improve the bonding ability of polytetrafluoroethylene.

[0035] 3. The two layers of polymers in the composite binder provided by the present invention are connected by hydrogen bonds, the two layers of polymers are in close contact, the intermolecular force is enhanced, and the bonding performance of polytetrafluoroethylene in the dry solid electrolyte is improved;

[0036] 4. The composite binder provided by the present invention can be used to prepare electrode sheets by a dry method, that is, electrode sheets can be prepared without adding a solvent, which can simplify the preparation process, reduce the preparation cost, and facilitate large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0038] Figure 1 This is the reaction route of the polydopamine layer of the composite adhesive prepared in Example 1;

[0039] Figure 2 This is the reaction route of the composite adhesive outer layer polymer Poly (EO-co-EEGE) prepared in Example 1;

[0040] Figure 3 Schematic diagram of obtaining a solid electrolyte film by fiberizing a composite binder in Example 1 of the present invention;

[0041] Figure 4 It is a physical picture of the solid electrolyte film obtained by fiberizing the composite binder in Example 1 of the present invention and its thickness test;

[0042] Figure 5 is a scanning electron microscope (SEM) image of a solid electrolyte film obtained by fiberizing a composite binder in Example 1 of the present invention;

[0043] Figure 6 is an impedance diagram of the calculated ionic conductivity of the solid electrolyte film obtained by fiberizing the composite binder in Example 1 of the present invention;

[0044] Figure 7 is an electrolyte / electrode stability diagram of a solid electrolyte film obtained by fiberizing a composite binder in Example 1 of the present invention;

[0045] Figure 8 This is a charge and discharge comparison diagram of a solid-state battery prepared by the composite binder in Example 1 of the present invention and a pure PTFE solid-state battery;

[0046] Fig. 9 This is a comparison chart of the coulombic efficiency of the solid-state battery prepared by the composite binder in Example 1 of the present invention and the pure PTFE solid-state battery in the first three cycle tests. DETAILED DESCRIPTION

[0047] The technical solutions in the embodiments of the present invention are described clearly and completely below. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. For greater clarity, the following embodiments are described in detail below.

[0048] Embodiment 1

[0049] This embodiment provides a synthesis of a double-layer polymer-modified composite binder, comprising the following steps:

[0050] Step 1: Pretreatment of polytetrafluoroethylene (PTFE). The specific operation is: potassium permanganate (KMnO4) / nitric acid (HNO3) is used as a pretreatment agent, wherein KMnO4:HNO3=3:1 (stoichiometric ratio). Add 12.00g (6.02wt%) KMnO4 to 200mL of distilled water and then add HNO3 (68wt%). Continue stirring at room temperature for 30 minutes to completely dissolve the potassium permanganate. Then, 50.00g of PTFE particles are immersed in the mixed solvent, and the flask is placed in a 60°C water bath for 3 hours.

[0051] Step 2: Polymerize dopamine monomer on the PTFE surface. The specific reaction route is as follows: Figure 1 As shown. The specific operation is: add tris(hydroxymethyl)aminomethane salt to the dopamine salt solution, adjust the pH to 8.5, and use KMnO4 that can accelerate the polymerization of dopamine as an oxidant. Add 0.04 mol of KMnO4 solid and 0.027 mol of dopamine monomer to the above alkaline solvent. Then slowly add 15.00 g of polytetrafluoroethylene pretreated in step 1. At 0°C, stir at high speed for 24 hours. After the reaction is completed, wash the obtained solid with water several times until the filtrate is clear and transparent, and then dry it under vacuum conditions at 100°C for 12 hours to obtain a single-layer polydopamine (PDA) modified composite adhesive.

[0052] Step 3: Polymerize ethylene oxide monomer and 1-ethoxy glycidyl ether monomer on the surface of PDA-modified PTFE. The specific reaction route is as follows: Figure 2 As shown. The specific operation is: at 0°C, add 2mL of diphenylmethyl potassium (DPMK, 0.002mol), 50mL of tetrahydrofuran solvent, 0.081mol of ethylene oxide and 0.040mol of 1-ethoxyglycidyl ether to a dry and clean flask, mix for 1h, and heat to 60°C. Transfer to the reactor and wait until the pressure inside the reactor becomes negative pressure. Add 11.93g of the single-layer PDA modified PTFE in step 2, and finally add a small amount of anhydrous methanol to terminate the reaction. After cooling, remove tetrahydrofuran at normal pressure, dissolve the crude product in anhydrous ethanol, wash, filter and dry, and vacuum dry at 60°C for 24 hours to obtain a polytetrafluoroethylene composite adhesive modified with an outer layer polymer Poly (EO-co-EEGE) and an inner layer polydopamine (PDA).

[0053] Embodiment 2

[0054] This embodiment provides a synthesis of a double-layer polymer-modified composite binder, comprising the following steps:

[0055] Step 1: Pretreatment of polytetrafluoroethylene (PTFE). The specific operation is: potassium permanganate (KMnO4) / nitric acid (HNO3) is used as a pretreatment agent, wherein KMnO4:HNO3=3:1 (stoichiometric ratio). Add 12.00g (6.02wt%) KMnO4 to 200mL of distilled water and then add HNO3 (68wt%). Continue stirring at room temperature for 30 minutes to completely dissolve the potassium permanganate. Then, 50.00g of PTFE particles are immersed in the mixed solvent, and the flask is placed in a 60°C water bath for 3 hours.

[0056] Step 2: Polymerize dopamine monomer on the PTFE surface. The specific reaction route is as follows: Figure 1 As shown. The specific operation is: add tris(hydroxymethyl)aminomethane salt to the dopamine salt solution, adjust the pH to 8.5, and use KMnO4 that can accelerate the polymerization of dopamine as an oxidant. Add 0.04 mol of KMnO4 solid and 0.009 mol of dopamine monomer to the above alkaline solvent. Then slowly add 15.00 g of polytetrafluoroethylene pretreated in step 1. At 0°C, stir at high speed for 24 hours. After the reaction is completed, wash the obtained solid with water several times until the filtrate is clear and transparent, and then dry it under vacuum conditions at 100°C for 12 hours to obtain a single-layer polydopamine (PDA) modified composite adhesive.

[0057] Step 3: Polymerize ethylene oxide monomer and 1-ethoxy glycidyl ether monomer on the surface of PDA-modified PTFE. The specific reaction route is as follows: Figure 2 As shown. The specific operation is: at 0°C, add 2mL of diphenylmethyl potassium (DPMK, 0.002mol), 50mL of tetrahydrofuran solvent, 0.081mol of ethylene oxide and 0.040mol of 1-ethoxyglycidyl ether to a dry and clean flask, mix for 1h, and heat to 60°C. Transfer to the reactor and wait until the pressure inside the reactor becomes negative pressure. Add 11.93g of the single-layer PDA modified PTFE in step 2, and finally add a small amount of anhydrous methanol to terminate the reaction. After cooling, remove tetrahydrofuran at normal pressure, dissolve the crude product in anhydrous ethanol, wash, filter and dry, and vacuum dry at 60°C for 24 hours to obtain a polytetrafluoroethylene composite adhesive modified with an outer layer polymer Poly (EO-co-EEGE) and an inner layer polydopamine (PDA).

[0058] Embodiment 3

[0059] This embodiment provides a synthesis of a double-layer polymer-modified composite binder, comprising the following steps:

[0060] Step 1: Pretreatment of polytetrafluoroethylene (PTFE). The specific operation is: potassium permanganate (KMnO4) / nitric acid (HNO3) is used as a pretreatment agent, wherein KMnO4:HNO3=3:1 (stoichiometric ratio). Add 12.00g (6.02wt%) KMnO4 to 200mL of distilled water and then add HNO3 (68wt%). Continue stirring at room temperature for 30 minutes to completely dissolve the potassium permanganate. Then, 50.00g of PTFE particles are immersed in the mixed solvent, and the flask is placed in a 60°C water bath for 3 hours.

[0061] Step 2: Polymerize dopamine monomer on the PTFE surface. The specific reaction route is as follows: Figure 1 As shown. The specific operation is: add tris(hydroxymethyl)aminomethane salt to the dopamine salt solution, adjust the pH to 8.5, and use KMnO4 that can accelerate the polymerization of dopamine as an oxidant. Add 0.04 mol of KMnO4 solid and 0.027 mol of dopamine monomer to the above alkaline solvent. Then slowly add 15.00 g of polytetrafluoroethylene pretreated in step 1. At 0°C, stir at high speed for 24 hours. After the reaction is completed, wash the obtained solid with water several times until the filtrate is clear and transparent, and then dry it under vacuum conditions at 100°C for 12 hours to obtain a single-layer polydopamine (PDA) modified composite adhesive.

[0062] Step 3: Polymerize ethylene oxide monomer and 1-ethoxy glycidyl ether monomer on the surface of PDA-modified PTFE. The specific reaction route is as follows: Figure 2 As shown. The specific operation is: at 0°C, add 2mL of diphenylmethyl potassium (DPMK, 0.002mol), 50mL of tetrahydrofuran solvent, 0.027mol of ethylene oxide and 0.013mol of 1-ethoxyglycidyl ether to a dry and clean flask, mix for 1h, and heat to 60°C. Transfer to the reactor and wait until the pressure inside the reactor becomes negative pressure. Add 11.93g of the single-layer PDA modified PTFE in step 2, and finally add a small amount of anhydrous methanol to terminate the reaction. After cooling, remove tetrahydrofuran at normal pressure, dissolve the crude product in anhydrous ethanol, wash, filter and dry, and vacuum dry at 60°C for 24 hours to obtain a polytetrafluoroethylene composite adhesive modified with an outer layer polymer Poly (EO-co-EEGE) and an inner layer polydopamine (PDA).

[0063] Embodiment 4

[0064] The present embodiment provides a synthesis of a solid electrolyte film, comprising the following steps: uniformly mixing a lithium lanthanum zirconium oxide inorganic solid electrolyte (LLZTO) and a double-layer polymer-modified polytetrafluoroethylene composite binder at a mass ratio of 97:3. Subsequently, the obtained mixture powder is ball-milled for 3 minutes to obtain a microfibrillated mixture powder. Finally, the obtained microfibrillated mixture powder is rolled 20 times in a bidirectional double-roll roller press at 80°C to obtain a 100μm solid electrolyte film.

[0065] Embodiment 5

[0066] The present embodiment provides a synthesis of a solid electrolyte film, comprising the following steps: uniformly mixing a lithium lanthanum zirconium oxide inorganic solid electrolyte (LLZTO) and a double-layer polymer-modified polytetrafluoroethylene composite adhesive at a mass ratio of 97:3. Subsequently, the obtained mixture powder is ball-milled for 3 minutes to obtain a microfibrillated mixture powder. Finally, the obtained microfibrillated mixture powder is set at 80°C with a double roller distance of 150 μm on a roller press, and the 150 μm solid electrolyte film is obtained by rolling the roller press 20 times in a bidirectional manner.

[0067] Embodiment 6

[0068] The present embodiment provides a synthesis of a solid electrolyte film, comprising the following steps: uniformly mixing a lithium lanthanum zirconium oxide inorganic solid electrolyte (LLZTO) and a double-layer polymer-modified polytetrafluoroethylene composite binder at a mass ratio of 97:3. Subsequently, the obtained mixture powder is ball-milled for 3 minutes to obtain a microfibrillated mixture powder. Finally, the obtained microfibrillated mixture powder is rolled 20 times in a bidirectional double-roll roller press at room temperature to obtain a 100 μm solid electrolyte film.

[0069] Embodiment 7

[0070] The present embodiment provides a method for preparing a battery cell, comprising the following steps: mixing lithium iron phosphate LiFePO4, conductive carbon Super P and a double-layer polymer-modified polytetrafluoroethylene composite adhesive at a ratio of 87:10:3 at 25°C for 2 hours to prepare an active mixture, and mixing at 25°C for 20 minutes to prepare a powdered mixture; hot-rolling the powdered mixture at 120°C into an active layer with a thickness of 80 μm and placing it on a current collector to obtain a positive electrode sheet.

[0071] Embodiment 8

[0072] The present embodiment provides a method for preparing a battery cell, comprising the following steps: mixing lithium iron phosphate LiFePO4, conductive carbon Super P and a double-layer polymer-modified polytetrafluoroethylene composite adhesive in a ratio of 80:10:10 at 25°C for 2 hours to prepare an active mixture, and mixing at 25°C for 20 minutes to prepare a powdered mixture; hot-rolling the powdered mixture at 120°C into an active layer with a thickness of 80 μm and placing it on a current collector to obtain a positive electrode sheet.

[0073] Embodiment 9

[0074] This embodiment provides an assembly of a solid-state battery, comprising the following steps: using the solid electrolyte film prepared by the double-layer polymer-modified composite adhesive in embodiment 4 as the solid electrolyte of the battery, using the electrode sheet prepared in embodiment 7 as the positive electrode of the battery, and the metal Li sheet as the negative electrode of the battery. Using a CR2032 button battery shell, the solid-state battery is assembled in the order of positive electrode-solid electrolyte-negative electrode.

[0075] Comparative Example 1

[0076] Comparative Example 1 is substantially the same as Example 9, except that the double-layer polymer-modified PTFE composite adhesive in Example 9 is replaced by a single-layer polydopamine-modified PTFE composite adhesive. See Table 1 for specific test conditions.

[0077] Comparative Example 2

[0078] Comparative Example 2 is substantially the same as Example 9, except that the double-layer polymer-modified PTFE composite adhesive in Example 9 is replaced with PTFE without any modification. See Table 1 for specific test conditions.

[0079] Embodiment 10

[0080] The solid electrolyte film in the fourth embodiment of the present invention is characterized by Figure 3 It can be seen that the fibers penetrate the solid electrolyte particles as a whole. Figure 4 It can be seen that the solid electrolyte film is 100 μm thick and has a smooth surface. Figure 5 It can be seen that at a scale of 50 μm, the composite adhesive can be clearly observed to be in the form of interlaced fibers.

[0081] Embodiment 11

[0082] The solid electrolyte film assembly of the fourth embodiment of the present invention is used to assemble a stainless steel sheet / solid electrolyte film / stainless steel sheet battery, and the ionic conductivity (σ) is tested using the formula: σ = L / (A*R), where L is the thickness of the solid electrolyte film 100 μm, A is a fixed value of 2, and R is obtained based on the impedance test. Figure 6 It can be seen that the impedance value is 2.38Ω. Please see Table 1 for specific σ.

[0083] The preparation conditions and proportions of representative embodiments and comparative examples are shown in Table 1.

[0084] Table 1

[0085]

[0086]

[0087] Note: “ / ” means the substance does not exist.

[0088] From the data in Table 1 and Figure 6 It can be seen that when the composite binder prepared by the technical solution of the present application is used to prepare a solid electrolyte, the ionic conductivity of the solid electrolyte can be improved. The ionic conductivity is obtained according to the impedance. The impedance test shows that Figure 6 , and the stability of the electrode sheet can be improved when preparing the electrode sheet, thereby improving the cycle performance of the battery.

[0089] Comparing Example 9 with Comparative Example 1, the results of electrolyte / electrode stability are as follows: Figure 7 The overpotential of the ninth embodiment is smaller, and the ability to improve the cycle stability of the battery is stronger.

[0090] Comparing Example 9 with Comparative Example 2, the charge-discharge redox reversibility of the battery is as follows: Figure 8 As shown in FIG. 1 , the charge-discharge reversibility of Example 9 is higher, and the discharge specific capacity is larger, which is close to the theoretical capacity of 170 mAh g -1 The Coulomb efficiency is Fig. 9 As shown, the coulombic efficiency of the battery in Example 9 in the first three cycles is higher than that of the battery in Comparative Example 2.

[0091] The composite binder uses a dry process to prepare electrolytes and electrode sheets without adding solvents, which greatly simplifies the preparation process, reduces preparation costs, and is conducive to large-scale production.

[0092] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0093] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a double-layer polymer-modified composite adhesive, characterized in that: The steps include: A. Preparation of polydopamine-coated polytetrafluoroethylene binder: A1. Pre-treating polytetrafluoroethylene with a potassium permanganate / nitric acid mixed solution to form hydrophilic manganese oxide or manganese hydroxide covering polytetrafluoroethylene particles; A2, adding dopamine monomer and potassium permanganate in proportion to an alkaline solution with a pH of 8.5, and then slowly adding the polytetrafluoroethylene pretreated in step A1 to carry out a polymerization reaction. After the reaction is completed, the mixture is filtered and ultrasonically washed with deionized water and then vacuum dried to obtain a polydopamine-coated polytetrafluoroethylene binder; B. Preparation of double-layer polymer-modified polytetrafluoroethylene binder: B1. Add initiator diphenylmethyl potassium, ethylene oxide, 1-ethoxy glycidyl ether monomer and tetrahydrofuran solvent to a dry and clean flask respectively, heat and stir and transfer to a reaction kettle to obtain a hydrophilic polymer with polyethylene oxide as the main chain and hydroxyl groups on the side chain; B2. Add the polydopamine-coated polytetrafluoroethylene binder obtained in step A into a reaction kettle, and finally add a small amount of anhydrous methanol. After cooling, remove tetrahydrofuran at normal pressure, dissolve the crude product in anhydrous ethanol, wash, filter and spin dry, and vacuum dry to obtain a double-layer polymer-modified polytetrafluoroethylene binder.

2. The method for preparing a double-layer polymer-modified composite adhesive according to claim 1, characterized in that: The molar ratio of potassium permanganate to nitric acid in step A1 is 3:1; the molar ratio of potassium permanganate to dopamine monomer in step A2 is 6:4; and the molar ratio of ethylene oxide to 1-ethoxyglycidyl ether monomer in step B1 is 2:

1.

3. The method for preparing a double-layer polymer-modified composite adhesive according to claim 1, characterized in that: In the step A1, based on the total mass of the single-layer polymer-modified polytetrafluoroethylene binder, the mass proportion of the polydopamine is 1 to 30%.

4. The method for preparing a double-layer polymer modified dry binder according to claim 1, characterized in that: In the step B1, based on the total mass of the double-layer polymer-modified polytetrafluoroethylene binder, the mass proportion of the hydrophilic polymer is 1-30%.

5. A double-layer polymer-modified composite adhesive, characterized in that: The binder is obtained by the preparation method according to any one of claims 1 to 4; The particle size of the binder is 10-800 μm.

6. A solid electrolyte film, characterized in that: The solid electrolyte film is prepared by proportioning an inorganic solid electrolyte and a double-layer polymer-modified composite binder as described in claim 5; the inorganic solid electrolyte is lithium lanthanum zirconium oxide; and the thickness of the solid electrolyte film is 100 to 200 μm.

7. The method for preparing a solid electrolyte film according to claim 6, characterized in that: The following steps are involved: Step 1, uniformly mixing the lithium lanthanum zirconium oxygen inorganic solid electrolyte and the double-layer polymer-modified polytetrafluoroethylene composite adhesive in a mass ratio of (99-97%): (1-3%); Step 2: ball milling the obtained mixture powder for 3 minutes to obtain microfibrillated mixture powder; Step 3: The microfibrillated mixture powder is subjected to bidirectional rolling using a double-roller press at a set rolling temperature to fully fiberize the binder to obtain a solid electrolyte film; the rolling temperature is 25 to 80°C.

8. An electrode sheet, characterized in that: The electrode sheet comprises a current collector and an active layer on the surface of the current collector, wherein the active layer comprises an electrode active material, conductive carbon and the double-layer polymer-modified composite binder according to claim 5; the double-layer polymer-modified composite binder accounts for 3-10% of the mass of the active layer.

9. A solid-state battery, characterized in that: The battery comprises the solid electrolyte film according to claim 6 and the electrode sheet according to claim 8.