Divalent europium-doped silicate fluorescent powder and preparation method thereof
By doping Li, Na or K ions in A2SiO5, the reduction of Eu3+ to Eu2+ is promoted, and the problem of difficulty in achieving luminescence in the trivalent cation lattice is solved, and the development of high-performance rare earth luminescent materials is realized, with excellent fluorescence Effects and simple preparation method.
Patent Information
- Application Number
- CN202411078964.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
In the A2SiO5 (A=Y, La or Lu) system, it is difficult for Eu2+ ions to maintain a low valence state, resulting in almost blank Eu2+ luminescence research, and Eu2+ is difficult to achieve luminescence in the trivalent cation lattice.
By doping Li, Na or K ions in the silicate phosphor, additional valence electrons are generated to promote the reduction of Eu3+ to Eu2+ and luminescence of Eu2+ is achieved in A2SiO5 with trivalent cationic lattice.
It successfully exists stably in the trivalent cation lattice and realizes the luminescence of Eu2+, and develops a high-performance rare earth luminescent material with excellent fluorescence effect and a simple and easy preparation method.
Smart Images

Figure HDA0004983169440000011 
Figure HDA0004983169440000012 
Figure HDA0004983169440000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of luminescent materials, and in particular relates to a silicate phosphor doped with divalent europium and a preparation method thereof. Background Art
[0002] Rare earth luminescent materials are one of the core materials for realizing high added value utilization of rare earth raw materials in my country, and are widely used in lighting, display, biomedicine, anti-counterfeiting and detection. Rare earth luminescent materials are usually composed of inorganic compound matrix and doped rare earth luminescent ions. Their luminescence mechanism is mainly based on the transition of rare earth 4f electrons within ff configuration or between fd configurations. 2+ / Ce 3+ The ion has the characteristics of 4f-5d electron transition. Since its 5d electron is exposed, it is easily affected by the crystal field. It can achieve multi-color luminescence with different bandwidths through component substitution, structural modulation and coordination environment regulation. 2+ / Ce 3+ Activated rare earth luminescent materials can meet various application requirements. 2 SiO 5 (A=Y, La or Lu) is an important luminescent matrix system and has broad application prospects in the field of luminescent materials. 2 SiO 5 For example, Lu 2 SiO 5 :Ce 3+ It is a commercial scintillating material with excellent performance, high density, high light yield, and fast decay time, and is widely used in various radiation detectors and sensors. 2 SiO 5 No Eu 2+ Since the cationic lattice of this type of matrix is Lu, which is a trivalent ion, Eu doping into this type of matrix usually presents a trivalent ion and is difficult to reduce to a divalent ion. 2+ It is also difficult for ions to remain in a low valence state without being oxidized. 2 SiO 5 (A=Y, La or Lu) system, Eu 2+ There is almost no research on luminescence. 3+ ions, Eu ions occupying the same lattice site in the same matrix material 2+ ions will exhibit longer-wavelength emission if Eu 2+ The doping of ions is expected to develop high-performance rare earth luminescent materials. Summary of the invention
[0003] In view of the above-mentioned prior art, the present invention provides a silicate phosphor doped with divalent europium and a preparation method thereof, which solves the problem that it is difficult to realize Eu in a silicate phosphor having only trivalent cation sites that can be replaced by Eu ions. 2+ Glowing question.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a silicate phosphor doped with divalent europium, the chemical formula of the silicate phosphor is A 2 SiO 5 :aM + ,bEu 2+ , wherein A is Y, La or Lu, M is Li, Na or K, 0.4≤a≤1.8, 0.001≤b≤0.1.
[0005] The beneficial effects of the present invention are as follows: the present invention introduces Li, Na or K into A 2 SiO 5 The interstitial sites generate additional valence electrons to promote Eu 3+ Reduction to Eu 2+ , effectively stabilize Eu 2+ In M 3+ The presence of trivalent cation sites in A 2 SiO 5 Eu 2+ The glow.
[0006] Based on the above technical solution, the present invention can also be improved as follows.
[0007] Further, 1≤a≤1.4, 0.005≤b≤0.03.
[0008] The beneficial effect of adopting the further technical solution is: optimizing the raw material ratio so that the silicate phosphor has a better fluorescent effect.
[0009] The present invention also discloses a method for preparing a divalent europium-doped silicate phosphor, comprising the following steps:
[0010] S1: weighing raw materials according to the ratio of each element in the chemical formula of silicate phosphor except Si element, with Si in excess of one time, and grinding and mixing the raw materials to obtain a mixed material;
[0011] S2: keeping the mixture at 1200-1400°C in a reducing atmosphere for 3-9 hours, and then cooling to obtain a crude product;
[0012] S3: grinding, acid washing and drying the crude product to obtain a silicate phosphor doped with divalent europium;
[0013] The raw materials are oxides or nitrates of Y, La or Lu, carbonates of Li, Na or K, and silicon dioxide or silicic acid.
[0014] The beneficial effect of the present invention is that the preparation method provided by the present invention promotes Eu by doping alkali metal into the interstitial lattice to generate additional valence electrons. 3+ Reduction to Eu 2+ , the Eu2+ emission of A2SiO5 is realized, and the preparation method provided by the present invention is simple and easy, suitable for production, and has excellent process prospects.
[0015] Furthermore, the reducing atmosphere is CO gas or N 2 / H 2 Mixed gases.
[0016] Further, N 2 / H 2 N in mixed gas 2 and H 2 The volume ratio is 4:1.
[0017] The beneficial effect of adopting a further technical solution is that high-valent rare earth ions can be reduced to low-valent states by calcining in a suitable reducing atmosphere, and calcining in a reducing atmosphere can reduce the formation of oxygen defects, so that the final silicate phosphor has better luminous efficiency and performance.
[0018] Furthermore, the specific method of pickling is: adding the ground crude product into 37 wt % hydrochloric acid to prepare a suspension with a mass fraction of 10-30%, stirring at room temperature for 5 minutes, and then washing with pure water until neutral.
[0019] The beneficial effect of adopting the further technical solution is that the redundant M can be effectively removed. 2 SiO 5 Impurities can improve the purity of silicate phosphors, improve particle morphology, and optimize luminescence performance.
[0020] The beneficial effects of the present invention are as follows: the present invention provides a silicate phosphor doped with divalent europium, which realizes the luminescence of divalent europium ions at trivalent cation sites, and has important scientific value for the research and development of new phosphors. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The X-ray (XRD) diffraction pattern of the divalent europium-doped silicate phosphor prepared in Example 1;
[0022] Figure 2 is the X-ray (XRD) diffraction pattern of the silicate phosphor prepared in the comparative example;
[0023] Figure 3The excitation and emission spectra of the divalent europium-doped silicate phosphor prepared in Example 1;
[0024] Figure 4 The excitation and emission spectra of the silicate phosphor prepared in the comparative example. DETAILED DESCRIPTION
[0025] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.
[0026] Example 1
[0027] A divalent europium-doped silicate phosphor, the chemical formula of which is: Lu 2 SiO 5 :1.2Na + ,0.01Eu 2+ ; Its preparation method comprises the following steps:
[0028] S1: weigh 1.1938g Lu 2 O 3 , 0.36 g SiO 2 , 0.1908g Na 2 CO 3 , 0.0106g Eu 2 O 3 , fully mix and grind evenly to obtain a mixed material;
[0029] S2: Transfer the mixed material to a corundum crucible and heat at 80% N 2 / 20%H 2 The temperature was kept at 1300°C for 4 hours under the atmosphere, and the furnace was cooled to below 100°C to obtain a crude product;
[0030] S3: Grind the crude product, add the ground crude product into 37wt% hydrochloric acid to prepare a suspension with a mass fraction of 20%, stir at room temperature for 5 minutes, then wash with pure water until neutral, and then dry the washed crude product to obtain a silicate phosphor doped with divalent europium.
[0031] Example 2
[0032] A divalent europium-doped silicate phosphor, the chemical formula of which is: 2 SiO 5 :0.4Li + ,0.001Eu 2+ ; Its preparation method comprises the following steps:
[0033] S1: Weigh 6.779g Y 2 O 3 , 3.6 g SiO 2 , 0.444 g Li 2CO 3 , 0.0106g Eu 2 O 3 , fully mix and grind evenly to obtain a mixed material;
[0034] S2: Transfer the mixed material to a corundum crucible and heat at 80% N 2 / 20%H 2 The temperature was kept at 1200°C for 9 hours under the atmosphere, and the furnace was cooled to below 100°C to obtain a crude product;
[0035] S3: Grind the crude product, add it into 37 wt % hydrochloric acid to prepare a suspension with a mass fraction of 10%, stir it at room temperature for 5 min, wash it with pure water until it is neutral, and then dry the washed crude product to obtain a silicate phosphor doped with divalent europium.
[0036] Example 3
[0037] A divalent europium-doped silicate phosphor, the chemical formula of which is: La 2 SiO 5 :1.8K + ,0.1Eu 2+ ; Its preparation method comprises the following steps:
[0038] S1: weigh 0.9778g La 2 O 3 , 0.36 g SiO 2 , 0.3996g K 2 CO 3 , 0.106g Eu 2 O 3 , fully mix and grind evenly to obtain a mixed material;
[0039] S2: The mixed material is transferred to a corundum crucible, kept at 1400°C for 3 hours under a CO atmosphere, and then cooled to below 100°C to obtain a crude product;
[0040] S3: Grind the crude product, add it into 37wt% hydrochloric acid to prepare a suspension with a mass fraction of 30%, stir it at room temperature for 5 minutes, wash it with pure water until it is neutral, and then dry the washed crude product to obtain a silicate phosphor doped with divalent europium.
[0041] Example 4
[0042] A divalent europium-doped silicate phosphor, the chemical formula of which is: Lu 2 SiO 5 :1Na + ,0.005Eu 2+ ; Its preparation method comprises the following steps:
[0043] S1: weigh 1.1938g Lu 2 O 3 , 0.36 g SiO 2 , 0.159 g Na 2 CO 3 , 0.0053g Eu 2 O 3 , fully mix and grind evenly to obtain a mixed material;
[0044] S2: Transfer the mixed material to a corundum crucible and heat at 80% N 2 / 20%H 2 The temperature was kept at 1300°C for 4 hours under the atmosphere, and the furnace was cooled to below 100°C to obtain a crude product;
[0045] S3: Grind the crude product, add the ground crude product into 37wt% hydrochloric acid to prepare a suspension with a mass fraction of 20%, stir at room temperature for 5 minutes, then wash with pure water until neutral, and then dry the washed crude product to obtain a silicate phosphor doped with divalent europium.
[0046] Example 5
[0047] A divalent europium-doped silicate phosphor, the chemical formula of which is: Lu 2 SiO 5 :1.4Na + ,0.03Eu 2+ ; Its preparation method comprises the following steps:
[0048] S1: weigh 1.1938g Lu 2 O 3 , 0.36 g SiO 2 , 0.2226g Na 2 CO 3 , 0.0318g Eu 2 O 3 , fully mix and grind evenly to obtain a mixed material;
[0049] S2: Transfer the mixed material to a corundum crucible and heat at 80% N 2 / 20%H 2 The temperature was kept at 1300°C for 4 hours under the atmosphere, and the furnace was cooled to below 100°C to obtain a crude product;
[0050] S3: Grind the crude product, add the ground crude product into 37wt% hydrochloric acid to prepare a suspension with a mass fraction of 20%, stir at room temperature for 5 minutes, then wash with pure water until neutral, and then dry the washed crude product to obtain a silicate phosphor doped with divalent europium.
[0051] The performance effects of the divalent europium-doped silicate phosphors prepared in Examples 1 to 5 are similar, and the divalent europium-doped silicate phosphor prepared in Example 1 is used in subsequent experiments.
[0052] Comparative Example
[0053] A silicate phosphor with the chemical formula: Lu 2 SiO 5 :0.1Eu 3+ ; Its preparation method comprises the following steps:
[0054] S1: weigh 1.1938g Lu 2 O 3 , 0.18 g SiO 2 , 0.106g Eu 2 O 3 , fully mix and grind evenly to obtain a mixed material;
[0055] S2: Transfer the mixed material to a corundum crucible and heat at 80% N 2 / 20%H 2 The temperature was kept at 1300°C for 4 hours under the atmosphere, and the furnace was cooled to below 100°C to obtain a crude product;
[0056] S3: Grind the crude product, add it into 37 wt % hydrochloric acid to prepare a suspension with a mass fraction of 20%, stir it at room temperature for 5 min, wash it with pure water until it is neutral, and then dry the washed crude product to obtain silicate phosphor.
[0057] Experimental Example 1
[0058] Composition detection: X-ray diffraction analysis was performed on the divalent europium-doped silicate phosphor prepared in Example 1 and the silicate phosphor prepared in the comparative example. The results are as follows: Figures 1-2 As shown: The divalent europium-doped silicate phosphor prepared in Example 1 and Lu 2 SiO 5 By comparing the PDF cards of the samples, it can be found that the doping of Na and Eu did not change the phase, and the sample was still Lu 2 SiO 5 Pure phase, no impurities; the silicate phosphor prepared in the comparative example and Lu 2 SiO 5 The PDF card comparison shows that the synthetic sample is Lu 2 SiO 5 , Eu doping does not change the phase.
[0059] Experimental Example 2
[0060] Luminescence performance test: The excitation and emission spectra of the divalent europium-doped silicate phosphor prepared in Example 1 are as follows: Figure 3 As shown in Figure 2, under the excitation of 365nm near-ultraviolet light, the sample exhibits green light emission with a main peak at 502nm, and the emission wavelength covers 450-600nm. The broadband emission indicates that the emission comes from Eu 2+ 5d-4f transition; under 502nm monitoring, its excitation wavelength range covers 250-450nm, and the optimal excitation is 370nm, indicating that the sample can be excited by commercial near-ultraviolet LED chips. + The ion part will enter Lu 2 SiO 5 The interstitial positions of the lattice generate additional valence electrons to promote Eu 3+ Reduction to Eu 2+ , making Eu 2+ Ions in Lu 3+ Stable existence in the lattice.
[0061] The excitation and emission spectra of the silicate phosphor prepared in the comparative example are as follows: Figure 4 As shown, under 365nm excitation, due to Eu 3+ The sample exhibits multiple narrow peak emissions corresponding to the 4f-4f transition of Eu 3+ of 5 D 1 → 7 F 1 (537nm), 5 D 0 → 7 F 0 (580nm), 5 D 0 → 7 F 1 (588, 595, 598nm), 5 D 0 → 7 F 2 (612, 619, 623nm) and 5 D 0 → 7 F 3 (654, 658nm) transition; under 612nm monitoring, its excitation spectrum also shows multiple narrow peaks, located at 319nm ( 7 F 0 → 5 H 6 ), 363nm( 7 F 0 → 5 D 4 ), 382nm( 7 F 0 → 5 L 7 ), 394nm(7 F 0 → 5 L 6 ), 414nm( 7 F 0 → 5 D 3 ) and 466nm( 7 F 0 → 5 D 2 ). Although the control sample is also at 80% N 2 / 20%H 2 Synthesized under reducing atmosphere, but due to Lu 3+ The trivalent characteristic of Eu is that trivalent Eu is more stable in this lattice. 3+ Cannot be reduced to Eu without Na doping 2+ , so only Eu 3+ characteristic emission peaks.
[0062] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.
Claims
1. A silicate phosphor doped with divalent europium, characterized in that: The chemical formula of the silicate phosphor is A2SiO5:aM + ,bEu 2+ , wherein A is Y, La or Lu, M is Li, Na or K, 0.4≤a≤1.8, 0.001≤b≤0.
1.
2. The divalent europium-doped silicate phosphor according to claim 1, characterized in that: 1≤a≤1.4, 0.005≤b≤0.
03.
3. The method for preparing the divalent europium-doped silicate phosphor according to claim 1 or 2, characterized in that: The following steps are involved: S1: weighing raw materials according to the ratio of each element in the chemical formula of silicate phosphor except Si element, with Si in excess of one time, and grinding and mixing the raw materials to obtain a mixed material; S2: keeping the mixture at 1200-1400°C in a reducing atmosphere for 3-9 hours, and then cooling to obtain a crude product; S3: grinding, acid washing and drying the crude product to obtain a silicate phosphor doped with divalent europium; The raw materials are oxides or nitrates of Y, La or Lu, carbonates of Li, Na or K, and silicon dioxide or silicic acid.
4. The method for preparing the divalent europium-doped silicate phosphor according to claim 3, characterized in that: The reducing atmosphere is CO gas or N2 / H2 mixed gas.
5. The method for preparing the divalent europium-doped silicate phosphor according to claim 4, characterized in that: The volume ratio of N2 to H2 in the N2 / H2 mixed gas is 4:
1.
6. The method for preparing divalent europium-doped silicate phosphor according to claim 3, characterized in that: The specific method of pickling is: adding the ground crude product into 37wt% hydrochloric acid to prepare a suspension with a mass fraction of 10-30%, stirring at room temperature for 5 minutes, and then washing with pure water until neutral.