Preparation method of titanium gypsum composite biochar and application of titanium gypsum composite biochar in arsenic-polluted soil
Through the composite biochar technology of titanium gypsum and straw, the problem of short curing and stabilization repair cycle and high cost in soil arsenic pollution repair is solved, and the effect of effectively reducing arsenic pollution is achieved, and soil fertility and plant growth are improved, which significantly reduces the number of soil fertility and plant growth. The biological effectiveness of arsenic.
Patent Information
- Application Number
- CN202411075373.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
In the repair of heavy metal pollution in soil, especially in the treatment of arsenic pollution, the curing and stabilization repair cycle is short and the cost is high, and the resource utilization of titanium gypsum is less, making it difficult to effectively reduce the ecological risks and treatment costs of arsenic. .
By combining titanium gypsum with straw, titanium gypsum composite biochar was prepared. The titanium gypsum and biochar were successfully combined by hydrothermal extraction and grinding co-heating method, and DRG-BC and GRG-BC were prepared for reducing The bioeffective arsenic content in the soil and acts as a passivator and water fertilizer regulator to reduce the absorption of arsenic by plants.
Effectively reduce the arsenic content in soil and plants, improve soil fertility, promote the increase of plant biomass and chlorophyll fluorescence, significantly reduce the bioavailability of arsenic ions, and maintain a high passivation rate under different conditions. , and good cost and preparation efficiency.
Smart Images

Figure CN118995228A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of soil heavy metal pollution remediation, and more specifically relates to a preparation method of titanium gypsum composite biochar and application thereof in arsenic contaminated soil. Background Art
[0002] Arsenic (As) is a toxic metalloid element that is ubiquitous in nature. The As content in the earth's crust ranks 20th. As exists in nature in the form of more than 200 minerals, of which 60% are arsenates, 20% are As sulfides and sulfate minerals, and the remaining 20% are arsenides, arsenites, and As oxides. The valence electron layer structure of the ground state As atom is 4S24Px'4Py'4P21, which can show a variety of valence states (-3, +3 and +5), among which the main valence states are positive trivalent and positive pentavalent. Among inorganic arsenic, the toxicity of As(III) is related to its high affinity for the sulfhydryl groups of biological molecules and the cysteine residues of many enzymes. The formed As(III)-S bond causes various harmful effects by inhibiting the activity of enzymes. Therefore, it is of great significance to clarify the transformation of As in soil and take measures to repair it to reduce the ecological risk of As in soil.
[0003] The remediation of As contaminated soil mainly reduces the total amount of As in the soil, or reduces the migration and diffusion capacity of As in the soil, thereby reducing the harm of As to the environment and human health. Currently, mature and widely used As contaminated soil remediation technologies include phytoremediation, solidification and stabilization remediation, leaching technology, and combined remediation of several technologies. Solidification and stabilization remediation is widely used in the actual application of soil As remediation due to its short remediation cycle and simple operation.
[0004] Biochar is a product obtained by thermochemical conversion of biomass under oxygen-limited environment. Crop straw is abundant and widely available, and is the main raw material for preparing biochar. The resource utilization of biochar can not only solve the problem of disposal of agricultural solid waste straw, but also conform to the sustainable development concept of the country's green economy, circular economy, and low-carbon economy, and produce good economic, environmental and social benefits.
[0005] More than 90% of titanium dioxide companies use the solid-phase sulfuric acid method for production. The sulfuric acid method produces a large amount of acidic wastewater. To treat the acidic wastewater, companies usually add lime-based alkaline substances to neutralize it. This neutralization process is how industrial solid waste titanium gypsum (RG, red gypsum) is produced.
[0006] Up to now, the research and development on titanium gypsum has not been fully utilized in the restoration of heavy metals in soil. The purpose is to comprehensively utilize titanium gypsum and straw as resources by treating waste with waste, combining the rich biomass in biochar with the rich metal oxides in titanium gypsum, while maintaining a high efficiency treatment effect and further reducing the treatment cost. Therefore, how to combine titanium gypsum and biochar to reduce the hazards of As pollution is an urgent problem that technicians in this field need to solve. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing titanium gypsum composite biochar and its application in arsenic contaminated soil, so as to solve the problems existing in the above-mentioned prior art and achieve the effect of further reducing the absorption of arsenic by plants while passivating arsenic in the soil.
[0008] To achieve the above object, the present invention provides the following solutions:
[0009] One of the technical solutions of the present invention is to provide a method for preparing titanium gypsum composite biochar, the steps comprising:
[0010] The straw is compounded with titanium gypsum and then pyrolyzed under nitrogen atmosphere to obtain titanium gypsum composite biochar.
[0011] The compounding is carried out by leaching method or mechanical grinding and mixing method.
[0012] Furthermore, the composite ratio of the straw and the titanium gypsum is such that the mass ratio of Fe in the titanium gypsum to the straw is 1:20.
[0013] Furthermore, the straw is air-dried, crushed and then passed through a 2 mm sieve.
[0014] Furthermore, the step of the leaching compounding method includes: adding titanium gypsum to a sulfuric acid solution, stirring and mixing until the reaction is complete, filtering, collecting the filtrate, soaking the straw in the filtrate, stirring for 2 hours in a 60°C water bath, and then drying to complete the leaching compounding method.
[0015] Preferably, the concentration of the sulfuric acid solution is 0.5 mol / L.
[0016] Preferably, the mass / volume ratio of the titanium gypsum and the sulfuric acid solution is 10 g:100 mL.
[0017] Preferably, the drying temperature is 100°C.
[0018] Furthermore, the step of compounding by mechanical grinding and mixing includes: stirring titanium gypsum and straw in a closed manner, and fully mixing them to complete the compounding by mechanical grinding and mixing.
[0019] Furthermore, the step parameters of the oxygen-limited pyrolysis are: heating to 800° C. at a heating rate of 20° C. / min, keeping the temperature for 1 hour, and then cooling to room temperature to complete the oxygen-limited pyrolysis.
[0020] The second technical solution of the present invention is to provide a titanium gypsum composite biochar prepared by the above method.
[0021] The third technical solution of the present invention is to provide an application of the titanium gypsum composite biochar as a passivating agent in repairing heavy metal pollution in soil or reducing the arsenic content in edible parts of plants.
[0022] Furthermore, the repair of soil heavy metal pollution is to reduce the arsenic content in the soil.
[0023] Technical solution four of the present invention: provides an application of the above-mentioned titanium gypsum composite biochar as a passivator coupled with water and fertilizer regulation in repairing soil heavy metal pollution or reducing the arsenic content in edible parts of plants.
[0024] The present invention discloses the following technical effects:
[0025] The present invention is based on the resource utilization of heavy metal arsenic pollution in farmland soil and industrial solid waste titanium gypsum (RG). The hydrothermal extraction method and the grinding co-heating method are used to successfully compound RG with biochar to prepare DRG-BC and GRG-BC, which can effectively reduce the biologically effective arsenic content in the soil, thereby reducing the arsenic content enriched from the soil to the roots and stems and leaves of plants. In addition, the titanium gypsum composite biochar prepared by the present invention is rich in active groups and a large amount of organic matter. After application, it can not only reduce the biological effectiveness of arsenic ions in the soil, but also improve soil fertility and promote the increase of plant biomass. It can significantly increase the biomass and chlorophyll fluorescence of plants, and has good economic benefits in terms of cost and preparation. The addition of 1.5% does not cause stress to plant growth, but further promotes it.
[0026] The titanium gypsum composite biochar prepared by the present invention is coupled with water and fertilizer regulation, and can maintain a high passivation rate under different moisture contents and fertility conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0028] Figure 1 The effect of pH value on the adsorption of BC, DRG-BC and GRG-BC;
[0029] Figure 2This is the adsorption curve of BC at 50 mg / L arsenic ion concentration;
[0030] Figure 3 This is the adsorption curve of DRG-BC at 50 mg / L arsenic ion concentration;
[0031] Figure 4 This is the adsorption curve of GRG-BC at 50 mg / L arsenic ion concentration;
[0032] Figure 5 is the FT-IR image of BC;
[0033] Figure 6 FT-IR image of DRG-BC;
[0034] Figure 7 is the FT-IR image of GRG-BC;
[0035] Figure 8 is the SEM image of BC;
[0036] Fig. 9 is the SEM image of DRG-BC;
[0037] Fig.10 is the SEM image of GRG-BC;
[0038] Fig.11 is the EDS diagram of BC;
[0039] Fig.12 This is the EDS diagram of DRG-BC;
[0040] Fig.13 is the EDS image of GRG-BC;
[0041] Fig.14 is the XRD pattern of BC;
[0042] Fig.15 is the XRD pattern of DRG-BC;
[0043] Fig.16 is the XRD pattern of GRG-BC;
[0044] Fig.17 This is a comparison chart of arsenic content in the aerial part of Chinese cabbage;
[0045] Fig.18 This is a comparison chart of arsenic content in the underground part of pakchoi;
[0046] Fig.19 The effects of BC, DRG-BC and GRG-BC on the available arsenic content in soil;
[0047] Fig. 20This is a comparison chart of arsenic content in the aboveground part of Chinese cabbage obtained by GRG-BC coupling water and fertilizer regulation;
[0048] Fig.21 This is a comparison chart of arsenic content in the underground part of Chinese cabbage obtained by GRG-BC coupling water and fertilizer regulation;
[0049] Fig. 22 This is the effect of GRG-BC coupled water-fertilizer regulation on the available arsenic content in soil. DETAILED DESCRIPTION
[0050] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0051] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0052] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0053] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0054] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0055] Unless otherwise specified, room temperature / normal temperature referred to in the present invention refers to 25±5°C.
[0056] The main components of the titanium gypsum used in the specific embodiment of the present invention are shown in Table 1, and are provided by Jiangsu Xuzhou Titanium Dioxide Chemical Co., Ltd.
[0057] Table 1
[0058]
[0059] Example 1
[0060] Preparation of titanium gypsum composite biochar:
[0061] S1. Air-dry and crush the straw, and pass it through a 2mm sieve for later use;
[0062] S2, weigh 20g of titanium gypsum, grind it and add it to 0.5mol / L sulfuric acid solution, stir and mix, filter after the reaction is complete, and take the crushed straw biomass and immerse it in the filtrate, so that the mass ratio of Fe in the titanium gypsum to the straw is 1:20, then place the beaker in a 60°C water bath and stir for 2h, and then put it in a 100°C oven to dry, and obtain the composite biomass after drying;
[0063] S3. The composite biomass was placed in a tubular furnace for oxygen-limited pyrolysis. During the pretreatment, nitrogen was passed through the tubular furnace for protection. The initial temperature was set to 25°C, the heating rate was 20°C / min, and the preparation temperature was set to 800°C. After the temperature was raised to 800°C, it was kept constant for 1 hour and then cooled to room temperature. Then it was taken out and sealed to obtain titanium gypsum composite biochar, which was recorded as DRG-BC.
[0064] Example 2
[0065] Preparation of titanium gypsum composite biochar:
[0066] S1. Air-dry and crush the straw, and pass it through a 2mm sieve for later use;
[0067] S2, titanium gypsum and crushed straw biomass are placed in a mixer, and the mass ratio of Fe in the titanium gypsum to the straw biomass is also 1:20. The mixer containing the titanium gypsum and the crushed straw biomass is sealed, and repeatedly stirred under mechanical action to fully mix the titanium gypsum and the straw biomass to obtain composite biomass;
[0068] S3. The composite biomass was placed in a tubular furnace for oxygen-limited pyrolysis. During the pretreatment, nitrogen was passed through the tubular furnace for protection. The initial temperature was set to 25°C, the heating rate was 20°C / min, and the preparation temperature was set to 800°C. After the temperature was raised to 800°C, it was kept constant for 1 hour and then cooled to room temperature. Then it was taken out and sealed to obtain titanium gypsum composite biochar, which was recorded as GRG-BC.
[0069] Comparative Example 1
[0070] Preparation of ordinary biochar:
[0071] S1. Air-dry and crush the straw, and pass it through a 2mm sieve for later use;
[0072] S2. The crushed straw was placed in a tubular furnace for oxygen-limited pyrolysis. During the pretreatment, nitrogen was passed through the tubular furnace for protection. The initial temperature was set to 25°C, the heating rate was 20°C / min, and the preparation temperature was set to 800°C. After the temperature was raised to 800°C, it was kept constant for 1 hour and then cooled to room temperature. Then it was taken out and sealed for storage to obtain ordinary biochar, which was recorded as BC.
[0073] Test example
[0074] 1. Experiment on the effect of pH value on the adsorption of heavy metal arsenic by BC, DRG-BC and DRG-BC materials
[0075] Solution pH value and As(Ⅲ) adsorption equilibrium experiment: dilute the arsenic standard solution and adjust its concentration to 50 mg / L. Each 150 mL conical flask is filled with 50 mL of dilution. Accurately weigh 0.02 g of adsorbent material and add it to the above conical flask. Use 1M HCl and 1M NaOH to adjust the initial pH value of the solution to 3, 4, 5, 6, 7, and 8, respectively. The adsorption time is 360 min, the temperature is 25 ° C, and the pH value is not adjusted during this period.
[0076] The pH value of the solution is crucial to the adsorption of heavy metal ions. The concentrations of hydrogen ions and hydroxide ions in the aqueous solution will affect the hydrolysis and surface charge of heavy metals in the aqueous solution. Figure 1 The effect of pH value on the adsorption of BC, DRG-BC and GRG-BC. Figure 1 It can be seen that when the pH is between 3 and 8, GRG-BC has the best adsorption effect on arsenic (56.75-69.25 mg / g), indicating that GRG-BC has a wide pH application range. As the initial pH value of the solution increases, the arsenic adsorption performance of the three materials gradually decreases. Under acidic conditions, GRG-BC and DRG-BC can more efficiently adsorb arsenic anions under the action of electrostatic attraction due to the presence of certain positive charges in substances such as metal oxides; as the pH increases, the positive charges carried by GRG-BC and DRG-BC themselves begin to decrease, so under the action of electrostatic repulsion, the adsorption performance of the two decreases, and the efficiency of removing arsenic ions gradually decreases, but overall they are significantly higher than the BC group.
[0077] 2. Adsorption kinetics experiment
[0078] Accurately weigh 0.02g of adsorption material and add it to a 150mL conical flask containing 50mL of 50mg / L diluted arsenic standard solution. The pH value of the solution is adjusted to 7.0, and the adsorption temperature is controlled at 25°C. Prepare multiple replicates at the same time. Take 3 replicates at 0, 10, 20, 30, 60, 120, 180, 240, 300, and 360 minutes from the start of the adsorption reaction, filter the solution immediately, and determine its concentration.
[0079] Figure 2 This is the adsorption curve of BC at 50 mg / L arsenic ion concentration; Figure 3 This is the adsorption curve of DRG-BC at 50 mg / L arsenic ion concentration; Figure 4 This is the adsorption curve of GRG-BC at 50 mg / L arsenic ion concentration. Figures 2 to 4 It can be seen that the removal rate of BC increased significantly within 30 minutes of contact time, and then the removal rate slowed down and gradually reached adsorption equilibrium at 300 minutes; the removal rate of DRG-BC changed rapidly from 0 to 50 minutes, and then the removal rate changed slowly, and gradually reached adsorption equilibrium at 300 minutes; GRG-BC also had a fast adsorption effect on heavy metal arsenic ions from 0 to 50 minutes, and gradually reached adsorption equilibrium at 240 minutes. Among them, GRG-BC and DRG-BC showed excellent adsorption performance for arsenic.
[0080] 3. Characterization of materials
[0081] Mix the materials BC, DRG-BC and GRG-BC with potassium bromide under a baking lamp, grind and press into tablets, and then test the samples.
[0082] Figure 5 is the FT-IR image of BC; Figure 6 FT-IR image of DRG-BC; Figure 7 is the FT-IR image of GRG-BC; Figures 5 to 7 It can be seen from the FTIR spectrum that the biochar-loaded titanium gypsum materials prepared by the hydrothermal synthesis method and the grinding co-thermal method show similar effects. -1 The stretching vibration of Fe-O bond was detected near 1043 cm -1 The characteristic peak detected at is caused by the bending vibration of the Fe-OH bond. BC may still contain cellulose, hemicellulose and lignin, and the spectrum shows many miscellaneous peaks.
[0083] Figure 8 is the SEM image of BC; Fig. 9 is the SEM image of DRG-BC; Fig.10 is the SEM image of GRG-BC; Figures 8 to 10It can be seen that the BC and two titanium gypsum composite biochars prepared at 800°C all present a typical porous structure. As the observation scale is further enlarged, the three biochar materials show different structural morphologies. For BC, the BC surface is relatively smooth, and no large amount of particles are observed. However, particles of different forms are distributed on the surface of the other two titanium gypsum composite biochar materials. Most of the surface particles are irregular spheres, and some particles are connected together, indicating that the material has been successfully loaded. The surface particles of GRG-BC are dispersed and relatively more uniform than those of DRG-BC. After complete grinding and mixing, the titanium gypsum is evenly distributed on the surface and pores of the biomass.
[0084] Fig.11 is the EDS diagram of BC; Fig.12 This is the EDS diagram of DRG-BC; Fig.13 is the EDS diagram of GRG-BC; Figures 11 to 13 It can be seen that the surface particles of the three materials were spectrally marked by FSEM-EDS to analyze the elemental composition of the particles. The surface particle element composition of BC and the two titanium gypsum composite biochars all contain a large amount of C and O, but the element ratios between the three materials are different. The particles on the surface of DEG-BC are mainly composed of Fe, C and O, while the particles on the surface of GRG-BC are mainly composed of Fe, C, O and Ca.
[0085] Fig.14 is the XRD pattern of BC; Fig.15 is the XRD pattern of DRG-BC; Fig.16 is the XRD pattern of GRG-BC; Figures 14 to 16 It can be seen that as the pyrolysis temperature reaches 800℃, DRG-BC and GRG-BC form a large number of peaks at 2θ=45° and around. Through the mineral comparison of Jade software and existing research, it can be known that Fig.15 and Fig.16 There are Fe3C and a certain amount of Fe 0 There is a peak, and it is mainly composed of Fe3C, which means that iron element appears in the composite materials compared with BC.
[0086] 4. Passivation and remediation effect of soil arsenic pollution
[0087] The test soil in this experiment was collected from the farmland of Liuxin Town, Xuzhou City, Jiangsu Province. The soil sampling depth was 0-20 cm. The residues (weeds, gravel and debris, etc.) in the soil samples were removed and dried naturally in the shade for seven days. Then, they were crushed and sieved with a wooden hammer. The mesh size was 2 mm. After sieving, they were stored in plastic bags for future use. The basic physical and chemical properties of the soil are shown in Table 2.
[0088] Table 2
[0089]
[0090] Experimental design: 10 treatments were set up as shown in Table 3. The blank control group was CK. Three parallel samples were set up in each treatment group, for a total of 30 samples. The size of the plastic flower pot was 16.5cm×11cm, and 1kg of arsenic-contaminated soil was added to each flower pot. BC, DRG-BC and GRG-BC were added to different treatment groups at a fixed ratio. In order to mix BC, DRG-BC and GRG-BC with the above soil evenly, a watering can was used to add water and stir after complete mixing. The amount of deionized water added was 60% of the maximum water holding capacity in the field, and the moisture content was kept constant at 60% within 14 stable days to ensure the passivation effect of the material.
[0091] Table 3
[0092]
[0093] After 14 days, BC, DRG-BC and GRG-BC were mixed with arsenic-contaminated soil by default and were uniformly and stably mixed. Ten Chinese cabbage seeds were sown in each pot. When most of the Chinese cabbage grew the first true leaves, thinning began. Three Chinese cabbage plants with equivalent and good growth were retained in each pot to ensure that the well-developed Chinese cabbage was finally harvested at the end of the experiment. The same field management measures were adopted before harvesting, and the growth cycle was 30 days. The Chinese cabbage was cut along the surface of the potted soil and divided into edible parts (including leaves and stems) and roots. The weights were weighed and recorded as the fresh weight of the aboveground part and the fresh weight of the underground part. After weighing, some fresh samples were ground and stored for subsequent experimental measurement and analysis. The samples were marked and placed in beakers, and placed in an oven at 105°C for half an hour to achieve the purpose of killing green and destroying the enzyme activity of the plants. Then the oven temperature was adjusted to 67°C and dried to constant weight. The dried plants were ground into powder according to the aboveground and underground parts for subsequent experimental measurement and analysis. The soil attached to the roots was air-dried and then ground and sieved with a mesh size of 1 mm for subsequent experimental measurement and analysis.
[0094] The pakchoi seeds used were provided by Tianjin Gengyun Seed Co., Ltd., and the variety was Jinzhi 30.
[0095] Determination of arsenic content in plants and soil: Plants were treated and digested according to the national standard GB5009.15, and the arsenic concentration in the digestion solution was measured using inductively coupled plasma mass spectrometry; soil was digested using the four-acid digestion method, and the arsenic concentration in the digestion solution was measured using LA-ICP-MS.
[0096] Fig.17 This is a comparison chart of arsenic content in the aboveground part of Chinese cabbage. Fig.17It can be seen that compared with the CK treatment, both DRG-BC and GRG-BC treatments reduced the arsenic content in the edible parts of Chinese cabbage and significantly inhibited the absorption of arsenic by Chinese cabbage. For different dosages, the arsenic content in the aboveground part of Chinese cabbage in the DRG-BC treatment group was reduced by 9.21%-15.26%, and the arsenic content in the aboveground part of Chinese cabbage in the GRG-BC treatment group was reduced by 14.08%-27.24%, which was significantly lower than that in CK. In the BC treatment group, the arsenic content in the aboveground part of Chinese cabbage increased. Compared with BC, titanium gypsum composite biochar has a better inhibitory effect on arsenic. At the same time, the remediation effect is also related to the addition ratio of composite biochar. The arsenic content in the aboveground part of Chinese cabbage in the GRG-BC treatment group with a 1.5% addition ratio was reduced by 27.24% compared with the CK treatment group.
[0097] Fig.18 This is a comparison chart of arsenic content in the underground part of Chinese cabbage. Fig.18 It can be seen that due to the large enrichment coefficient of leafy vegetables, under the BC treatment conditions, the arsenic content in the underground part of the plants exceeded that of the CK control group. It is difficult to repair and passivate arsenic in the soil only through BC. Under the DRG-BC and GRG-BC treatment conditions, the arsenic content in the underground part of Chinese cabbage also showed a good treatment effect. At the same time, with the increase of GRG-BC dosage, the arsenic content in the underground part of Chinese cabbage is further reduced. The actual application effect of titanium gypsum composite biochar is very good and the feasibility is high.
[0098] The transport capacity of pakchoi from underground to aboveground parts of cadmium is expressed by the translocation factors (TF), and the calculation formula is:
[0099]
[0100] Among them, C 地上 and C 地下 They are the arsenic concentrations in the aboveground and underground parts of Chinese cabbage, respectively. The results are shown in Table 4.
[0101] Table 4
[0102]
[0103]
[0104] As can be seen from Table 4, both DRG-BC and GRG-BC treatments reduced the arsenic transport coefficient (P < 0.05), with significant differences. The BC treatment group decreased from 0.043 to 0.040 compared with the CK treatment group, the DRG-BC treatment group decreased from 0.043 to 0.0393 compared with the CK treatment group, and the GRG-BC treatment group decreased from 0.043 to 0.0379 compared with the CK treatment group.
[0105] Titanium-gypsum composite biochar is rich in active groups and a large amount of organic matter, so it can not only reduce the bioavailability of arsenic ions in the soil, but also improve soil fertility and promote the increase of plant biomass. As can be seen from Table 5, in this round of planting, the aboveground fresh weight of the treatment with BC increased by 2.5%-6.9% compared with the control CK. At the addition ratio of 0.5%-1.5%, increasing the addition ratio had a positive effect on the increase of biomass; and the aboveground fresh weight of plants in the treatment groups with DRG-BC and GRG-BC increased significantly compared with the CK group (p<0.05), and increased by 6.1%-16.8% and 12.5%-23.2% respectively compared with the control CK. The addition of titanium-gypsum composite biochar in the soil promotes the growth of plants. When the addition ratio is 1.5%, the aboveground dry fresh weight of Chinese cabbage reaches the maximum. In this round of planting, the root biomass of plants in the treatment group with passivators also increased significantly. Compared with the control group CK, the root fresh weight of the treatment group with BC increased by 11.65% when the addition amount was 1.5%. The root fresh weight of plants in the treatment groups with DRG-BC and GRG-BC increased significantly compared with the CK group (p<0.05), increasing by 12.8%-25.1% and 19.2%-37.6%, respectively.
[0106] Table 5 Effect of titanium-gypsum composite biochar on plant biomass
[0107]
[0108]
[0109] Determination of plant quality indicators: The vitamin C content in plants was determined by the 2,6-dichloroindophenol titration method, with oxalic acid as the extract; the soluble protein content in plants was determined by the Coomassie brilliant blue colorimetric method, with a mixed solution of phosphoric acid and ethanol as the extractant; the soluble sugar content in plants was determined using the anthrone colorimetric method; the chlorophyll fluorescence of plants was determined by using a handheld chlorophyll fluorescence meter to measure the chlorophyll fluorescence response of the edible parts of the plants, and the results are shown in Table 6.
[0110] Table 6 Effects of titanium-gypsum composite biochar on plant quality
[0111]
[0112] The edibility of Chinese cabbage is an extremely important indicator, and its quality also needs further analysis. Therefore, vitamin C and chlorophyll fluorescence were selected as quality evaluation indicators. As shown in Table 6, the vitamin C content of the four groups of DRG-BC, GRG-BC, CK and BC is basically similar, so the addition of titanium gypsum-loaded biochar has little effect on the vitamin C content, and there is no obvious regularity. However, the chlorophyll fluorescence content of the GRG-BC treatment group has been significantly increased because the TiO2 and other substances in the titanium gypsum contained in GRG-BC have a promoting effect on photocatalysis, greatly enhancing the photosynthesis of plants and promoting stomatal respiration. Therefore, the chlorophyll fluorescence of the Chinese cabbage in this treatment group has been significantly improved, compared with the CK group, it has increased by 7.2%-9.8%.
[0113] The effects of titanium gypsum composite biochar on root soil pH and Eh value are shown in Table 7.
[0114] Table 7
[0115]
[0116] From the data in Table 7, it can be seen that the original soil was added with biochar and two titanium gypsum composite biochars. Since biochar is alkaline, the pH of the soil in the BC treatment group was improved, and each treatment increased by 0.01-0.12 pH units compared with the CK group. The alkaline groups in the biochar combined with carbonates to reduce soil acidity and increase pH. The soil pH of the treatment groups added with DRG-BC and GRG-BC also increased to varying degrees, but under the conditions, the reduction of oxides such as iron and manganese would produce H +, which leads to a decrease in pH. Therefore, in the entire mixing process, the improvement brought about by the low addition ratio is limited. 30 days after planting the plants, the pH of the soil at the roots of some plants decreased. Compared with the treatment with the addition of ordinary biochar, the passivation of titanium gypsum composite biochar and the inhibition of plant absorption of arsenic are mainly through two pathways. One is to adsorb and passivate arsenic in the soil by a large amount of metal oxides, and the other is to inhibit the enrichment of arsenic in the roots of plants through the antagonistic effect of plant root cell walls and transmembrane transport proteins. The decrease in soil pH at the roots is due to the large amount of amino acids, organic acids and other substances contained in plant root secretions. Plants use these substances to form complexes with mineral elements in the soil to improve biological effectiveness, so some treatment groups showed a decrease in pH 30 days after planting. The Eh of the plant root soil in the treatment group with GRG-BC added was significantly higher than that in the CK group, with different addition ratios increasing by 32.3%-44.4%. It was also higher than the 3.5%-12% in the BC group and the 11.6%-16.7% in the DRG-BC group. Under the same moisture content, it may be that GRG-BC not only stabilized the effective arsenic in the soil that inhibited plants, but also further promoted the secretion of plant roots, thereby increasing the Eh of the soil.
[0117] Fig.19 The effects of BC, DRG-BC and GRG-BC on the available arsenic content in soil. Fig.19 It can be seen that the addition of DRG-BC and GRG-BC, two titanium gypsum biochar composite materials, can effectively reduce the content of water-soluble and exchangeable arsenic in the soil, and with the increase of the amount of composite material added, the stabilization rate of soil available arsenic increases. The initial content of available arsenic in the arsenic-contaminated soil sample of the control group CK was 4.92 mg / kg. After adding 0.5%, 1%, and 1.5% GRG-BC, the content of available arsenic in the soil decreased to 4.37, 4.23, and 3.89 mg / kg, respectively, with a decrease of 11.7% to 20.9%; after adding 0.5%, 1%, and 1.5% DRG-BC, the content of available arsenic in the soil decreased to 4.56, 4.47, and 4.32 mg / kg, respectively, with a decrease of 7.3% to 12.3%, which significantly reduced the content of available arsenic in the soil compared with CK (p<0.05). And the greater the addition ratio, the more obvious the effect of reducing the content of available arsenic in the soil.
[0118] The effects of titanium gypsum composite biochar on the contents of soil alkaline nitrogen, available phosphorus and available potassium are shown in Table 8 (the determination methods of soil available nutrients are all based on the book "Soil Agrochemical Analysis" by Bao Shidan).
[0119] Table 8
[0120]
[0121] It can be seen from Table 8 that DRG-BC and GRG-BC have a certain effect on improving the effective fertility of the soil. They have increased the content of available phosphorus in the upper soil to a certain extent, promoted the content of organic nutrients into inorganic activated bioavailable nitrogen, increased the content of effective potassium in the soil, promoted the transformation of organic nutrients into inorganic nutrients, and improved the overall fertility of the soil.
[0122] 5. Experiment on titanium gypsum composite biochar as a passivator coupled with water and fertilizer regulation
[0123] Experimental design: 12 treatments were set up, as shown in Table 9. Three parallel samples were set up in each treatment group, for a total of 36 samples. The same soil as the soil arsenic contamination passivation remediation effect experiment was used. Among them, three conventional fertilization groups were set up, denoted as W; three nitrogen fertilizer groups were denoted as NW; three phosphorus fertilizer groups were denoted as PW; three potassium fertilizer groups were denoted as KW, and each fertilizer group was denoted as 50% of the corresponding fertilizer. Each group was set up with three treatments of controlling the moisture content to 40%, 60%, and 80% of the maximum water holding capacity. Then GRG-BC was added at a dosing ratio of 1.5%, and after mixing, it was stabilized for 14 days, and Chinese cabbage was planted. The variety was the same as the above experiment, the planting method was the same as the above experiment, and the disposal measures were the same as the above experiment.
[0124] Table 9
[0125]
[0126] Fig. 20 This is a comparison chart of arsenic content in the aboveground part of Chinese cabbage obtained by GRG-BC coupling water and fertilizer regulation. Fig. 20 It can be seen that in the W treatment group with normal fertilization, the arsenic concentration in the aboveground part of the cabbage mixed with GRG-BC was positively correlated with the water content of the potted plants as the water content changed. As the soil water content increased, the arsenic concentration in the aboveground part of the cabbage increased to a certain extent, but the increase was extremely limited. From 40% water content to 80% water content, it only increased by 9.7%. In the NW and PW treatment groups with additional N and P additions, the arsenic content in the aboveground part of Chinese cabbage increased significantly, reaching 57.3% and 79.6%, which was extremely significant. It may be that with the additional application of N and P, the growth of plants was better than that of the normal W component of fertilization, and the roots absorbed arsenic in the soil in the surrounding area more strongly. In the PW treatment group with additional P application, the arsenic content in the aboveground part of Chinese cabbage decreased significantly. This may be because phosphorus and arsenic are in similar main groups, and phosphorus and arsenic will compete for adsorption when occupying the absorption points of Chinese cabbage. Therefore, the arsenic content in the aboveground part of Chinese cabbage in the treatment group with additional P application decreased.
[0127] Fig.21This is a comparison chart of arsenic content in the underground part of Chinese cabbage obtained by GRG-BC coupling water and fertilizer regulation. Fig.21 It can be seen that due to the large enrichment coefficient of leafy vegetables, under the treatment condition of 80% moisture content, the arsenic content in the underground part of the plant increased to a certain extent compared with that at 40% moisture content, and the increase brought by the NW and KW groups was extremely significant. The additional N and K not only supplemented the growth substances of pakchoi, but also greatly enhanced the absorption of arsenic in the soil by pakchoi. With the increase of moisture content, the free degree of soluble and exchangeable arsenic in the soil increased and was further absorbed by pakchoi. The arsenic content in the underground part of pakchoi in the PW treatment group with added P also decreased. This conclusion is consistent with the conclusion of the aboveground part of pakchoi, indicating that P had already competed with arsenic for adsorption when absorbed by the roots of pakchoi, resulting in a decrease in the arsenic content in both the aboveground and underground parts of pakchoi.
[0128] The effects of GRG-BC coupled water and fertilizer regulation on plant biomass are shown in Table 10.
[0129] Table 10
[0130]
[0131] It can be seen from the data in Table 10 that the additional N and K components significantly increased the aboveground and underground biomass compared with the conventional fertilization group. The aboveground fresh weight increased by 1.52%-9.96% and 4.54%-7.98%, respectively. At a moisture ratio of 40%-80%, increasing soil moisture content had a positive effect on the increase in biomass; at the same time, the underground fresh weight of plants in the additional K treatment group increased significantly compared with the conventional fertilization group (p<0.05), and increased by 26.62%-132.24% compared with the control, respectively. The additional K in the soil promoted the growth of plant roots. When the soil moisture content was 80%, the underground weight of Chinese cabbage reached a maximum of 2.16g.
[0132] Fig. 22 The effect of GRG-BC coupled water-fertilizer regulation on soil available arsenic content is shown in Figure 2. Fig. 22 It can be seen that the moisture content of the four treatment groups ranged from 40% to 80%, reflecting a certain degree of increase in the effective arsenic content in the soil. The moisture content was inversely proportional to the effective arsenic in the soil. It may be that the excessively high moisture content dissolved the arsenic in the soil that was originally in an unstable state and converted it into effective arsenic. At the same time, a higher moisture content would keep the soil in an anaerobic state for a long time, and the redox potential of the soil would also decrease. Part of the arsenic in the reduced state for a long time would also migrate and be converted into water, thereby increasing the effective arsenic content in the soil.
[0133] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0134] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing titanium gypsum composite biochar, characterized in that the steps include: The straw is compounded with titanium gypsum and then pyrolyzed under nitrogen atmosphere to obtain titanium gypsum composite biochar. The compounding is carried out by leaching method or mechanical grinding and mixing method.
2. The preparation method according to claim 1, characterized in that: The composite ratio of the straw and the titanium gypsum is that the mass ratio of Fe in the titanium gypsum to the straw is 1:
20.
3. The preparation method according to claim 1, characterized in that: The steps of the leaching compounding method include: adding titanium gypsum to a sulfuric acid solution, stirring and mixing, filtering after the reaction is complete, collecting the filtrate, soaking the straw in the filtrate, stirring for 2 hours in a 60° C. water bath, and then drying to complete the leaching compounding method.
4. The preparation method according to claim 3, characterized in that: The concentration of the sulfuric acid solution is 0.5 mol / L; the mass / volume ratio of the titanium gypsum and the sulfuric acid solution is 10 g:100 mL; and the drying temperature is 100°C.
5. The preparation method according to claim 1, characterized in that: The mechanical grinding and mixing compounding step comprises: stirring titanium gypsum and straw in a closed manner, and fully mixing them to complete the mechanical grinding and mixing compounding.
6. The preparation method according to claim 1, characterized in that: The oxygen-limited pyrolysis step parameters are: heating to 800° C. at a heating rate of 20° C. / min, keeping the temperature for 1 hour, and then cooling to room temperature to complete the oxygen-limited pyrolysis.
7. Titanium gypsum composite biochar prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the titanium gypsum composite biochar as claimed in claim 7 as a passivating agent in repairing heavy metal pollution in soil or reducing the arsenic content in edible parts of plants.
9. An application of the titanium gypsum composite biochar as claimed in claim 7 as a passivating agent coupled with water and fertilizer regulation in repairing soil heavy metal pollution or reducing the arsenic content in edible parts of plants.
Citation Information
Patent Citations
Method for preparing magnetic biochar from titanium gypsum
CN115400729A
Porous biochar prepared from red gypsum and crop straw and application of porous biochar in heavy metal adsorption
CN116173901A
Titanium gypsum modified biochar for heavy metal adsorption and preparation method thereof
CN117046440A
Method for improving saline alkali soil by compounding charcoal-based material with sulfur
CN118048157A
Cited By
Method for synergistically improving soil carbon sequestration yield and efficiency by using modified carbon material
CN120153800A
Titanium gypsum biochar composite material as well as preparation method and application thereof
CN122006664A