Multi-element nitroalloy cored wire and application thereof in steel
Through the design of multi-element nitride alloy core wire, the use of multi-element wire core powder and control of void volume, the existing nitride alloy core wire is solved. The alloy utilization rate and unstable strengthening effect in steel smelting are low. The problem has achieved efficient steel reinforcement and cost reduction.
Patent Information
- Application Number
- CN202411095729.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The existing nitrogen alloy core wire is poorly used in steel smelting, has low alloy utilization, unstable reinforcement effect, high cost, and insufficient improvement effect on steel performance.
The multi-element nitrogen alloy core wire is used to enclose the storage cavity through an outer sheath formed by a metal belt, fill the granular or powdered wire core powder composed of multi-elements, control the proportion of void volume, and contains 13-32% nitrogen. Elements, 21-60% silicon and 0-27% vanadium, rare earth and alkaline earth metal elements, the outer sheath material is aluminum, low carbon steel or pure iron, with a thickness of 0.2-2.0mm, and the wire core powder material accounts for 23-82% of the total weight to improve the yield and melting efficiency of the nitride alloy.
The yield and melting efficiency and stability of the nitride alloy are improved, the strength, yield strength and impact toughness of the steel are enhanced, the decomposition situation is reduced, the utilization rate of alloy elements is improved, and the cost of use is reduced.
Smart Images

Figure CN118996049A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nitrided alloy materials, and more specifically, relates to a multi-element nitrided alloy cored wire and application thereof in steel. Background Art
[0002] Nitriding alloy is an alloy widely used in the process of steel smelting. In today's steel production, in order to improve the strength of steel, it is necessary to add alloys such as ferrovanadium or ferroniobium during the steelmaking process to achieve this effect through microalloying. In order to give full play to the microalloying strengthening effect of vanadium and niobium, it is generally necessary to add an appropriate amount of nitriding alloy during steelmaking to form strong carbonitrides with microalloying elements niobium and vanadium, thereby improving the precipitation strengthening and precipitation strengthening effects of microalloying elements. Therefore, nitriding alloys are widely used in steel smelting. At present, nitride alloys are all generated by the reaction of a single element with nitrogen, such as vanadium nitride, silicon nitride, manganese nitride, titanium nitride, chromium nitride, boron nitride, niobium nitride and other nitride alloys. In metallurgy, when producing steels with special performance requirements such as high strength, wear resistance and corrosion resistance, molten steel micro-alloying technology is usually used. For example, when producing high-strength corrosion-resistant steel, single-element nitride alloys are usually added under appropriate steelmaking processes. However, the above method has the following outstanding problems: first, the effective utilization rate of the alloy is low; second, the addition time, addition order and addition amount ratio of multiple varieties of single-element nitride alloys put forward stringent requirements on the design and implementation of the steelmaking process; third, the strengthening effect on steel performance is insufficient and unstable; fourth, the cost of use is high.
[0003] There are three main methods for vanadium-nitrogen microalloying: 1) adding vanadium-nitrogen alloy; 2) adding ferrovanadium and adding nitrogen-increasing agents (such as silicon-nitrogen alloy) during the smelting process; 3) adding ferrovanadium and blowing nitrogen or adding nitriding alloy during the smelting process.
[0004] Among them, the cored wire technology is a technical method for adding nitride alloys into molten steel. Its use process is to first crush various additive raw materials (such as deoxidizer, desulfurizer, modifier, alloy material, etc.) to be added to the molten steel or molten iron into powders of a certain particle size, and then wrap it with a cold-rolled low-carbon steel (or non-ferrous metal) strip to form a composite material (i.e., cored wire) of any length. Then, with the help of a wire feeder, the cored wire of a specified length is fed into the ladle through the slag layer at a certain speed and inserted into the molten steel to a certain depth. As the cored wire continues to melt at a certain place, the additives wrapped by it will also be continuously melted into the molten steel or molten iron, interacting with the surrounding molten steel or molten iron, and deoxidizing, desulfurizing, micro-alloying, fine-tuning the composition, and modifying the treated molten liquid, so as to achieve the purpose of improving the performance of the treated metal and improving its cleanliness.
[0005] There are related technical solutions for cored wires, such as: Chinese patent application No. 201210377151.X, the invention name disclosed on October 8, 2012 is: A technical solution for a cored wire with vanadium nitrogen microalloying and composite deoxidation for metallurgy; Chinese patent application No. 201410131544.1, the invention name disclosed on April 3, 2014 is: A technical solution for silicon manganese nitride cored wire for nitrogen enhancement of vanadium microalloyed steel; Chinese patent application No. 201320280835.8, the invention name disclosed on May 22, 2013 is: A technical solution for a cored wire with vanadium nitrogen microalloying and composite deoxidation for metallurgy.
[0006] However, the performance of the core-spun wire disclosed in the above patent cannot meet the use requirements, so the structure still needs to be further improved. Summary of the invention
[0007] 1. Problem to be solved
[0008] In view of the problems existing in the existing cored wires, one of the purposes of the present invention is to provide a multi-element nitride alloy cored wire, optimize the structure of the cored wire, and improve the use effect.
[0009] A second object of the present invention is to provide an application in steel, including but not limited to HRB500(E) high-strength earthquake-resistant steel, HRB400(E) steel, HRB600 steel and Q620D steel.
[0010] 2. Technical solution
[0011] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0012] A first aspect of the present invention provides a multi-element nitride alloy cored wire, comprising:
[0013] An outer sheath formed of a metal strip is provided, wherein the outer sheath formed of the metal strip extends along a length direction and is bent to both sides in a width direction to form a receiving cavity;
[0014] Granular and / or powdered wire core powder composed of multiple elements filled in the accommodating cavity, wherein the outer sheath closes the accommodating cavity by a seam or fold extending along the length of the cored wire;
[0015] The volume of the accommodating cavity is composed of the volume of the wire core powder and the void volume, and the void volume accounts for 19-62% per unit length;
[0016] The wire core powder contains 13-32% nitrogen, 21-60% silicon and 0-27% vanadium according to mass fraction.
[0017] According to any embodiment of the first aspect of the present invention, the wire core powder is made of a multi-element nitrided alloy material with a particle size of 0.01-5.5 mm.
[0018] According to any embodiment of the first aspect of the present invention, it also contains rare earth elements and / or alkaline earth metal elements, wherein the rare earth elements include Ce, La, Pr, Nd and Sm, and the content thereof does not exceed 20%; the alkaline earth metal elements include beryllium, magnesium, calcium, strontium and barium, and the content thereof does not exceed 12%.
[0019] According to any embodiment of the first aspect of the present invention, the metal strip of the outer sheath is made of aluminum, low carbon steel or pure iron, wherein the thickness of the outer sheath is 0.2-2.0 mm, preferably, the thickness of the outer sheath is 0.2-0.8 mm or 0.8-1.2 mm or 1.2-2.0 mm.
[0020] According to any embodiment of the first aspect of the present invention, the granular and / or powdered core powder accounts for 23% to 82% of the total cored wire weight per unit length.
[0021] According to any embodiment of the first aspect of the present invention, the outer sheath closes the accommodating cavity by a seam extending along the length of the core wire, so that the cross-sectional shape of the core wire is substantially circular.
[0022] A second aspect of the present invention provides an application of the multi-element nitride alloy material, and the multi-element nitride alloy material can be applied to steel.
[0023] According to any embodiment of the second aspect of the present invention, the application includes using the multi-element nitrided alloy material for smelting high-strength steel, H-shaped steel, and high-chromium cast iron, wherein the high-strength steel includes but is not limited to HRB500 (E) high-strength earthquake-resistant steel, HRB400 (E) steel, HRB600 steel, and Q620D steel. The alloy elements can achieve a strength of 600MPa or more due to the combined effect of solid solution strengthening and nitrided alloy precipitation strengthening. The yield strength of special steel can reach a very high level, while the elongation exceeds 40%, the necking exceeds 60%, and the impact toughness is greater than 150KJ / cm 2 , magnetic permeability is less than 1.01Gs / E, high corrosion resistance.
[0024] 3. Beneficial effects
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) In the multi-element nitride alloy cored wire of the present invention, especially when the cored wire is in a closed state, the air in the void volume will participate in the reaction, thereby reducing the yield of the nitride alloy. By controlling the proportion of the void volume, the yield of the nitride alloy is improved.
[0027] (2) The multi-element nitride alloy cored wire of the present invention can bring the multi-element nitride alloy powder into the deep melting of molten steel, thereby improving the melting efficiency of the nitride alloy, improving the yield of the nitride alloy, and ensuring the stability of the strengthening effect of the nitride alloy on steel.
[0028] (3) The core powder of the multi-element nitride alloy cored wire of the present invention improves the ratio of each component, stabilizes the proportion of each component, ensures the stability of the melting point of the material, effectively reduces the decomposition of the nitride alloy, and avoids boiling of the molten steel due to decomposition; the melting rate of the nitride alloy is improved, the strengthening effect is good, and the utilization rate of the alloy elements is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but it should be understood that these drawings are designed only for explanation purposes and are not intended to limit the scope of the present invention. In addition, unless otherwise specified, these drawings are intended only to conceptually illustrate the structural configurations described herein and are not necessarily drawn to scale.
[0030] Figure 1 This is a scanning electron microscope image of the nitrided alloy block after crushing according to Example 1 of the present invention;
[0031] Figure 2 This is a physical picture of the nitride alloy compact according to Example 1 of the present invention;
[0032] Figure 3 This is a real picture of the load-bearing mold subjected to nitriding treatment according to the present invention.
[0033] Figure 4 This is a physical picture of Example 1 of the nitride alloy cored wire of the present invention;
[0034] Figure 5 This is a schematic structural diagram of Example 1 of the nitride alloy cored wire of the present invention;
[0035] Figure 6 This is a schematic structural diagram of Example 2 of the nitride alloy cored wire of the present invention;
[0036] Figure 7 It is a schematic structural diagram of Example 2 of the nitride alloy cored wire of the present invention.
[0037] Description of reference numerals:
[0038] 100, outer sheath; 110, accommodating cavity; 111, gap; 120, seam; 130, folded edge; 200, wire core powder. DETAILED DESCRIPTION
[0039] The present disclosure may be more easily understood by reference to the following description in conjunction with the accompanying drawings and examples, all of which constitute a part of the present disclosure. It should be understood that the present disclosure is not limited to the specific products, methods, conditions or parameters described and / or shown herein. Further, the terms used herein are only used for the purpose of describing specific embodiments by way of example and are not intended to be limiting unless otherwise stated.
[0040] It should also be understood that, for the sake of clarity, certain features of the present disclosure may be described herein in the context of separate embodiments, but may also be provided in combination with each other in a single embodiment. That is, unless clearly incompatible or specifically not included, each separate embodiment is considered to be combinable with any other embodiment, and the combination is considered to represent another different embodiment. Conversely, for the sake of simplicity, the various features of the present disclosure described in the context of a single embodiment may also be provided individually or in any sub-combination. Finally, although a particular embodiment may be described as part of a series of steps or part of a more general structure, each step or substructure itself may also be considered to be an independent embodiment.
[0041] Unless otherwise indicated, it should be understood that each individual element in a list and each combination of individual elements in the list will be interpreted as a different embodiment. For example, a list of embodiments represented as "A, B, or C" should be interpreted to include embodiments "A", "B", "C", "A or B", "A or C", "B or C", or "A, B, or C".
[0042] In the present disclosure, the singular forms of the articles "a," "an," and "the" also include the corresponding plural references, and a reference to a specific value includes at least that specific value unless the context clearly indicates otherwise. Thus, for example, a reference to "a substance" is a reference to at least one of that substance and equivalents thereof.
[0043] The terms including ordinal numbers such as "first" and "second" can be used to explain various components or fluids, but these components and fluids are not limited by these terms. Therefore, without departing from the teachings of the present disclosure, these terms are only used to distinguish the component / fluid from another component / fluid.
[0044] When items are described by using the conjunction terms "... and / or...," etc., the description should be understood to include any one of the associated listed items and all combinations of one or more thereof.
[0045] In general, the use of the term "about" indicates an approximate value that may vary depending on the desired properties obtained by the disclosed subject matter, and will be interpreted in a context-dependent manner based on function. Therefore, one of ordinary skill in the art will be able to interpret a certain degree of difference on a case-by-case basis. In some cases, the number of significant figures used when expressing a particular value can be a representative technique for determining the difference allowed by the term "about". In other cases, a gradient in a range of values can be used to determine the range of differences allowed by the term "about". Further, all ranges in this disclosure are inclusive and combinable, and reference to the values stated in the range includes each value within the range.
[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the terms used herein and / or include any and all combinations of one or more of the associated listed items.
[0047]
Wire core powder
[0048] The wire core powder of the present invention satisfies at least one of the following conditions:
[0049] 1) According to the mass fraction, it contains 13-32% nitrogen, specifically 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%; 21-60% silicon, specifically 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, 101%, 102%, 103%, 104%, 105%, 106%, 107%, 108%, 109%, 110%, 111%, 112%, 113%, 114%, 115%, 11 0%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60% silicon; 0-27% vanadium, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27% vanadium;
[0050] 2) It also contains 0-19% titanium, specifically 0, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, and 19%.
[0051] 3) It also contains rare earth elements and / or alkaline earth metal elements, the rare earth elements include Ce, La, Pr, Nd and Sm, the content of which does not exceed 20%, specifically 0, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%; the alkaline earth metal elements include beryllium, magnesium, calcium, strontium and barium, the content of which does not exceed 12%, specifically 0, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%.
[0052] [Preparation method of wire core powder]
[0053] The preparation method of the wire core powder of the present invention comprises the following steps:
[0054] Step S1, selecting raw materials: ferrovanadium, vanadium pentoxide, vanadium-containing slag, ferrosilicon, metallic silicon or ferrotitanium;
[0055] Step S2, crushing the materials selected in step S1 respectively, and then grinding them to a particle size of 120-600 mesh;
[0056] Step S3, the raw material fine powders obtained in step S2 are batched according to the above mass fractions (21-60% silicon, 0-27% vanadium, 0-19% titanium), and then 2-3% of a binder and 2-27% of a reducing agent are added to the total raw material fine powder, mixed and pressed into blocks using a strong ball press at a pressure greater than 100 MPa;
[0057] Step S4, placing the compact obtained in step S3 into a pretreatment furnace, heating it to 680-750°C for insulation, and filling the furnace with protective gas (argon-nitrogen mixed gas, wherein the purity of Ar gas is ≥99%, and the purity of N2 is ≥98%), and pretreating for 3-5 hours; the pretreatment furnace includes a vacuum furnace, etc.;
[0058] Step S5, placing the pretreated compact into a nitriding furnace for nitriding treatment;
[0059] Step S6: After the nitriding treatment is completed, the alloy is naturally cooled slowly in the furnace to below 300° C., and then taken out of the furnace and cooled to room temperature to obtain a multi-element nitrided alloy with a particle size of 3-70 mm.
[0060] Furthermore, the binder is: polyborosiloxane, borax, polymer resin, carboxymethyl cellulose, butyl stearate, polyvinyl alcohol, sodium polystyrene sulfonate and polyacrylamide; the reducing agent is graphite carbon or metal aluminum or metal silicon.
[0061] The nitriding process first converts nitrogen (N2) into ionized nitrogen, and the furnace is evacuated to a vacuum for 10 -2 -10-3 Torr (mmHg), then N2 gas or N2+Ar mixed gas is introduced, the furnace body is connected to the anode, the mold (made of metal ceramic) carrying the briquette is connected to the cathode, and a DC voltage of 100-1000 volts is passed between the two electrodes, so that the N2 gas in the furnace undergoes glow discharge to form positive ions, which move to the surface of the material briquette. In an instant, the cathode voltage drops sharply, causing the positive ions to rush to the surface of the briquette at high speed, and produce nitriding effect with the V, Si and other elements of the briquette, and react for 0.5-2 hours; secondly, nitrogen is introduced into the nitriding furnace with a pressure of ≥0.15Mpa, and the temperature is first raised to 900℃ and kept for 3 hours, then raised to 1150℃ and kept for 10 hours, and then continued to rise to 1350℃ and kept for 7 hours, until it is heated to 1500℃ and kept for 11 hours.
[0062] The present invention causes N2 gas to glow discharge to form nitrogen positive ions. These nitrogen positive ions have good activity and can react with elements such as V and Si in the compact to accelerate the reaction rate and produce good application effects.
[0063] The inventors were surprised to find that the alloy material obtained from the above-mentioned nitrided alloy has good nitriding uniformity. The reason for this is that the graphite mold has an internal cavity shape (the shape of the cavity is square or circular), and the heating effect of the glow discharge heat-affected zone in the cavity is superimposed to make the temperature of the upper and lower parts and the inside and outside of the compact in the mold more consistent, thereby improving the problem of insufficient uniformity of the reaction temperature of the compact.
[0064] In addition, through a large number of experimental analyses, it was found that when the cooling rate is controlled to be less than 3°C / s during the cooling process, the alloy block is prone to stick to the nitriding mold (the granular material is added to the graphite mold for nitriding treatment); when the cooling rate is controlled to be greater than 5°C / s during the cooling process, pits or grooves are easily formed on the surface of the alloy block, which is not conducive to moisture prevention.
[0065] Through a large number of experiments, it was found that the glow discharge + nitrogen high-temperature nitriding (which can react the raw materials inside the compact) is carried out, the combination ratio of nitrogen and other elements is reasonable, that is, the nitrogen proportion in the nitrided alloy is well adjustable; the bonding strength between nitrogen and the elements is appropriate, that is, the nitrided alloy has good machinability; the bonding structure between nitrogen and the elements is stable, that is, the nitrided alloy is not easy to decompose at high temperature.
[0066]
Nitride alloy material testing method
[0067] 1. Detection of silicon nitride, vanadium nitride and nitrides
[0068] The standards involved in the content detection include: (1) GB / T 20567-2020 "Vanadium Nitrogen Alloy"; (2) GB / T24583.1-2019 "Vanadium Nitrogen Alloy - Determination of Vanadium Content - Ammonium Ferrous Sulfate Titration Method"; (3) GB / T 24583.2-2019 "Vanadium Nitrogen Alloy - Determination of Nitrogen Content - Inert Gas Melting Thermal Conductivity Method"; (4) GB / T 24583.8-2019 "Vanadium Nitrogen Alloy - Determination of Silicon, Manganese, Phosphorus and Aluminum Content - Inductively Coupled Plasma Atomic Emission Spectrometry"; (5) GB / T 37258-2018 "Silicon Nitride Ceramic Powder".
[0069] 2. Phase detection of silicon nitride and vanadium nitride
[0070] For the nitride alloy material of the present invention, the X-ray diffractometer is used for phase qualitative analysis and quantitative analysis. Through phase qualitative analysis, the measured lattice plane spacing and diffraction intensity of the material are compared with the diffraction data of the standard phase to determine the phases present in the material; according to the intensity of the diffraction pattern, the content of each phase in the material is determined.
[0071] [Application in steel] The multi-element nitride alloy material can be used in steel, especially special steel; the application includes using the multi-element nitride alloy material to smelt high-strength steel, H-shaped steel, and high-chromium cast iron, wherein the high-strength steel includes but is not limited to HRB500(E) high-strength earthquake-resistant steel, HRB400(E) steel, HRB600 steel, and Q620D steel.
[0072] Since nitrogen in cast iron alloys is almost completely absorbed, the nitrogen content in steel can be predicted with high accuracy. However, a high degree of assimilation of this method can be achieved by introducing large amounts of nitride-forming elements: silicon, vanadium and titanium.
[0073] The main components of the alloy material include silicon nitride, titanium nitride, vanadium nitride, silicon vanadium nitride, vanadium titanium nitride, silicon iron nitride, etc. Microalloyed steel containing vanadium, titanium and nitrides inhibits grain growth when heated, refines austenite grains, and refines martensite and bainite grains. The stability of supercooled austenite not only determines the hardenability during quenching to form martensite, but also forms bainite during air cooling. Nitrogen and vanadium steels have a narrow temperature range for the formation of bainite, a uniform structure, and uniform distribution of the finest bainite grains and dispersed cementite particles.
[0074] Silicon is added as a reducing agent and deoxidizer during the steelmaking process, so killed steel contains 0.15-0.30% silicon. If the silicon content in steel exceeds 0.50-0.60%, silicon is considered an alloying element. Silicon can significantly improve the elastic limit, yield point and tensile strength of steel, so it is widely used to make spring steel. Adding 1.0-1.2% silicon to quenched and tempered structural steel can increase the strength by 15-20%. Silicon combined with molybdenum, tungsten, chromium, etc. has the effect of improving corrosion resistance and oxidation resistance, and can be used to make heat-resistant steel. Low carbon steel containing 1-4% silicon has extremely high magnetic permeability and is used in the electrical industry to make silicon steel sheets. The increase in silicon content will reduce the welding performance of steel.
[0075] In microalloyed steels, all the beneficial effects of nitrogen are in its interaction with microalloying elements, where it takes the form of precipitation reactions in ferrite to form chlorides or carbides. The efficiency of any precipitation reaction depends on the degree of dispersion and particle size. Nitrides of microalloying elements are more stable than carbides and have a lower tendency to aggregate. Adding nitrogen will maximize the ratio of particle volume fraction to particle size, thereby maximizing the key microstructure of microalloyed steels, namely grain refinement and precipitation strengthening. Nitride particles can increase the austenite grain refinement temperature during heating, prevent grain growth during rolling, delay recrystallization, increase phase transformation ratio, and increase precipitation strengthening.
[0076] Titanium is the main microalloying element of early microalloyed steel. In the past, there were many titanium-containing steels in the steel material standards, such as my country's 15MnTi, 13MnTi, 15MnVTi, 20Ti, 10Ti, etc. Adding trace amounts of titanium to low-alloy high-strength steel can improve the strength of the steel and improve the cold forming and welding properties of the steel. Due to the high chemical activity of titanium, it is easy to form compounds with N, O, C, S, etc. in steel. Titanium has a strong affinity with oxygen, and the molten steel must be fully deoxidized with aluminum before titanium can be added. Titanium exists in steel mainly in the form of TiC or T (C, N). The solid solution temperature of titanium is slightly lower than that of niobium, that is, at the same solid solution temperature, titanium dissolves more than niobium. Titanium has the function of preventing the recrystallization of deformed austenite and can refine the grains; in addition, Ti has the function of promoting the formation of granular bainite, and is used in low-carbon bainite non-quenched and tempered steel with controlled rolling and controlled cooling. Titanium forms TiN which is very stable at high temperature, and inhibits the grain growth of austenite during the reheating process before hot working. The solid solubility of titanium is very low. Only when the titanium content of steel is appropriate (0.01% to 0.02%) can it meet all requirements at the same time. A lower titanium content will not be able to obtain a sufficient volume fraction of TiN to effectively prevent grain coarsening. Although a higher titanium content will lead to the appearance of coarse liquid precipitated TiN and will not play a role in preventing grain growth, titanium that exceeds the ideal chemical ratio of w(Ti) / w(N) will significantly prevent recrystallization in the form of solid solution titanium or fine TiC particles, playing a precipitation strengthening role. Titanium can also be used as a sulfide modifier in steel to improve the poor longitudinal and transverse properties of steel plates.
[0077] The alloying element vanadium exists in the steel mainly in the form of carbon and nitride in the matrix and grain boundaries, which plays a role in precipitation strengthening and inhibiting grain growth. The solubility of vanadium in ferrite is much smaller than that in austenite. As the phase transformation proceeds, under certain thermodynamic and kinetic conditions, the carbon and nitride of vanadium precipitate at the phase boundary. By accelerating cooling in the two-phase region, the grains can be refined and the precipitation of carbon and nitride can be controlled. The size and distribution of the precipitate determine the effect of precipitation strengthening. Since vanadium and nitrogen have a strong affinity, adding a certain amount of nitrogen while adding a certain amount of vanadium can make its strengthening effect more effective.
[0078] Example 1
[0079] like Figure 1 and Figure 2 As shown, the nitride alloy cored wire of the present embodiment includes an outer sheath 100 formed by a metal strip, wherein the outer sheath 100 formed by a metal strip extends along the length (X) direction and is bent to both sides in the width (Y) direction to form a receiving cavity 110; the specific metal strip can be in the form of a continuous metal strip, which is initially flat (for example, a flat cross-section), which can be formed by roll forming to shape the contour of the metal strip and finally form a surrounding tubular shape to completely surround (form a seam); a granular and / or powdered wire core powder 200 composed of multiple elements is filled in the receiving cavity 110.
[0080] The granular and / or powdered wire core powder 200 includes vanadium nitride, silicon nitride, titanium nitride, etc. The method for preparing the wire core powder includes the following steps:
[0081] Step S1, selecting raw materials: ferrovanadium, vanadium pentoxide, vanadium-containing slag, ferrosilicon, metallic silicon or ferrotitanium;
[0082] Step S2, crushing the materials selected in step S1 respectively, and then grinding them to a particle size of 120-600 mesh;
[0083] Step S3, the raw material fine powders obtained in step S2 are batched according to the above mass fractions (21-60% silicon, 0-27% vanadium, 0-19% titanium), and then 3% of polyborosiloxane and 25% of graphite carbon reducing agent accounting for the total raw material fine powder mass fraction are added, mixed and pressed into blocks at a pressure of 110 MPa using a strong ball press;
[0084] Step S4, placing the compact obtained in step S3 into a pretreatment furnace and heating it to 700°C for insulation, and filling the furnace with protective gas (argon-nitrogen mixed gas, wherein the purity of Ar gas is 99% and the purity of N2 is 99%), and pretreating for 5 hours;
[0085] Step S5, placing the pretreated compact into a nitriding furnace for nitriding treatment; the nitriding process converts nitrogen (N2) into ionized nitrogen, and the furnace is evacuated to a vacuum for 10 -2 Torr (mmHg) and then N2 gas is introduced, the furnace body is connected to the anode, the graphite mold carrying the briquette is connected to the cathode, and a DC voltage of 400 volts is applied between the two electrodes. At this time, the N2 gas in the furnace undergoes glow discharge to form positive ions, which move to the surface of the material briquette. Instantaneously, the cathode voltage drops sharply, causing the positive ions to rush to the cathode surface at high speed and produce nitriding reaction with the briquette, reacting for 0.5 hours; secondly, nitrogen is introduced into the nitriding furnace with a pressure of ≥0.15Mpa, firstly the temperature is raised to 900℃ and kept for 3 hours, then raised to 1150℃ and kept for 10 hours, and then continued to rise to 1350℃ and kept for 7 hours, until it is heated to 1500℃ and kept for 11 hours;
[0086] Step S6, after the nitriding treatment is completed, the alloy is naturally cooled slowly in the furnace to below 300°C, the cooling rate is controlled to 3°C / s, and then taken out of the furnace and cooled to room temperature to obtain a multi-element nitrided alloy with a particle size of 3-70mm;
[0087] Step S7, further making the 3-70 mm multi-element nitrided alloy into 0.01-5.5 mm granular and / or powdered wire core powder 200, and then winding and coating it with a steel strip.
[0088]
Nitride alloy material testing method
[0089] 1. Detection of silicon nitride, vanadium nitride and nitrides
[0090] The standards involved in the content detection include: (1) GB / T 20567-2020 "Vanadium Nitrogen Alloy"; (2) GB / T24583.1-2019 "Vanadium Nitrogen Alloy - Determination of Vanadium Content - Ammonium Ferrous Sulfate Titration Method"; (3) GB / T 24583.2-2019 "Vanadium Nitrogen Alloy - Determination of Nitrogen Content - Inert Gas Melting Thermal Conductivity Method"; (4) GB / T 24583.8-2019 "Vanadium Nitrogen Alloy - Determination of Silicon, Manganese, Phosphorus and Aluminum Content - Inductively Coupled Plasma Atomic Emission Spectrometry"; (5) GB / T 37258-2018 "Silicon Nitride Ceramic Powder".
[0091] 2. Phase detection of silicon nitride and vanadium nitride
[0092] For the nitride alloy material of the present invention, the X-ray diffractometer is used for phase qualitative analysis and quantitative analysis. Through phase qualitative analysis, the measured lattice plane spacing and diffraction intensity of the material are compared with the diffraction data of the standard phase to determine the phases present in the material; according to the intensity of the diffraction pattern, the content of each phase in the material is determined.
[0093] The nitriding uniformity of the alloy material obtained by the above-mentioned nitrided alloy is better than that of the prior art. Through on-site observation and records, a superimposed heating effect is generated in the cavity, which makes the temperature of the upper and lower parts and the inside and outside of the pressing block in the mold more consistent, improving the problem of insufficient uniformity of the reaction temperature of the pressing block.
[0094] The outer sheath 100 encloses the accommodating cavity 110 by a seam 120 extending along the length of the cored wire; the volume of the accommodating cavity 110 is composed of the volume of the core powder 200 and the volume of the gap 111; for the above-mentioned volume of the accommodating cavity 110, the volume of the core powder 200 and the volume of the gap 111, the unit length (1m) can be used to first measure the volume of the accommodating cavity 110, then measure the volume of the core powder 200, and then calculate the difference to obtain the corresponding data ratio.
[0095] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was selected to be 13 mm. After measuring the unit length (the length was 1 m), the average volume proportion of the gaps 111 was 19%.
[0096] Serial number <![CDATA[Volume of accommodation cavity / m 3 > <![CDATA[Void volume / m 3 > Proportion / % 1# <![CDATA[132.75*10 -6 ]]> <![CDATA[26.948*10 -6 ]]> 20.3 2# <![CDATA[132.69*10 -6 ]]> <![CDATA[25.343*10 -6 ]]> 19.1
[0097] Since most of the wire core powder 200 is in granular or powder form, the cored wire is usually not 100% filled, and the voids 111 in the cored wire are too high, which will affect the reaction of the cored wire in the steel, especially when the cored wire is in a closed state, the air in the volume of the voids 111 will participate in the reaction, thereby reducing the yield of the nitride alloy.
[0098] In this embodiment, the metal strip of the outer sheath 100 is made of low carbon steel so that the composition of the finished steel is interfered as little as possible by the carbon in the outer sheath 100; wherein the thickness of the outer sheath 100 is 0.2 mm, 0.5 mm, 0.8 mm, 1 mm or 1.5 mm.
[0099] In addition, the cored wires of the same batch were cut and weighed in unit length to obtain: the average value of the granular and / or powdered core powder 200 accounting for about 75% of the total cored wire weight.
[0100] Combined with Figure 1 As shown, the outer sheath 100 closes the accommodating cavity 110 by a seam 120 extending along the length of the core-covered wire, so that the cross-sectional shape of the core-covered wire is substantially circular.
[0101] Example 2
[0102] like Figure 3 and Figure 4 As shown, the structure of this embodiment is basically the same as that of Embodiment 1, except that the outer sheath 100 closes the accommodating cavity 110 by a folded edge 130 extending along the length of the cored wire.
[0103] The granular and / or powdered wire core powder 200 includes at least one nitride or nitride alloy, and the nitride includes vanadium nitride, silicon nitride, etc. The preparation method of the wire core powder 200 includes the following steps:
[0104] Step S1, selecting raw materials: ferrovanadium, vanadium pentoxide, ferrosilicon, metallic silicon or ferrotitanium;
[0105] Step S2, crushing the materials selected in step S1 respectively, and then grinding them to a particle size of 120-600 mesh;
[0106] Step S3, the raw material fine powders obtained in step S2 are mixed according to the above mass fractions (21-60% silicon, 0-27% vanadium, 0-19% titanium), and then 2% of polyborosiloxane and 3% of graphite carbon reducing agent are added to the total raw material fine powder, mixed and pressed into blocks with a strong ball press at a pressure of 100 MPa;
[0107] Step S4, placing the pressed blocks obtained in step S3 into a pretreatment furnace, heating them to 750°C for insulation, and filling the furnace with protective gas for pretreatment for 4 hours;
[0108] Step S5, placing the pretreated compact into a nitriding furnace for nitriding treatment; the nitriding process converts nitrogen (N2) into ionized nitrogen, and the furnace is evacuated to a vacuum for 10 -3 Torr (mmHg) and then N2 gas is introduced, the furnace body is connected to the anode, the graphite mold carrying the pressed block is connected to the cathode, and a DC voltage of 500 volts is applied between the two electrodes. At this time, the N2 gas in the furnace undergoes glow discharge to form positive ions, which move to the surface of the material pressed block. Instantaneously, the cathode voltage drops sharply, causing the positive ions to rush to the cathode surface at high speed and produce nitriding reaction with the pressed block; react for 1 hour; secondly, nitrogen is introduced into the nitriding furnace with a pressure of ≥0.15Mpa, firstly the temperature is raised to 900℃ and kept for 3 hours, then raised to 1150℃ and kept for 10 hours, and then continued to rise to 1350℃ and kept for 7 hours, until it is heated to 1500℃ and kept for 11 hours;
[0109] Step S6: After the nitriding treatment is completed, the alloy is naturally cooled slowly in the furnace to below 300° C., and then taken out of the furnace and cooled to room temperature to obtain a multi-element nitrided alloy with a particle size of 3-70 mm.
[0110]
Nitride alloy material testing method
[0111] 1. Detection of silicon nitride, vanadium nitride and nitrides
[0112] The standards involved in the content detection include: (1) GB / T 20567-2020 "Vanadium Nitrogen Alloy"; (2) GB / T24583.1-2019 "Vanadium Nitrogen Alloy - Determination of Vanadium Content - Ammonium Ferrous Sulfate Titration Method"; (3) GB / T 24583.2-2019 "Vanadium Nitrogen Alloy - Determination of Nitrogen Content - Inert Gas Melting Thermal Conductivity Method"; (4) GB / T 24583.8-2019 "Vanadium Nitrogen Alloy - Determination of Silicon, Manganese, Phosphorus and Aluminum Content - Inductively Coupled Plasma Atomic Emission Spectrometry"; (5) GB / T 37258-2018 "Silicon Nitride Ceramic Powder".
[0113] 2. Phase detection of silicon nitride and vanadium nitride
[0114] For the nitride alloy material of the present invention, the X-ray diffractometer is used for phase qualitative analysis and quantitative analysis. Through phase qualitative analysis, the measured lattice plane spacing and diffraction intensity of the material are compared with the diffraction data of the standard phase to determine the phases present in the material; according to the intensity of the diffraction pattern, the content of each phase in the material is determined.
[0115] The outer sheath 100 encloses the accommodating cavity 110 by a seam 120 extending along the length of the cored wire; the volume of the accommodating cavity 110 is composed of the volume of the core powder 200 and the volume of the gap 111; for the above-mentioned volume of the accommodating cavity 110, the volume of the core powder 200 and the volume of the gap 111, the unit length (1m) can be used to first measure the volume of the accommodating cavity 110, then measure the volume of the core powder 200, and then calculate the difference to obtain the corresponding data ratio.
[0116] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 62%.
[0117] Serial number <![CDATA[Volume of accommodation cavity / m 3 > <![CDATA[Void volume / m 3 > Proportion / % 1# <![CDATA[130.15*10 -6 ]]> <![CDATA[81.05*10 -6 ]]> 62.3 2# <![CDATA[131.98*10 -6 ]]> <![CDATA[81.432*10 -6 ]]> 61.7
[0118] Since most of the wire core powder 200 is in granular or powder form, the cored wire is usually not 100% filled, and the voids 111 in the cored wire are too high, which will affect the reaction of the cored wire in the steel, especially when the cored wire is in a closed state, the air in the volume of the voids 111 will participate in the reaction, thereby reducing the yield of the nitride alloy.
[0119] In this embodiment, the metal belt of the outer sheath 100 is made of a composite layer of low-carbon steel and aluminum, and the aluminum can be used as a deoxidizer; wherein the thickness of the outer sheath 100 is 0.2 mm, 0.5 mm or 0.8 mm.
[0120] In addition, the cored wires of the same batch were cut and weighed per unit length to obtain: the average value of the granular and / or powdered core powder 200 accounting for about 34% of the total cored wire weight.
[0121] Combined with Figure 3 As shown, the outer sheath 100 closes the accommodating cavity 110 by a folded edge 130 extending along the length of the cored wire, so that the cross-sectional shape of the cored wire is substantially circular.
[0122] Example 3
[0123] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 20%.
[0124] Example 4
[0125] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 21%.
[0126] Example 5
[0127] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 22%.
[0128] Example 6
[0129] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 23%.
[0130] Example 7
[0131] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 24%.
[0132] Example 8
[0133] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 25%.
[0134] Example 9
[0135] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 26%.
[0136] Example 10
[0137] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 27%.
[0138] Embodiment 11
[0139] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 28%.
[0140] Example 12
[0141] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 29%.
[0142] Example 13
[0143] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 30%.
[0144] Embodiment 14
[0145] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 31%.
[0146] Embodiment 15
[0147] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 32%.
[0148] Example 16
[0149] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 33%.
[0150] Embodiment 17
[0151] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 34%.
[0152] Embodiment 18
[0153] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 35%.
[0154] Embodiment 19
[0155] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 36%.
[0156] Embodiment 20
[0157] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 37%.
[0158] Embodiment 21
[0159] The cored wire of this embodiment was measured. The effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 38%.
[0160] Embodiment 22
[0161] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 40%.
[0162] Embodiment 23
[0163] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 42%.
[0164] Embodiment 24
[0165] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 45%.
[0166] Embodiment 25
[0167] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 48%.
[0168] Embodiment 26
[0169] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 50%.
[0170] Embodiment 27
[0171] The cored wire of this embodiment was measured. The effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 52%.
[0172] Embodiment 28
[0173] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 55%.
[0174] Embodiment 29
[0175] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 57%.
[0176] Embodiment 30
[0177] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 59%.
[0178] Embodiment 31
[0179] The cored wire of this embodiment was measured, and the effective diameter of the cored wire was 13 mm. After measuring the unit length (1 m), the average volume proportion of the voids 111 was 61%.
Claims
1. A multi-element nitride alloy cored wire, characterized in that: include: An outer sheath formed of a metal strip is provided, wherein the outer sheath formed of the metal strip extends along a length direction and is bent to both sides in a width direction to form a receiving cavity; Granular and / or powdered wire core powder composed of multiple elements filled in the accommodating cavity, wherein the outer sheath closes the accommodating cavity by a seam or fold extending along the length of the cored wire; The volume of the accommodating cavity is composed of the volume of the wire core powder and the void volume, and the void volume accounts for 19-62% per unit length; The wire core powder contains 13-32% nitrogen, 21-60% silicon and 0-27% vanadium according to mass fraction.
2. The multi-element nitride alloy cored wire according to claim 1, characterized in that: It also contains 0-19% titanium.
3. The multi-element nitride alloy cored wire according to claim 1, characterized in that: The wire core powder is made of a multi-element nitrided alloy material with a particle size of 0.01-5.5 mm.
4. The multi-element nitride alloy cored wire according to claim 1, characterized in that: It also contains rare earth elements and / or alkaline earth metal elements, wherein the rare earth elements include Ce, La, Pr, Nd and Sm, with a content not exceeding 20%; the alkaline earth metal elements include beryllium, magnesium, calcium, strontium and barium, with a content not exceeding 12%.
5. The multi-element nitride alloy cored wire according to claim 1, characterized in that: The metal belt of the outer sheath is made of a composite layer of low-carbon steel and aluminum, low-carbon steel or pure iron, wherein the thickness of the outer sheath is 0.2-2.0 mm.
6. The multi-element nitride alloy cored wire according to claim 5, characterized in that: The thickness of the outer sheath is 0.2-0.8 mm or 0.8-1.2 mm or 1.2-2.0 mm.
7. The multi-element nitride alloy cored wire according to any one of claims 1 to 4, characterized in that: The granular and / or powdered core powder accounts for 23% to 82% of the total cored wire weight per unit length.
8. The multi-element nitride alloy cored wire according to claim 5, characterized in that: The outer sheath closes the accommodating cavity by a seam extending along the length of the cored wire, so that the cross-sectional shape of the cored wire is substantially circular.
9. Use of the multi-element nitride alloy cored wire according to any one of claims 1 to 8 in steel.
Citation Information
Cited By
A vanadium-containing polycrystalline alloy cored wire and its application in steel
CN122669165A