Aluminum alloy support with two flattened ends and machining technology and application of aluminum alloy support
By precisely controlling the elemental composition and processing technology of aluminum alloy, the problems in the annealing and flattening process in aluminum alloy bracket processing are solved, the process flow is simplified, the production efficiency and component quality are improved, and the cost is reduced.
Patent Information
- Application Number
- CN202411185061.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-27
AI Technical Summary
In the existing aluminum alloy bracket processing technology, the profile changes in size during the annealing process, cracking and deformation are prone to occur during the flattening process at both ends, and the annealing and offline solution, and the aging process is complex, resulting in an extended production cycle and increased costs.
By precisely controlling the elemental components in aluminum alloys, such as Mg, Si, Fe, Cu, Mn, Cr, Sn, La, the alloy components are designed to improve plasticity and toughness, and the end stamping is directly carried out by using homogeneous insulation and extrusion molding technology. Flattening processing, simplify the heat treatment process, and perform manual aging treatment.
The processing process is simplified, production efficiency is improved, production costs are reduced, profile size changes, cracking and deformation problems are avoided, and the accuracy and mechanical properties of parts are improved.
Smart Images

Figure CN118996178A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloy processing and preparation, and in particular to a low-cost, high-strength, two-end-flattened aluminum alloy bracket and a processing technology and application thereof. Background Art
[0002] Aluminum alloys are widely used in the automotive manufacturing field due to their advantages such as light weight, high strength and good corrosion resistance, especially in the manufacture of automotive structural parts and engine parts. In the processing of aluminum alloys, extrusion molding is an important processing method, which can press aluminum alloy raw materials into profiles of the desired shape through a mold. However, in the subsequent processing of aluminum alloys after extrusion molding, due to their special physical and chemical properties, they are prone to cracking, deformation and other problems. Therefore, the subsequent processing technology of aluminum alloys has become an important research field.
[0003] In the existing technology, automotive aluminum alloy brackets usually adopt the process of extrusion profile-profile annealing-profile flattening processing-parts offline solid solution and aging. In this process, the aluminum alloy raw material is first made into a profile by extrusion molding, and then the profile is annealed to eliminate internal stress, reduce material strength, and improve the plasticity and toughness of the profile. Next, the annealed profile is flattened at both ends to obtain the desired part shape. Finally, the processed parts are subjected to offline solid solution and aging treatment to improve the mechanical properties of the parts.
[0004] However, the existing processing process of automotive aluminum alloy brackets has the following problems: 1) The profile needs to undergo high-temperature heating and slow cooling during the annealing process, which is not only time-consuming and energy-consuming, but also easily causes changes in the profile size, affecting the accuracy of the final parts. 2) During the flattening process at both ends, the solid solution process may cause the internal grain size of the aluminum alloy to increase, thereby causing the plasticity and toughness of the aluminum alloy to decrease, and it is easy to cause cracking, deformation and other problems, which not only affects the quality of the parts, but also increases the difficulty and cost of processing. 3) The annealing plus offline solid solution and aging treatment process is relatively complicated, which not only prolongs the production cycle, but also increases the production cost. Therefore, the existing process needs to be further improved. Summary of the invention
[0005] The purpose of the present invention is to provide a processing technology for a flattened aluminum alloy bracket at both ends that takes into account cost, strength and elongation, and to at least provide a beneficial option or create conditions for solving one or more technical problems existing in the prior art.
[0006] To achieve the above objectives, the present invention adopts the following technical solutions.
[0007] A processing technology for an aluminum alloy bracket with flattened ends, the steps of which are as follows.
[0008] 1) Design alloy composition: By precisely controlling the content of various elements in the aluminum alloy, such as Mg, Si, Fe, Cu, Mn, Cr, Sn, La, etc., the aluminum alloy has good plasticity and toughness, while ensuring that the profile will not crack, deform, or have other problems during subsequent processing.
[0009] Among them, the Mg content is 0.7-1.0wt%, the Si content is 0.7-1.0wt%, and the Mg / Si ratio is controlled at 1.0-1.3. This control is mainly to avoid excessive Si reducing the plasticity of the material, and also to avoid too little Si affecting the strength after aging.
[0010] The Fe content is 0.1-0.3 wt%, and the difference between the Si element content and the Fe element content, the Si-Fe composition control range is 0.5-0.7 wt%. This control is mainly to avoid the influence of too little effective Si content on material strength.
[0011] The Cu content is 0.1-0.3 wt %, mainly to improve the strength of the material; the Mn content is 0.4-0.6wt%, the Cr content is 0.05-0.20wt%, and the La content is 0.05-0.2wt%, among which the composition control range of the sum of the Mn content, Cr content and La content Mn+Cr+La is 0.6-0.8wt%. This control is mainly to increase the recrystallization temperature of the material, reduce the grain size of the material, and thus greatly improve the plasticity of the material; the Sn content is 0.05-0.20wt%, mainly to delay the influence of hardening due to natural aging, and to avoid the influence of long natural aging time on the performance after artificial aging.
[0012] 2) Melting and casting: Put the aluminum alloy material into the melting furnace and heat it to 700-750℃. After heating and melting, the hydrogen content of the aluminum liquid is controlled within 0.15ml / 100g through refining and online degassing. Use a 50-mesh filter plate to filter impurities, and then cast it into a 100mm diameter aluminum rod. Here, a high-precision filter plate is used to filter impurities and strictly control the hydrogen content in the aluminum liquid to ensure the quality of the aluminum liquid, thereby improving the performance of the profile.
[0013] 3) Homogenization and insulation: The aluminum bar is homogenized at a temperature of 550-570°C for 8-10 hours. The cooling rate after homogenization needs to be greater than 300°C / h. By precisely controlling the temperature and time of homogenization and insulation, as well as the subsequent cooling rate, the structure and performance of the profile are ensured to be uniform.
[0014] 4) Extrusion molding: Heat the homogenized aluminum rod to 500-520℃ and put it into the extruder to extrude a round tube bracket profile with a wall thickness of 2mm and an outer diameter of 20mm. The extrusion profile discharge speed is 6-8m / min, the extrusion outlet temperature is ≥530℃, and the material is quickly cooled by water after discharge.
[0015] Use appropriate extrusion temperature and speed, as well as precisely controlled outlet temperature, to ensure accurate size and shape of the profile, while avoiding problems such as cracking and deformation of the profile during the extrusion process.
[0016] 5) End stamping and flattening processing: The end stamping and flattening processing is directly carried out when the profile is not aged, without annealing treatment, which greatly reduces the processing and heat treatment processes, improves production efficiency and reduces production costs.
[0017] 6) Aging treatment: After the parts are processed, they can be directly subjected to artificial aging treatment. The aging temperature is 160-180℃ and the insulation time is 8-10h, which greatly shortens the production cycle and reduces the production cost.
[0018] Through the above technical means, the present invention not only solves the problems that occur in the annealing and flattening processes of profiles in the prior art, but also greatly reduces the processing steps and heat treatment steps, improves production efficiency, reduces production costs, and ensures the quality of parts.
[0019] Compared with the prior art, the present invention mainly solves the following technical problems: 1) It solves the problem that the profile in the prior art needs to undergo high-temperature heating and slow cooling during the annealing process, which is not only time-consuming and energy-consuming, but also easily causes the size of the profile to change, affecting the accuracy of the final parts. 2) It solves the problem that the profile in the prior art is prone to cracking and deformation during the flattening process at both ends due to the low plasticity and toughness of the aluminum alloy, which not only affects the quality of the parts, but also increases the difficulty and cost of processing. 3) It solves the problem that the annealing plus offline solution and aging treatment process in the prior art is complicated, which not only prolongs the production cycle, but also increases the production cost.
[0020] On the other hand, the present invention further provides an aluminum alloy bracket with flattened ends, which is manufactured using the above-mentioned vehicle aluminum alloy bracket processing technology.
[0021] On the other hand, the present invention also provides the use of the aluminum alloy bracket with flattened ends as described above in automobile parts.
[0022] Compared with the prior art, the present invention has the following advantages and beneficial effects.
[0023] 1. The aluminum alloy bracket processing technology provided by the present invention omits the two steps of profile annealing and offline solid solution, greatly simplifies the processing flow, improves production efficiency, and reduces production costs. At the same time, since the heat treatment process is reduced, the quality fluctuations that may be caused by excessive heat treatment are avoided, and the consistency and stability of the product are improved.
[0024] 2. The aluminum alloy bracket processing technology provided by the present invention directly performs flattening processing on both ends after extruding the profile, avoiding the dimensional changes that may occur in the profile during the annealing process, thereby improving the accuracy and consistency of parts.
[0025] 3. The aluminum alloy bracket processing technology provided by the present invention ensures the plasticity and toughness of the aluminum alloy profile by accurately controlling the alloy composition and the smelting and casting process before the flattening process at both ends, thereby reducing problems such as cracking and deformation that may occur during the flattening process at both ends, and improving the quality and yield rate of parts.
[0026] 4. The aluminum alloy bracket processing technology provided by the present invention is placed naturally for 2-7 days before aging treatment to avoid the situation where the hardness is too high during natural aging and affects the effect of artificial aging, thereby improving the effect of aging treatment and further improving the mechanical properties of parts.
[0027] 5. The aluminum alloy bracket processing technology provided by the present invention ensures the structure and performance of the aluminum alloy profile and improves the performance and reliability of the product by accurately controlling the extrusion temperature, speed and outlet temperature, as well as subsequent rapid cooling through water.
[0028] In general, the aluminum alloy bracket processing technology of the present invention not only improves the performance and quality of the product, but also improves the production efficiency and reduces the production cost by optimizing the alloy composition, improving the melting casting and extrusion molding process, simplifying the heat treatment process and other measures, and has significant advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The figure shows a sample of an aluminum alloy bracket for a vehicle with both ends flattened, which is made by using Example 1 of the present invention.
[0030] Figure 2-Figure 3 The sample picture showing cracking in Comparative Example 1 is shown. DETAILED DESCRIPTION
[0031] The specific implementation of the present invention is further described below to make the technical solution and beneficial effects of the present invention clearer and more specific. The following embodiments are exemplary and intended to explain the present invention, but cannot be understood as limiting the present invention.
[0032] Additional aspects and advantages of the present invention will become apparent from the following description or may be learned by practice of the present invention. Example
[0033] A processing technology for a vehicle aluminum alloy bracket with flattened ends, the specific steps are as follows: Step 1: alloy composition design. First, Mg, Si, Fe, Cu, Mn, Cr, Sn, La and other elements are configured in precise proportions, wherein the Mg content is 0.75%, the Si content is 0.73%, the Mg / Si ratio is controlled at 1.03, the Fe content is 0.15%, the Si-Fe content difference is controlled to be 0.58%, the Cu content is 0.28%, the Mn content is 0.45%, the Cr content is 0.12%, the Sn content is 0.10%, the La content is 0.14%, and the content of Mn+Cr+La is controlled to be 0.71%; the remainder is Al; all are calculated by weight percentage.
[0034] Step 2: Melting and casting process. The aluminum alloy material is placed in a melting furnace and heated to 750°C. After heating and melting, the hydrogen content of the aluminum liquid is controlled within 0.15ml / 100g through refining and online degassing. A 50-mesh filter plate is used to filter impurities, and then cast into an aluminum rod with a diameter of 100mm.
[0035] Step 3: Homogenization and heat preservation. The aluminum bar is homogenized at a temperature of 550°C for 8 hours. The cooling rate after homogenization needs to be greater than 300°C / h.
[0036] Step 4: Extrusion molding. The homogenized aluminum rod is heated to 500℃ and put into the extruder to extrude a round tube bracket profile with a wall thickness of 2mm and an outer diameter of 20mm. The extrusion profile discharge speed is 8m / min, the extrusion outlet temperature is ≥530℃, and the material is quickly cooled by water after discharge.
[0037] Step 5: Punching and flattening of the ends. When the profile is not aged, use a punching machine to flatten the two ends of the profile.
[0038] Step 6: Aging treatment. After the parts are processed, they are aged at 170°C for 8 hours.
[0039] The aluminum alloy bracket sample for automobiles with both ends flattened prepared in this embodiment is shown in Figure 1, and there is basically no flattening and cracking phenomenon. Example
[0040] A processing technology for a vehicle aluminum alloy bracket with flattened ends, the specific steps are as follows: Step 1: alloy composition design. First, Mg, Si, Fe, Cu, Mn, Cr, Sn, La and other elements are configured in precise proportions, wherein the Mg content is 0.95%, the Si content is 0.75%, the Mg / Si ratio is controlled at 1.27, the Fe content is 0.2%, the Si-Fe content difference is controlled to be 0.6%, the Cu content is 0.15%, the Mn content is 0.55%, the Cr content is 0.10%, the Sn content is 0.12%, the La content is 0.08%, and the content sum of Mn+Cr+La is controlled to be 0.73%; the remainder is Al; all are calculated by weight percentage.
[0041] Step 2: Melting and casting process. The aluminum alloy material is placed in a melting furnace and heated to 700°C. After heating and melting, the hydrogen content of the aluminum liquid is controlled within 0.15ml / 100g through refining and online degassing. A 50-mesh filter plate is used to filter impurities, and then cast into an aluminum rod with a diameter of 100mm.
[0042] Step 3: Homogenization and heat preservation. The aluminum bar is homogenized at a temperature of 560°C for 8 hours. The cooling rate after homogenization needs to be greater than 300°C / h.
[0043] Step 4: Extrusion molding. The homogenized aluminum rod is heated to 510℃ and put into the extruder to extrude a round tube bracket profile with a wall thickness of 2mm and an outer diameter of 20mm. The extrusion profile discharge speed is 7m / min, the extrusion outlet temperature is ≥530℃, and the material is quickly cooled by water after discharge.
[0044] Step 5: Punching and flattening of the ends. When the profile is not aged, use a punching machine to flatten the two ends of the profile.
[0045] Step 6: Aging treatment. After the parts are processed, they are aged at 170°C for 8 hours. Example
[0046] A processing technology for a vehicle aluminum alloy bracket with flattened ends, the specific steps are as follows: Step 1: alloy composition design. First, Mg, Si, Fe, Cu, Mn, Cr, Sn, La and other elements are configured in precise proportions, wherein the Mg content is 0.93%, the Si content is 0.88%, the Mg / Si ratio is controlled at 1.06, the Fe content is 0.21%, the Si-Fe content difference is controlled to be 0.67%, the Cu content is 0.26%, the Mn content is 0.58%, the Cr content is 0.14%, the Sn content is 0.08%, the La content is 0.06%, and the content of Mn+Cr+La is controlled to be 0.78%; the remainder is Al; all are calculated by weight percentage.
[0047] Step 2: Melting and casting process. The aluminum alloy material is placed in a melting furnace and heated to 730°C. After heating and melting, the hydrogen content of the aluminum liquid is controlled within 0.15ml / 100g through refining and online degassing. A 50-mesh filter plate is used to filter impurities, and then cast into an aluminum rod with a diameter of 100mm.
[0048] Step 3: Homogenization and heat preservation. The aluminum bar is homogenized at a temperature of 565°C for 8 hours. The cooling rate after homogenization needs to be greater than 300°C / h.
[0049] Step 4: Extrusion molding. The homogenized aluminum rod is heated to 515℃ and put into the extruder to extrude a round tube bracket profile with a wall thickness of 2mm and an outer diameter of 20mm. The extrusion profile discharge speed is 6m / min, the extrusion outlet temperature is ≥530℃, and the material is quickly cooled by water after discharge.
[0050] Step 5: Punching and flattening of the ends. When the profile is not aged, use a punching machine to flatten the two ends of the profile.
[0051] Step 6: Aging treatment. After the parts are processed, they are aged at 170°C for 8 hours.
[0052] Comparative Example 1
[0053] A processing technology for a vehicle aluminum alloy bracket with flattened ends, the specific steps are as follows: Step 1: alloy composition design. First, Mg, Si, Fe, Cu, Mn, Cr, Sn, La and other elements are configured in precise proportions, wherein the Mg content is 0.72%, the Si content is 0.88%, the Mg / Si ratio is controlled at 0.82, the Fe content is 0.22%, the Si-Fe content difference is controlled at 0.66%, the Cu content is 0.27%, the Mn content is 0.45%, the Cr content is 0.14%, the Sn content is 0.10%, the La content is 0.10%, and the content of Mn+Cr+La is controlled at 0.69%; the remainder is Al; all are calculated by weight percentage.
[0054] Step 2: Melting and casting process. The aluminum alloy material is placed in a melting furnace and heated to 750°C. After heating and melting, the hydrogen content of the aluminum liquid is controlled within 0.15ml / 100g through refining and online degassing. A 50-mesh filter plate is used to filter impurities, and then cast into an aluminum rod with a diameter of 100mm.
[0055] Step 3: Homogenization and heat preservation. The aluminum bar is homogenized at a temperature of 565°C for 8 hours. The cooling rate after homogenization needs to be greater than 300°C / h.
[0056] Step 4: Extrusion molding. The homogenized aluminum rod is heated to 500℃ and put into the extruder to extrude a round tube bracket profile with a wall thickness of 2mm and an outer diameter of 20mm. The extrusion profile discharge speed is 8m / min, the extrusion outlet temperature is ≥530℃, and the material is quickly cooled by water after discharge.
[0057] Step 5: Punching and flattening of the ends. When the profile is not aged, use a punching machine to flatten the two ends of the profile.
[0058] Step 6: Aging treatment. After the parts are processed, they are aged at 170°C for 8 hours.
[0059] The aluminum alloy bracket for automobiles with flattened ends prepared in this comparative example has cracks. Figure 2 , Figure 3 shown.
[0060] Comparative example 2.
[0061] A processing technology for a vehicle aluminum alloy bracket with flattened ends, the specific steps are as follows: Step 1: alloy composition design. First, Mg, Si, Fe, Cu, Mn, Cr, Sn, La and other elements are configured in precise proportions, wherein the Mg content is 0.86%, the Si content is 0.67%, the Mg / Si ratio is controlled at 1.28, the Fe content is 0.28%, the Si-Fe content difference is controlled to be 0.39%, the Cu content is 0.15%, the Mn content is 0.43%, the Cr content is 0.14%, the Sn content is 0.12%, the La content is 0.08%, and the content sum of Mn+Cr+La is controlled to be 0.63%; the remainder is Al; all are calculated by weight percentage.
[0062] Step 2: Melting and casting process. Put the aluminum alloy material into the melting furnace, heat it to completely melt, control the hydrogen content of the aluminum liquid within 0.15ml / 100g through refining and online degassing, use a 50-mesh filter plate to filter impurities, and then cast it into an aluminum rod with a diameter of 100mm.
[0063] Step 3: Homogenization and heat preservation. The aluminum bar is homogenized at a temperature of 565°C for 8 hours. The cooling rate after homogenization needs to be greater than 300°C / h.
[0064] Step 4: Extrusion molding. The homogenized aluminum rod is heated to 500℃ and put into the extruder to extrude a round tube bracket profile with a wall thickness of 2mm and an outer diameter of 20mm. The extrusion profile discharge speed is 8m / min, the extrusion outlet temperature is ≥530℃, and the material is quickly cooled by water after discharge.
[0065] Step 5: Punching and flattening of the ends. When the profile is not aged, use a punching machine to flatten the two ends of the profile.
[0066] Step 6: Aging treatment. After the parts are processed, they are aged at 170°C for 8 hours.
[0067] Comparative example 3.
[0068] A processing technology for a vehicle aluminum alloy bracket with flattened ends, the specific steps are as follows: Step 1: alloy composition design. First, Mg, Si, Fe, Cu, Mn, Cr, Sn, La and other elements are configured in precise proportions, wherein the Mg content is 0.86%, the Si content is 0.77%, the Mg / Si ratio is controlled at 1.12, the Fe content is 0.20%, the Si-Fe content difference is controlled to be 0.57%, the Cu content is 0.18%, the Mn content is 0.41%, the Cr content is 0.06%, the Sn content is 0.11%, the La content is 0.07%, and the content sum of Mn+Cr+La is controlled to be 0.54%; the remainder is Al; all are calculated by weight percentage.
[0069] Step 2: Melting and casting process. Put the aluminum alloy material into the melting furnace, heat it to completely melt, control the hydrogen content of the aluminum liquid within 0.15ml / 100g through refining and online degassing, use a 50-mesh filter plate to filter impurities, and then cast it into an aluminum rod with a diameter of 100mm.
[0070] Step 3: Homogenization and heat preservation. The aluminum bar is homogenized at a temperature of 565°C for 8 hours. The cooling rate after homogenization needs to be greater than 300°C / h.
[0071] Step 4: Extrusion molding. The homogenized aluminum rod is heated to 500℃ and put into the extruder to extrude a round tube bracket profile with a wall thickness of 2mm and an outer diameter of 20mm. The extrusion profile discharge speed is 8m / min, the extrusion outlet temperature is ≥530℃, and the material is quickly cooled by water after discharge.
[0072] Step 5: Punching and flattening of the ends. When the profile is not aged, use a punching machine to flatten the two ends of the profile.
[0073] Step 6: Aging treatment. After the parts are processed, they are aged at 170°C for 8 hours.
[0074] Comparative example 4.
[0075] A processing technology for a vehicle aluminum alloy bracket with flattened ends, the specific steps are as follows: Step 1: alloy composition design. First, Mg, Si, Fe, Cu, Mn, Cr, Sn, La and other elements are configured in precise proportions, wherein the Mg content is 0.77%, the Si content is 0.72%, the Mg / Si ratio is controlled at 1.07, the Fe content is 0.15%, the Si-Fe content difference is controlled to be 0.57%, the Cu content is 0.22%, the Mn content is 0.47%, the Cr content is 0.10%, the Sn content is 0.02%, the La content is 0.10%, and the content of Mn+Cr+La is controlled to be 0.67%; the remainder is Al; all are calculated by weight percentage.
[0076] Step 2: Melting and casting process. Put the aluminum alloy material into the melting furnace, heat it to completely melt, control the hydrogen content of the aluminum liquid within 0.15ml / 100g through refining and online degassing, use a 50-mesh filter plate to filter impurities, and then cast it into an aluminum rod with a diameter of 100mm.
[0077] Step 3: Homogenization and heat preservation. The aluminum bar is homogenized at a temperature of 565°C for 8 hours. The cooling rate after homogenization needs to be greater than 300°C / h.
[0078] Step 4: Extrusion molding. The homogenized aluminum rod is heated to 500℃ and put into the extruder to extrude a round tube bracket profile with a wall thickness of 2mm and an outer diameter of 20mm. The extrusion profile discharge speed is 8m / min, the extrusion outlet temperature is ≥530℃, and the material is quickly cooled by water after discharge.
[0079] Step 5: Punching and flattening of the ends. When the profile is not aged, use a punching machine to flatten the two ends of the profile.
[0080] Step 6: Aging treatment. After the parts are processed, they are aged at 170°C for 8 hours. Tensile strength after aging MPa Yield strength after aging MPa Elongation after aging % Yield after 2-day flattening 7-day flattening yield 10-day flattening yield Example 1 342 305 13.5 100% 100% 88% Example 2 338 299 14.7 100% 100% 94% Example 3 351 312 14.3 100% 100% 91% Comparative Example 1 345 310 10.2 80% 65% 43% Comparative Example 2 298 261 15.2 100% 100% 98% Comparative Example 3 341 302 13.2 98% 95% 85% Comparative Example 4 332 295 14.2 100% 92% 80% .
[0081] It can be seen from Table 1 that the alloy composition design of the present invention is particular. When one or more of the composition design features change, one or more of the strength, elongation, and flattening yield will deteriorate, and the effect of taking into account the strength, elongation, and flattening yield cannot be achieved.
[0082] Due to the advanced nature of the present invention, it can be widely used in the fields of automobile manufacturing, metal processing and aluminum alloy materials. In the field of automobile manufacturing, the present invention provides a new processing technology for a vehicle aluminum alloy bracket with flattened ends, which can not only improve the mechanical properties of the aluminum alloy bracket, but also greatly reduce the processing procedures of parts and components and reduce production costs. In addition, since aluminum alloy has the advantages of light weight, high strength and good corrosion resistance, the present invention has broad application prospects in the manufacture of automobile structural parts and engine parts. In the field of metal processing, the present invention provides a new processing technology for aluminum alloy profiles, which can not only improve the plasticity and toughness of aluminum alloy profiles, but also avoid problems such as cracking and deformation of profiles during processing. In addition, since aluminum alloy has good machinability, the present invention has broad application prospects in the field of metal processing. In the field of aluminum alloy materials, the present invention provides a new processing technology for aluminum alloy materials, which can not only improve the mechanical properties of aluminum alloy materials, but also avoid problems such as cracking and deformation of aluminum alloy materials during processing. In addition, since aluminum alloy materials have good comprehensive properties, the present invention has broad application prospects in the field of aluminum alloy materials.
[0083] In general, due to its unique process and technical advantages, the present invention can not only improve the quality and performance of aluminum alloy products, but also significantly reduce production costs and improve production efficiency. Therefore, it has broad application prospects and market demand in application fields such as automobile manufacturing, metal processing and aluminum alloy materials.
[0084] It should be noted that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0085] The above embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. The parts not described in the specific embodiments are all prior art or common knowledge.
[0086] It should be noted that, in the description of the present invention, the content of the present invention can be more easily understood by referring to the detailed description of the preferred implementation method of the present invention above and the embodiments included. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those of ordinary skill in the art to which the present invention belongs. When there is a conflict, the definitions in this specification shall prevail.
[0087] In the present invention, the term "prepared from..." is used synonymously with "comprising". The terms "comprising", "including", "having", "containing" or any other variation thereof, as used in the present invention, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0088] In the present invention, when an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range limited by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including a range of "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When a numerical range is described in the present invention, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0089] In addition, the indefinite articles "a" and "an" before the elements or components of the present invention have no restrictions on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number is obviously intended to be in the singular form.
Claims
1. A processing technology for an aluminum alloy bracket with flattened ends, characterized in that: Here are the steps: 1) Design alloy composition: accurately control the content of various elements in the aluminum alloy, among which Mg 0.7-1.0wt%, Si 0.7-1.0wt%, Mg / Si ratio controlled at 1.0-1.3; Fe 0.1-0.3 wt%, the difference between Si and Fe content controlled at 0.5-0.7wt%; Cu 0.1-0.3wt%, Mn 0.4-0.6wt%, Cr 0.05-0.20wt%, La 0.05-0.2wt%, the sum of Mn, Cr and La content controlled at 0.6-0.8wt%; Sn 0.05-0.20wt%; the balance is Al; 2) Melting and casting: Put the aluminum alloy material into the melting furnace, heat it to completely melt, and then control the hydrogen content of the aluminum liquid to less than 0.15ml / 100g through refining and online degassing. Use a filter plate to filter impurities, and then cast it into aluminum rods; 3) Homogenization and insulation: The aluminum rod is homogenized to ensure that the structure and performance of the profile are uniform; 4) Extrusion molding: The homogenized aluminum rod is heated and placed into an extruder to extrude a round tube bracket profile; 5) End stamping and flattening processing: The end stamping and flattening processing is directly carried out when the profile is not aged; 6) Aging treatment: Artificial aging treatment is carried out after the parts are processed.
2. The processing technology of the aluminum alloy bracket with flattened ends according to claim 1 is characterized in that: In the melting and casting step, the heating and melting temperature is 700-750°C.
3. The processing technology of the aluminum alloy bracket with flattened ends according to claim 1 is characterized in that: In the smelting and casting step, the filter plate is a high-precision filter plate with a pore size less than 50 meshes.
4. The processing technology of the aluminum alloy bracket with flattened ends according to claim 1 is characterized in that: In the homogenization and heat preservation step, the homogenization and heat preservation temperature is 550-570°C, the heat preservation time is 8-10h, and the cooling rate after homogenization is greater than 300°C / h.
5. The processing technology of the aluminum alloy bracket with flattened ends according to claim 1 is characterized in that: In the extrusion molding step, the homogenized aluminum rod is heated to 500-520°C and put into the extruder. The extruded profile discharge speed is 6-8m / min, the extrusion discharge port temperature is ≥530°C, and the material is quickly cooled by water after discharge.
6. The processing technology of the aluminum alloy bracket with flattened ends according to claim 1 is characterized in that: In the aging treatment step, the aging temperature is 160-180°C and the insulation time is 8-10h.
7. An aluminum alloy bracket with flattened ends, characterized in that: The bracket is manufactured by using the above-mentioned processing technology of an aluminum alloy bracket with flattened ends.
8. Application of the aluminum alloy bracket with flattened ends as claimed in claim 7 in automobile parts.
Citation Information
Patent Citations
Aluminum alloy and aluminum alloy extruded profile machining method
CN108118210A
Recycled aluminum alloys from manufacturing scrap with cosmetic appeal
CN110819859A
Aluminium alloys
WO2021003528A1
Cited By
High-strength aluminum alloy for 3C electronic products and preparation method of high-strength aluminum alloy
CN121380639A