Ultrafine-grain-size carburizing bearing steel for robot RV speed reducer eccentric shaft and production method of ultra-fine-grain-size carburizing bearing steel

Through the large-section continuous casting blank combined with forging + rolling process and double quenching + tempering and tempering process, the chemical composition and smelting process are optimized, and the problem of insufficient service life of the eccentric shaft material of the RV reducer under high stress environment is solved, and the service life of the eccentric shaft material of the RV reducer is achieved. The effects of high strength, impact toughness and long life reduce production costs.

CN118996249AActive Publication Date: 2024-11-22JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD

Patent Information

Application Number
CN202410877561.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-22
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

The existing RV reducer eccentric shaft materials lack service life in high stress environments, the traditional process has high production costs and high processing energy consumption, making it difficult to meet the needs of high-end fields.

Method used

Using a large-section continuous casting billet combined with forging + rolling process, through double quenching + tempering and tempering, chemical composition and smelting process are optimized, the density, structure uniformity and high-temperature austenite grain size of steel are improved, and the density of steel is improved, so as to reduce the Production cost.

Benefits of technology

It realizes the high strength, impact toughness and long life of steel, broadens the market application of RV reducers, improves the purity and stability of products, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996249A_ABST
    Figure CN118996249A_ABST
Patent Text Reader

Abstract

The invention relates to carburized bearing steel for an eccentric shaft of a robot RV speed reducer with an ultra-fine grain size. The carburized bearing steel comprises the following chemical components: 0.10-0.20% of C, 0.20-0.40% of Si, 0.60-1.00% of Mn, less than or equal to 0.020% of P, less than or equal to 0.015% of S, 1.50-1.80% of Cr, 0.25-0.35% of Mo, 1.40-1.70% of Ni, 0.02-0.05% of Nb, less than or equal to 0.008% of W, less than or equal to 0.002% of Ti, 0.020-0.050% of Al and the balance of Fe and inevitable impurities. The production process comprises the steps of KR molten iron pretreatment, converter treatment, LF external refining, RH vacuum degassing and CCM continuous casting, continuous casting blank slow cooling, continuous casting blank forging to form an intermediate blank, intermediate blank stack cooling, intermediate blank heating and rolling to form a material, rolled material stack cooling, double quenching, tempering treatment of tempering and finishing. According to the carburizing bearing steel for the robot RV speed reducer eccentric shaft, a continuous casting billet is subjected to pit entering slow cooling, an intermediate billet and a rolled material are subjected to stack cooling, and the steel has high hardenability, high mechanical property, fine grain size and high purity and meets the requirements of the carburizing bearing steel for the robot RV speed reducer eccentric shaft.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of special steel smelting, and specifically relates to a carburized bearing steel with ultra-fine grain size for an eccentric shaft of a robot RV reducer and a production method thereof. Background Art

[0002] RV reducers are widely used in heavy load parts such as the arms of industrial robots due to their high precision, large transmission ratio, high transmission efficiency and high load-bearing capacity. The eccentric shaft is the power input component of the RV reducer, and its quality determines the service life of the RV reducer.

[0003] The eccentric shaft of the RV reducer is mostly made of traditional high-carbon chromium bearing steel GCr15 material and hot forging + tempering treatment + turning process. The eccentric shaft of the RV reducer produced by this manufacturing process has high surface wear resistance and uses high-carbon chromium bearing steel to meet the long-life use conditions of the eccentric shaft. However, the eccentric shaft produced by this process can only withstand low stress and cannot meet the requirements of high-end fields such as automobile manufacturing, aerospace, and biomedicine for the eccentric shaft of the RV reducer.

[0004] With the large-scale development of RV reducers, the input end needs to bear more impact stress. Many domestic RV reducer manufacturers use carburized bearing steel as the raw material for the production of eccentric shafts. Usually, 20CrMoH high hardenability carburized bearing steel is used to replace traditional high carbon chromium bearing steel. The manufacturing process is also gradually changed to a new production process of hot forging + high temperature quenching + low temperature tempering + carburizing heat treatment + turning. Carburized bearing steel not only ensures high surface wear resistance but also has a certain core impact toughness, which greatly extends the service life of the RV reducer and meets the extreme use conditions of the eccentric shaft of the RV reducer. The advantage of the new "hot forging" production process is that it does not put forward requirements for raw materials, but there is a bottleneck in the strength of the 20CrMoH material.

[0005] With the rapid development of heat treatment technology in my country, the traditional process of "hot forging" has gradually been replaced by the "cold forging" process. Although the cold forging process can greatly reduce material loss, it also places strict requirements on raw materials. The delivery state of the material usually requires spheroidizing annealing silver bright state, the structure needs to be spheroidized structure, the spheroidization rate ≥ 60%, the hardness ≤ 200HBW, the raw materials need spheroidizing annealing treatment, and quenching + tempering heat treatment is required before carburizing heat treatment, resulting in a long production process and high processing energy consumption of this process, which does not have advantages.

[0006] For the new production process of eccentric shafts, the key lies in the control of the key quality of the raw materials of carburized bearing steel to ensure high strength and impact toughness, as well as extremely fine high-temperature austenite grain size after carburizing treatment. Therefore, the present invention proposes a carburized bearing steel with ultra-fine grain size for the eccentric shaft of a robot RV reducer and a production method thereof. On the one hand, by combining the forging + rolling process, the forging process before the quenching and tempering treatment is reduced, the density and organizational uniformity of the raw materials are improved, and the production cost is reduced. On the other hand, through the innovative proportioning of the chemical composition of the raw materials and the innovative research on the double quenching + tempering process, the mechanical properties of the material are improved, and the austenite grain size after carburizing is refined. Secondly, the key smelting process is optimized, studied and controlled, and by improving the purity of the steel, a long-life, high-stability product is obtained, broadening the market application of RV reducers. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a method for producing carburized bearing steel with ultra-fine grain size for eccentric shaft of robot RV reducer in view of the above-mentioned prior art. By adopting the method of continuous casting billet with large section and combining forging + rolling process, the compactness of the finished steel is ensured; through the innovative research of double quenching + tempering process, the product has fine tempered troostite structure, and the high temperature austenite grain size of the steel is ≥7 levels. At present, there is no product report with similar performance in China. On the basis of ensuring the high surface wear resistance and core impact toughness of the eccentric shaft, the purity and uniformity of the steel are improved, so that the product has strong market competitiveness.

[0008] The technical solution adopted by the present invention to solve the above problems is: a carburized bearing steel for the eccentric shaft of the robot RV reducer with ultra-fine grain size, the chemical composition by mass percentage is: C: 0.10-0.20%, Si: 0.20-0.40%, Mn: 0.60-1.00%, P≤0.020%, S≤0.015%, Cr: 1.50-1.80%, Mo: 0.25-0.35%, Ni: 1.40-1.70%, Nb: 0.02-0.05%, W≤0.008%, Ti≤0.002%, Al: 0.020-0.050%, the remainder is Fe and unavoidable impurities. The chemical composition design basis of the carburized bearing steel for the eccentric shaft of the robot RV reducer of the present invention is as follows:

[0009] (1) Determination of C content

[0010] Increasing the C content in steel can significantly improve the tensile strength, hardness and wear resistance of steel, and C is also the most economical element to improve the hardenability of steel. However, too high C content will also significantly reduce plasticity and impact toughness. The C content of carburized bearing steel for eccentric shaft of RV reducer is generally controlled at about 0.23%. In order to improve the impact toughness of the product, the C content of the present invention is determined to be 0.10% to 0.20%.

[0011] (2) Determination of Si content

[0012] The Si element plays a major role in reducing and deoxidizing during the steelmaking process. Increasing the Si content of steel is beneficial to reducing the oxygen content during the steelmaking process. In killed steel, in order to ensure deoxidation, the Si content is generally 0.15% to 0.30%. Increasing the Si content can significantly increase the elastic limit, yield point and tensile strength of the steel, but too high a Si content will significantly increase the depth of the decarburized layer of the steel. Therefore, the Si content of the present invention is 0.20% to 0.40%.

[0013] (3) Determination of Mn content

[0014] Mn is a good deoxidizing and desulfurizing element. The Mn content in the killed steel is generally controlled between 0.30% and 0.50%. During the smelting process of steel, Mn can form MnS with high melting point with S, thereby weakening and eliminating the hot brittleness caused by S. Mn can also significantly improve the hardenability of steel and the strength of steel. Therefore, the Mn content of the present invention is controlled between 0.60% and 1.00%.

[0015] (4) Determination of P and S content

[0016] The P element causes element segregation during the solidification of steel. It dissolves in ferrite to make the grains distorted and coarse, and increases cold brittleness. Therefore, P is determined to be ≤ 0.020%. The S element tends to make the steel hot brittle, reducing the ductility and toughness of the steel, but the formed sulfide has the effect of improving the cutting performance. Therefore, S is determined to be ≤ 0.015%.

[0017] (5) Determination of Cr content

[0018] Increasing the Cr content can significantly improve the hardenability of steel. Moreover, Cr is a strong carbide-forming element, and it is very easy to precipitate fine dispersed carbides during tempering, which can improve the strength and wear resistance of steel. However, if the Cr content is too high, it will lead to the formation of blocky carbides, reduce the impact toughness of the steel, and affect the service life of the material. Therefore, the range of the Cr content of the present invention is determined to be 1.50% to 1.80%.

[0019] (6) Determination of Mo content

[0020] The main function of Mo in carburized bearing steel is to improve hardenability and mechanical properties of steel, especially to improve toughness. Therefore, according to the high hardenability requirement of steel for eccentric shaft of robot RV reducer, the control range of Mo content in the present invention is determined to be 0.25% to 0.35%.

[0021] (7) Determination of Ni content

[0022] Nickel can significantly improve the yield strength and tensile strength of steel after quenching and tempering, and significantly improve impact toughness. To meet the use requirements of the eccentric shaft of the robot RV reducer, the Ni content of the present invention is controlled at 1.40% to 1.70%.

[0023] (8) Determination of Nb content

[0024] Nb is a strong carbide-forming element and exists in the steel in the form of nano-scale carbonitrides. These carbonitrides often precipitate in high-temperature processes and play a pinning role on austenite grain boundaries, which can significantly hinder the growth of austenite grains and refine the high-temperature austenite grain size of the steel. However, Nb also has the effect of damaging the surface quality of the steel. Therefore, in order to balance the requirements of the high-temperature grain size of the eccentric shaft and the surface quality of the steel, the control range of the Nb content in the present invention is determined to be 0.02% to 0.05%.

[0025] (9) Determination of W content

[0026] W has the characteristics of high melting point and high density. It is a strong carbide-forming element and can promote the grain refinement of steel, especially at high temperature. W can also enhance the tempering stability of steel. However, as a precious metal element, W has a high cost of addition. Therefore, considering the ultra-fine high-temperature austenite grain size and production economy of the eccentric shaft, the W content of the present invention is ≤0.008%

[0027] (10) Determination of Ti content

[0028] Ti is very easy to form non-metallic inclusions such as TiN or Ti(C,N) in molten steel, and such inclusions are extremely hard, have almost no plasticity, and are usually angular. During product processing, microcracks are very easy to form near such inclusions, which seriously reduces the fatigue life of the product. Therefore, the Ti content of the present invention shall not exceed 0.002%.

[0029] (11) Determination of Al content

[0030] Al is usually added as the main deoxidizing element, and generates high-melting-point Al2O3 non-metallic inclusions with dissolved oxygen in molten steel, which can be removed by a specific method. If it remains in molten steel, it will seriously reduce the purity of molten steel, thereby affecting the service life of the product. Al is also easy to combine with N to generate stable nano-scale AlN precipitates at the grain boundary, which has the effect of hindering the growth of austenite grains and can significantly refine austenite grains. Therefore, considering the high-temperature austenite grain size and ultra-long fatigue life requirements of the eccentric shaft, the Al content of the present invention is determined to be in the range of 0.020% to 0.050%.

[0031] (12) Determination of N content

[0032] The main purpose of N element in carburized bearing steel is to form more nano-scale AlN precipitates, thereby refining the austenite grain size. Since AlN is precipitated according to an atomic ratio of 1:1, that is, a weight ratio of 27:14, a high N content is conducive to the nucleation of AlN, but TiN will also be generated more due to the high N content. Therefore, in order to match the composition design of the Al content and reduce the precipitation of TiN inclusions, the N content of the present invention must be controlled within 300ppm.

[0033] (13) Determination of O content

[0034] The O content represents the amount of oxide inclusions in the steel. A large number of tests have shown that reducing the oxygen content can significantly improve the purity of the steel and increase the service life of the material. Therefore, in order to meet the high purity requirements of the steel used for the cycloid gear of the robot RV reducer, the range of the O content in the present invention is determined to be within 10ppm.

[0035] The main technical indicators of the carburized bearing steel for the eccentric shaft of the robot RV reducer and the production method thereof of the present invention are as follows:

[0036] The present invention requires that the steel material first undergo a normalizing treatment of 900°C*1h + a quenching heat treatment of 860°C*1h, and then the terminal hardenability of the steel material is tested according to ISO642. The specific hardenability requirements are shown in Table 1 below.

[0037] Table 1

[0038] End quenching distance, mm J5 J11 J25 J40 Hardness, HRC 39~48 36~47 31~43 29~41

[0039] Secondly, according to the use requirements of the eccentric shaft of the robot RV reducer, the steel is required to have higher strength, as well as certain toughness and impact toughness. The specific mechanical property requirements are shown in Table 2.

[0040] Table 2

[0041]

[0042] The carburized bearing steel for the eccentric shaft of the robot RV reducer of the present invention has an ultra-fine high-temperature austenite grain size. The steel is required to be air-cooled after carburizing heat treatment at 980°C*5h to inspect the austenite grain size. The grain size should be finer than level 7, and mixed crystal structure is not allowed to exist.

[0043] In order to meet the requirement of long fatigue life of the eccentric shaft of the robot RV reducer, the steel is required to have ultra-high macro and micro purity. First, to ensure macro purity, the present invention needs to perform high-frequency flaw detection on the steel in accordance with SEP 1927, requiring defects not exceeding 2mm / dm 3 , a single defect does not exceed 5mm. Secondly, in order to ensure microscopic purity, the present invention requires that microscopic non-metallic inclusions be inspected according to the GB / T 10561A method. The specific requirements for the rating of non-metallic inclusions are shown in Table 3 below.

[0044] Table 3

[0045]

[0046] The production process of the above-mentioned ultra-fine grain carburized bearing steel for the eccentric shaft of the robot RV reducer is KR hot metal pretreatment - converter - LF refining outside the furnace - RH vacuum degassing - CCM continuous casting - continuous casting billet slow cooling - continuous casting billet forging into intermediate billet - intermediate billet stack cooling - intermediate billet heating and rolling into finished product - rolled product stack cooling - double quenching + tempering quenching and tempering - finishing. The main production process features are as follows:

[0047] (1) KR hot metal pretreatment is used to reduce the content of harmful element S in hot metal. The S content in the hot metal after deoxidation is ≤0.03%. In order to improve the deoxidation performance of hot metal, the Si content in the hot metal is guaranteed to be ≥0.15%; secondly, the hot metal pretreated by KR is initially smelted in a converter to reduce the content of C and P elements. The final C of the converter is ≤0.2%, and the final P is ≤0.02%. The tapping temperature of the converter is ≥1600°C. When the converter taps 3-5 tons of steel, 3-5 bags of SiC are manually added to further increase the Si content in the steel, so that the steel has good deoxidation conditions when it arrives at the LF furnace. When the converter taps, ≥250kg of aluminum iron is added from the high-level silo for pre-deoxidation; secondly, the temperature from the converter to the LF furnace is ≥1520°C, and W iron, Nb iron, Ni iron, Mo iron and low-Ti chromium iron alloy are added in sequence. , strictly follow the alloy ratio to ensure the hardenability of the material, and prevent the formation of large-sized TiN, and use imported refractory materials to prevent the formation of large-sized Al-Mg oxides, ensure that the material passes the high-frequency flaw detection inspection, use high-performance refined synthetic slag, maintain a long refining and slag-making process, LF process ≥50min, so that non-metallic inclusions can be fully floated; when the RH furnace is vacuum degassing, the furnace reaches a sufficient vacuum degree, the vacuum degree needs to be maintained between 100-150Pa, and the high vacuum time is ≥20min, to further remove harmful gases and non-metallic inclusions in the molten steel. After breaking the air, the nitrogen content of the molten steel is increased by manual argon connection, and the nitrogen flow rate is ≤300L / min, ensuring that the nitrogen content of the molten steel is within 300ppm, so that the inclusions can be fully floated;

[0048] (2) Continuous casting: Use three-machine three-stream large-section continuous casting billets with specifications of 350mm×500mm and above to ensure high compression ratio rolling of steel, thereby ensuring the density of the material; use argon protection casting and add protective slag throughout the process to protect the molten steel from secondary oxidation contamination; use light pressure reduction technology, with a light pressure reduction of ≤18mm, effectively improving low-magnification defects such as central looseness and shrinkage holes; use high superheat casting, and control the superheat at ≥30℃ to reduce the number of inclusions in the billet; the pulling speed of the continuous casting billet is ≤0.8m / min, and the remaining steel in the ladle is not less than 5 tons. The continuous casting billet should be slowly cooled at a temperature above 600℃ to prevent cracking of the continuous casting billet. The slow cooling time should be greater than 48 hours, and the exit temperature should be ≥200℃;

[0049] (3) Forging intermediate billets from continuous casting billets: The continuous casting billets are sent to a heating furnace in a neutral or weakly oxidizing atmosphere for heating. The heating temperature is controlled at 1050-1250°C. The heating time of the billets is ≥5h to ensure that the material is fully heated. Subsequently, the billets are forged by a precision forging machine to form square intermediate billets of 200mm×200mm-300mm×300mm. After studying the thermoplasticity of the carburized bearing steel of the present invention, the forging temperature is around 950°C, and the material has good high-temperature plasticity. Therefore, low-temperature forging and three-pass forging processes are used during the forging process, and the forging rate is strictly controlled. Specifically, the initial forging temperature is 1000±50°C, the initial forging rate is 7.0m / min, the second pass forging rate is 5.0m / min, the last pass forging rate is 2.0m / min, the interval time between each pass is ≤5min, the final forging temperature is controlled to be ≥850°C, and the intermediate billet is pile-cooled after forging, and the pile-cooling time is ≥60h. The novel low-temperature forging process of the present invention reduces the initial forging temperature, adopts a three-step forging process and strictly controls the forging rate and interval time to ensure the final forging temperature, so that the forging process is more suitable for the thermoplasticity of the carburized bearing steel of the present invention;

[0050] (4) Rolling the intermediate billet into finished products: The intermediate billet is sent to the heating furnace for heating and then rolled into finished steel products. A high-temperature heating process is used, specifically: the temperature of the preheating section is controlled at 650-900°C, the temperature of the heating section is controlled at 1100-1250°C, the temperature of the soaking section is controlled at 1200-1280°C, the compression ratio of the first rolling process is 2.3-3.0, the temperature of the second rolling is 980°C-1100°C, the compression ratio is controlled at above 2.8, the temperature of the third final rolling is controlled at above 920°C, the compression ratio is controlled at above 2.5, the total compression ratio of the three rolling passes is ≥20, and the temperature of the rolled material out of the cold pit is ≤200°C;

[0051] (5) Double quenching + tempering treatment: In order to ensure that the eccentric shaft of the RV reducer has an extremely small grain size after carburizing, it is necessary to perform a quenching and tempering preheating treatment to make the structure obtain a finer and more uniform tempered sorbite structure. The new double quenching + tempering quenching and tempering treatment process in this invention is as follows: the rolled round bar is loaded into an induction heating quenching furnace, and the round bar is heated with the furnace (heating rate 5℃ / min) to 860℃-900℃, and kept at this temperature for 3.5h-4.0h, and then removed from the furnace for oil cooling and placed for 1~2h, and then the round bar is quickly transferred to another furnace at a temperature of 770℃-810℃ for 2.0h-3.0h, and then removed from the furnace for oil cooling. The two quenching heat treatments further refine the austenite grains. After cooling, the round bar is tempered at a tempering temperature of 150℃-200℃ and kept for 1.5h-2.5h. Finally, the steel is removed from the furnace and naturally cooled in the air.

[0052] (6) Finishing: including straightening, chamfering and non-destructive testing and other finishing processes. All products must undergo 100% non-destructive testing to ensure the surface and internal quality of the products.

[0053] Compared with the prior art, the advantages of the present invention are:

[0054] (1) The hardenability of steel meets J5 (39-48HRC), J11 (36-47HRC), J25 (31-43HRC), J40 (29-41HRC).

[0055] (2) The yield strength of the steel shall be ≥905MPa, the tensile strength shall be ≥1200Mpa, the elongation after fracture shall be ≥11%, the cross-sectional shrinkage shall be ≥35%, and the impact energy at room temperature shall be ≥50J.

[0056] (3) After high-temperature carburizing, the grain size of the steel is required to be finer than level 7, and there is no mixed crystal structure.

[0057] (4) Microscopic inclusions are tested according to GB / T 10561A method, and the following conditions are met: Class A fine system ≤ 2.0, Class A coarse system ≤ 1.5, Class B fine system ≤ 1.0, Class B coarse system ≤ 0.5, Class C fine system ≤ 0.5, Class C coarse system ≤ 0.5, Class D fine system ≤ 1.0, Class D coarse system ≤ 0.5, Class DS ≤ 1.0. Macroscopic inclusions are tested according to SEP1927 high frequency flaw detection method, and the defects shall not exceed 2mm / dm 3 , a single defect does not exceed 5mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 is the grain size of the products of Examples 1 and 2 of the present invention;

[0059] Figure 2 The grain size of the products of Comparative Examples 1 and 2 of the present invention;

[0060] Figure 3 The metallographic structures of the products of various embodiments of the present invention under the “double quenching + tempering” heat treatment. DETAILED DESCRIPTION

[0061] The technical solution of the present invention is described in more detail in conjunction with the preferred embodiments of the present invention. However, these embodiments are only descriptions of the preferred implementation methods of the present invention and cannot impose any limitation on the scope of the present invention.

[0062] The chemical compositions of the embodiments of the present invention and the comparative example (carburized bearing steel for conventional eccentric shaft) are shown in Table 4.

[0063] Table 4

[0064]

[0065] The test data of the terminal hardenability of each embodiment of the present invention and the comparative example are shown in Table 5.

[0066] Table 5

[0067] Serial number J5 J11 J25 J40 Example 1 45 44.5 40 35 Example 2 43.5 43.0 40.5 37 Comparative Example 1 45.0 43.5 35 29 Comparative Example 2 44 42.5 32.5 28

[0068] The mechanical property results of the embodiments of the present invention after double quenching + tempering and the comparative examples after conventional quenching and tempering are shown in Table 6.

[0069] Table 6

[0070]

[0071] The embodiments of the present invention and the comparative examples were subjected to carburizing heat treatment at 980°C*5h, air-cooled, and the austenite grain size was tested as shown in Table 7. The grain size photos of the embodiments of the present invention are shown in Table 7. Figure 1 and 2 .

[0072] Table 7

[0073] Serial number Grain size / grade Example 1 9.0 Example 2 9.0 Comparative Example 1 7.0 Comparative Example 2 mixed crystal

[0074] The microscopic non-metallic inclusion rating and high-frequency flaw detection results of the embodiments of the present invention and the comparative examples are shown in Table 8.

[0075] Table 8

[0076]

[0077]

[0078] Compared with the chemical composition, hardenability, mechanical properties, grain size and purity of conventional RV reducer eccentric shaft products 1 and 2, the embodiments of the present invention reduce the C content and Mn content, increase the Cr and Mo contents, ensure that the hardenability of the material meets the requirements, and improve the Rockwell hardness of J25 and J40; in order to refine the high-temperature grain size, the present invention adds Nb and W elements; in order to improve the strength of this product, the present invention increases the Ni content; since the molten steel smelting adopts a specific vacuum degassing technology, the oxygen content tested on the finished steel in the embodiments of the present invention is relatively low, and the inclusion and high-frequency flaw detection inspections are better than the comparative examples.

[0079] The technical solution of the present invention is described in more detail below in conjunction with the preferred embodiments of the present invention.

[0080] Specifically, the molten iron is first pretreated with KR molten iron, the converter end point C≤0.2%, the end point P≤0.02%, and the converter tapping temperature≥1600℃. During the LF refining outside the furnace, W iron, Nb iron, Ni iron, Mo iron and low-Ti chromium iron alloy are added in sequence, and imported refractory materials are used to prevent the formation of large-sized Al-Mg oxides, and high-performance refining synthetic slag is used to maintain a long-term refining and slagging process; when vacuum degassing in the RH furnace, the high vacuum time is ≥20min to further remove harmful gases and non-metallic inclusions in the molten steel. After breaking the air, the nitrogen content of the molten steel is increased by manual argon connection to ensure that the nitrogen content of the molten steel is within 300ppm, and further make the inclusions fully float; the continuous casting process adopts protective pouring throughout the process, and adopts the induction heating of the tundish, light pressure, and electromagnetic stirring technology, the superheat is controlled at ≥30℃, and the cross-sectional size of the continuous casting billet is 390mm*510mm.

[0081] The continuous casting billet is sent to a heating furnace in a neutral or weakly oxidizing atmosphere for heating. The heating temperature is controlled at about 1150℃. The heating time of the billet is 6 hours. The billet is forged into a 230mm×230mm square intermediate billet. After forging, it is pile-cooled for 72 hours. Subsequently, the intermediate billet is sent to a heating furnace for high-temperature heating. The temperature of the soaking section is controlled at about 1250℃. It is rolled into a φ60mm rolled material. The temperature of the rolled material after pile cooling is ≤200℃.

[0082] Double quenching + tempering treatment: the rolled round bar is loaded into the induction heating quenching furnace, the round bar is heated to 880℃ with the furnace, and kept at this temperature for 4.0 hours, and then the round bar is oil-cooled and placed for 1.2 hours, and then the round bar is quickly transferred to another furnace at 790℃ for 2.5 hours, and then the round bar is oil-cooled. The two quenching heat treatments further refine the austenite grains. After cooling, the round bar is tempered at 180℃ and kept for 2 hours. Finally, the steel is taken out of the furnace and cooled naturally in the air. Finally, the steel is straightened, chamfered and non-destructive testing to obtain finished bars.

[0083] In summary, the present invention relates to a carburized bearing steel for an eccentric shaft of a robot RV reducer and a production method thereof. In terms of purity, the key parameters of each process of molten iron pretreatment, refining, and vacuum degassing are optimized and controlled to effectively remove harmful non-metallic inclusions; in terms of high-temperature grain size, the austenite grain size of the steel is controlled by adding a certain amount of Al, N, Nb and W elements to the molten steel, and adopting a high-temperature heating process during the rolling process. The Ni content is added to improve the mechanical properties of the steel; the forging + rolling process is used to ensure the density and uniformity of the steel. Thereby, on the basis of satisfying the hardenability and mechanical properties of the steel, the steel obtains a higher purity and a higher grain size, which significantly enhances the competitiveness of the product in terms of production efficiency, production cost and product quality stability.

[0084] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A carburized bearing steel for the eccentric shaft of a robot RV reducer. Features: The chemical composition of the steel is as follows by mass percentage: C: 0.10-0.20%, Si: 0.20-0.40%, Mn: 0.60-1.00%, P≤0.020%, S≤0.015%, Cr: 1.50-1.80%, Mo: 0.25-0.35%, Ni: 1.40-1.70%, Nb: 0.02-0.05%, W≤0.008%, Ti≤0.002%, Al: 0.020-0.050%, and the balance is Fe and unavoidable impurities.

2. The carburized bearing steel for the eccentric shaft of a robot RV reducer according to claim 1, Features: The steel is first subjected to a normalizing heat treatment of 900°C*1h + a quenching heat treatment of 860°C*1h, and then the terminal hardenability of the steel is tested according to ISO 642, with specific hardenability of J5: 39-48HRC, J11: 36-47HRC, J25: 31-43HRC, and J40: 29-41HRC.

3. The carburized bearing steel for the eccentric shaft of a robot RV reducer according to claim 1, Features: The steel has a yield strength of ≥905MPa, a tensile strength of ≥1200Mpa, a fracture elongation of ≥11%, a cross-sectional shrinkage of ≥35%, a room temperature impact energy of ≥50J, and a grain size finer than grade 7.

4. The carburized bearing steel for the eccentric shaft of a robot RV reducer according to claim 1, Features: The steel is tested by GB / T 10561A method for microscopic non-metallic inclusions: A fine system ≤2.0, A coarse system ≤1.5, B fine system ≤1.0, B coarse system ≤0.5, C fine system ≤0.5, C coarse system ≤0.5, D fine system ≤1.0, D coarse system ≤0.5, DS ≤1.0; macroscopic inclusions are tested by SEP1927 high-frequency flaw detection method, and defects do not exceed 2mm / dm 3 , a single defect does not exceed 5mm.

5. A method for manufacturing carburized bearing steel for an eccentric shaft of a robot RV reducer according to claim 1, Features: The method specifically comprises the following steps: (1) Molten steel smelting: KR hot metal pretreatment is used to reduce the harmful element S content in the hot metal, and the S content is ≤0.03%. In order to improve the deoxidation performance of the hot metal, the Si content in the hot metal is guaranteed to be ≥0.15%. Secondly, the converter is used for primary smelting, and the converter end point C is ≤0.2%, the end point P is ≤0.02%, and the converter tapping temperature is ≥1600℃; the temperature from the converter to the LF furnace is ≥1520℃, and the LF furnace is added with low Ti alloy to prevent the formation of large-sized TiN, and refractory materials and high-performance refined synthetic slag are used to prevent the formation of large-sized Al-Mg oxides. The refining and slagging process is maintained for a long time, and the LF process is ≥50min, so that non-metallic inclusions can be fully floated; vacuum degassing is carried out in the RH furnace, and the high vacuum time is ≥20min. After breaking the air, the nitrogen content of the molten steel is increased by manual argon connection to ensure that the nitrogen content of the molten steel is within 300ppm, which further allows the inclusions to fully float; (2) Large-section CCM continuous casting billet: large-section continuous casting billet with a specification of 350mm×500mm and above is used to ensure high compression ratio rolling of steel, thereby ensuring the density of the material; argon protection casting is used throughout the process and protective slag is added to protect the molten steel from secondary oxidation contamination; light pressure reduction technology and high superheat casting are used to reduce the number of inclusions in the billet; the continuous casting billet is slowly cooled at a temperature above 600℃ to prevent cracking of the continuous casting billet, the slow cooling time is ≥48h, and the exit temperature is ≥200℃; (3) Forging the continuous casting billet into an intermediate billet: The continuous casting billet is sent to a heating furnace in a neutral or weakly oxidizing atmosphere for heating. The heating temperature is controlled at 1050-1250°C. The heating time of the billet is ≥5h to ensure that the material is fully heated. The low-temperature forging and three-time forging process are adopted. The forging rate is strictly controlled to forge the billet into a square intermediate billet of 200mm×200mm-300mm×300mm. After forging, the intermediate billet is pile-cooled for a cooling time of ≥60h. (4) Rolling the intermediate billet into finished products: The intermediate billet is sent to a heating furnace for heating and then rolled into finished steel products. The temperature of the rolled product out of the cold pit is ≤200°C. (5) "Double quenching + tempering" quenching and tempering treatment: the rolled round bar is loaded into an induction heating quenching furnace, and the round bar is heated to 860℃-900℃ with the furnace, and kept at this temperature for 3.5h-4.0h, and then taken out of the furnace for oil cooling and placed for 1-2h, and then the round bar is quickly transferred to another furnace at a temperature of 770℃-810℃ for 2.0h-3.0h, and then taken out of the furnace for oil cooling. The two quenching heat treatments further refine the austenite grains. After cooling, the round bar is tempered at a tempering temperature of 150℃-200℃, and kept for 1.5h-2.5h. Finally, the steel is taken out of the furnace and cooled naturally in the air; (6) Finishing: including straightening, chamfering and non-destructive testing and other finishing processes. All products must undergo 100% non-destructive testing to ensure the surface and internal quality of the products.

6. A method for manufacturing carburized bearing steel for an eccentric shaft of a robot RV reducer according to claim 5, Features: Step (1) When the converter produces 3-5 tons of steel, 3-5 bags of SiC are manually added. When the steel is finished being produced, ≥250 kg of aluminum iron is added from the high-level silo for pre-deoxidation.

7. A method for manufacturing carburized bearing steel for an eccentric shaft of a robot RV reducer according to claim 5, Features: In step (2), three-machine three-stream large-section continuous casting billets are used, the pulling speed of the continuous casting billets is ≤0.8m / min, and the remaining steel volume in the ladle is not less than 5 tons.

8. A method for manufacturing carburized bearing steel for an eccentric shaft of a robot RV reducer according to claim 5, Features: In step (3), the initial forging temperature is 1000±50°C, the initial forging rate is 7.0 m / min, the second forging rate is 5.0 m / min, the last forging rate is 2.0 m / min, the interval between each pass is ≤5 min, and the final forging temperature is controlled to be ≥850°C.

9. A method for manufacturing carburized bearing steel for an eccentric shaft of a robot RV reducer according to claim 5, Features: In step (4), a high temperature heating process is adopted, specifically: the temperature of the preheating section is controlled at 650-900°C, the temperature of the heating section is controlled at 1100-1250°C, the temperature of the soaking section is controlled at 1200-1280°C, the compression ratio of the first rolling process is 2.3-3.0, the temperature of the second rolling is 980°C-1100°C, the compression ratio is controlled at above 2.8, the temperature of the third final rolling is controlled at above 920°C, the compression ratio is controlled at above 2.5, and the total compression ratio of the three rolling passes is ≥20.

10. A method for manufacturing carburized bearing steel for an eccentric shaft of a robot RV reducer according to claim 5, Features: The heating rate of the first quenching in step (3) is 5°C / min.

Citation Information

Patent Citations

  • Carburizing bearing steel for railway freight car and preparing method of carburizing bearing steel

    CN107904498A

  • Production method of 18CrNiMo7-6 forging for wind power equipment gear

    CN111636033A

  • Gear steel resistant to high-temperature carburization and grain growth and control method

    CN112831723A

  • Manufacturing method of steel for speed reducer gear of electric automobile

    CN112981271A

  • Manufacturing method of microalloyed wind power transmission gear steel

    CN114959415A

Cited By

  • Efficient machining method, device and equipment for RV reducer eccentric shaft

    CN120249634A

  • An efficient processing method, device and equipment for the eccentric shaft of an RV reducer

    CN120249634B

  • Production process for improving density and grain size of high-carbon bearing steel core