Preparation method of die-casting die, die-casting die and die-casting method
By forming an F-DLC coating on the die-casting mold, the problem of poor fluidity of semi-solid metals is solved, the yield of die-casting and thermal insulation and lubricity of the mold is improved, and a more efficient die-casting effect is achieved.
Patent Information
- Application Number
- CN202411219493.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-31
- Publication Date
- 2024-11-22
AI Technical Summary
When using semi-solid metals, existing die-casting molds have poor fluidity, resulting in low yields of die-casting parts, which are prone to defects such as cracking and unsaturated molds.
The cathode vacuum arc plasma device is used to form an F-DLC coating. By adjusting the air pressure and pulse bias, a fluorine-containing F-DLC coating is formed, which improves the insulation and lubricity of the mold and delays the curing of semi-solid metals, thereby achieving more Good fluidity and saturation.
Improves the yield of die-casting, reduces cracking, and ensures that semi-solid metal can fill the mold and die-cast successfully.
Smart Images

Figure CN118996346A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of die-casting technology, and in particular to a method for preparing a die-casting mold, a die-casting mold and a die-casting method. Background Art
[0002] Diamond-like carbon coating material (DLC) is a general term for a type of amorphous carbon film material, mainly composed of sp 3 Hybridized carbon (diamond phase) and sp 2 It is a mixture of three-dimensional cross-network of hybrid carbon (graphite phase) and has many excellent properties such as high hardness, low friction coefficient, high infrared transmittance, good chemical inertness and biocompatibility. It has broad application prospects in the fields of ocean, aerospace, biomedicine, micro-electromechanical, automobile, etc.
[0003] Current coating technology often uses physical deposition (PVD) to sputter or evaporate conventional diamond-like carbon coatings onto the die-casting cavity of the mold. Since semi-solid metals such as high-strength aluminum alloys have poor fluidity, the semi-solid metal cannot fill the die-casting cavity of the die-casting mold. The yield of die-castings obtained by the die-casting mold is low, and die-castings are prone to defects such as cracking and incomplete mold. Summary of the invention
[0004] In view of the above, it is necessary to propose a method for preparing a die-casting mold, a die-casting mold and a die-casting method to improve the yield of the obtained die-casting parts.
[0005] A first aspect of an embodiment of the present application provides a method for preparing a die-casting mold, comprising the following steps:
[0006] Evacuating a vacuum ballast chamber of a cathode vacuum arc plasma device to adjust the air pressure in the vacuum ballast chamber to a first air pressure value, and adjusting the cathode pulse bias voltage to a first bias voltage value;
[0007] Placing a die-casting mold body and a graphite target in the cathode vacuum arc plasma equipment, wherein a die-casting cavity is provided on the die-casting mold body;
[0008] The gas pressure in the vacuum ballast chamber of the cathode vacuum arc plasma device is lowered from the first gas pressure value to a second gas pressure value, and the pulse bias voltage of the graphite target is lowered from the first bias voltage value to the second bias voltage value, wherein the second bias voltage value has a value range of 100V to 700V;
[0009] Fluorine-containing gas is introduced into the cathode vacuum arc plasma equipment to form an F-DLC coating on the surface of the die-casting cavity, thereby obtaining a die-casting mold.
[0010] In a possible implementation, the F-DLC coating includes sp 3Hybridized carbon and sp 2 Hybridized carbon, the sp 3 Hybridized carbon with the sp 2 The ratio of hybrid carbon ranges from 4% to 72%.
[0011] In a possible implementation manner, the F-DLC coating includes F element and C element, and the ratio of the F element to the C element ranges from 1% to 10%.
[0012] In a possible implementation manner, the first air pressure value is in the range of 5.9×10 -3 Pa~6.1×10 -3 Pa, the value range of the second air pressure value is 4.9×10 -3 Pa~5.1×10 -3 Pa, the first bias voltage value ranges from 950V to 1050V, and the time for forming the F-DLC coating after the pulse bias of the graphite target is reduced from the first bias voltage value to the second bias value ranges from 15min to 25min.
[0013] In a possible implementation manner, the water contact angle of the F-DLC coating ranges from 103° to 159°.
[0014] In a possible implementation manner, the roughness of the F-DLC coating ranges from 50.8 nm to 55.6 nm.
[0015] In a possible implementation manner, the grain size in the F-DLC coating ranges from 4.7 μm to 53.2 μm.
[0016] A second aspect of an embodiment of the present application provides a die-casting mold, comprising:
[0017] A die-casting mold body, wherein a die-casting cavity is formed on the die-casting mold body;
[0018] The F-DLC coating as described in any one of the above items is provided on the cavity wall of the die-casting cavity of the die-casting mold body.
[0019] A third aspect of the embodiment of the present application provides a die-casting method, comprising the following steps:
[0020] Obtaining a semi-solid pre-pressed material;
[0021] The pre-pressed material is injected into the F-DLC coating surface on the cavity wall of the die-casting cavity of the die-casting mold as described above to obtain a die-casting part after die-casting.
[0022] In a possible implementation, the step of obtaining a semi-solid pre-pressed material includes:
[0023] Obtaining a pre-pressed blank, wherein the pre-pressed blank comprises, by mass percentage: 0.4% silicon, 0.5% iron, 1.5% copper, 2.5% magnesium, 0.2% chromium, 5.5% zinc, 0.2% titanium, 0.3% manganese, and the remainder aluminum;
[0024] Heating the pre-pressed blank to 850° C. to 950° C. to melt the pre-pressed blank;
[0025] Homogenize the melted pre-pressed blank for 35 to 45 minutes;
[0026] The homogenized pre-pressed blank is cooled to a semi-solidification point to obtain a semi-solid pre-pressed blank.
[0027] In the technical solution provided in the embodiment of the present application, the vacuum ballast chamber of the cathode vacuum arc plasma device is first evacuated to make the air pressure in the vacuum ballast chamber reach the first air pressure value, and the cathode pulse bias is adjusted to the first bias value; then the die-casting mold body and the graphite target are placed in the cathode vacuum arc plasma device; then the air pressure in the vacuum ballast chamber of the cathode vacuum arc plasma device is adjusted from the first air pressure value to the second air pressure value, and the pulse bias of the graphite target is adjusted from the first bias value to the second bias value, and the second bias value ranges from 100V to 700V; finally, fluorine-containing gas is introduced into the cathode vacuum arc plasma device to form an F-DLC coating on the surface of the die-casting cavity, thereby obtaining a die-casting mold. By setting the second bias value to 100V to 700V, the sp in the F-DLC coating can be increased. 3 Hybridized carbon with sp 2 The ratio of hybrid carbon, as well as the ratio of F element to C element, can effectively improve the thermal insulation and lubricity of the die-casting mold, which is beneficial to the fluidity of the spherical crystal soup and the saturation of the complex product structure required by the semi-solid die-casting technology. The solidification of the semi-solid metal can be delayed during die-casting, so that the semi-solid metal can fill the die-casting cavity of the die-casting mold and be die-cast. The yield of the obtained die-casting is high, and the die-casting is not prone to cracking. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a flow chart of the method for preparing a die-casting mold provided in an embodiment of the present application.
[0029] Figure 2 is the sp in the F-DLC coating obtained when the target pulse bias voltage in the embodiment of the present application is adjusted to 700V 2 Hybridized carbon and sp 3 The X-ray photoelectron spectroscopy (XPS) spectrum curve obtained by hybridizing carbon.
[0030] Figure 3 is the sp in the F-DLC coating obtained when the target pulse bias voltage in the embodiment of the present application is adjusted to 100V 2 Hybridized carbon and sp 3 The X-ray photoelectron spectroscopy (XPS) spectrum curve obtained by hybridizing carbon.
[0031] Figure 4 The X-ray photoelectron spectroscopy (XPS) spectrum curve obtained by adjusting the target pulse bias voltage to 100V, 220V, 340V, 460V, 580V and 700V in the embodiment of the present application is expressed by the percentage content of fluorine atoms in the F-DLC coating.
[0032] Figure 5 is a metallographic image of the F-DLC coating obtained in one embodiment of the present application.
[0033] Figure 6 It is a schematic diagram of the structure of the die-casting mold provided in an embodiment of the present application.
[0034] Figure 7 It is a flow chart of the die-casting method provided in an embodiment of the present application.
[0035] Figure 8 yes Figure 7 Figure 2 shows the steps for obtaining a semi-solid pre-pressed material.
[0036] Main component symbols
[0037] Die casting mold 100
[0038] Die casting mold body 10
[0039] Die casting cavity 11
[0040] F-DLC coating 20
[0041] Die casting 200 DETAILED DESCRIPTION
[0042] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0043] In the description of the present invention, it should be understood that the terms indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0044] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the term "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0045] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can appreciate the application of other processes and / or the use of other materials.
[0046] The embodiments of the present application will be described in detail below with reference to the accompanying drawings.
[0047] See also Figure 1 In a first aspect, an embodiment of the present application provides a method for preparing a die-casting mold, comprising the following steps:
[0048] S11, evacuating a vacuum ballast chamber of a cathode vacuum arc plasma device to adjust the air pressure in the vacuum ballast chamber to a first air pressure value, and adjusting the cathode pulse bias voltage to a first bias voltage value.
[0049] It should be noted that the cathode vacuum arc plasma equipment is mainly composed of a vacuum ballast, a sample table, a magnetic filter elbow wrapped with a copper coil, an anode cylinder and a cathode target. In the cathode vacuum arc plasma equipment, the cathode target is ionized into plasma under the action of the field effect. The sample table can be set by the program to revolve around the vertical axis and rotate around the horizontal axis to ensure the uniformity of the coating.
[0050] Among them, by evacuating the vacuum ballast chamber of the cathode vacuum arc plasma equipment to make the air pressure in the vacuum ballast chamber reach a first air pressure value, as a preset or test step before sputtering, it can be ensured that the required air pressure environment is reached in the vacuum ballast chamber, creating conditions for subsequent target material sputtering and coating deposition; and the vacuum environment helps to reduce the interference of gas molecules and particles on the deposition process, and improve the quality and purity of the coating; in addition, it can also prevent gases and water vapor in the atmosphere from corroding or damaging the components of the cathode vacuum arc plasma equipment.
[0051] Specifically, the value range of the first air pressure value is 5.9×10 -3 Pa~6.1×10 -3 Pa. It can be understood that the first air pressure value can be 5.9×10 -3 Pa, 5.95×10 -3 Pa, 6.0×10 -3 Pa, 6.05×10 -3 Pa, 6.1×10 -3 Pa. Since the first gas pressure value is in a relatively low pressure range, it helps to reduce the interference of gas molecules on the deposition process and improve the quality and purity of the film. Preferably, the first gas pressure value is 6.0×10 -3 Pa.
[0052] Among them, by adjusting the cathode pulse bias to the first bias value as a preset or test step before sputtering, the working state of the cathode vacuum arc plasma equipment can be tested and adjusted to ensure that the system is stable and ready for the subsequent sputtering process, and can be used to optimize the sputtering efficiency and provide a reference for the actual sputtering process. A higher bias voltage can be used to pre-clean the target surface and remove the oxide layer or other contaminants on the surface, thereby obtaining a purer sputtering source.
[0053] Specifically, the first bias voltage ranges from 950V to 1050V. It is understood that the first bias voltage may be 950V, 975V, 1000V, or 1050V. Since the first bias voltage is a relatively high bias voltage, it helps to sputter more atoms and molecules from the graphite target, promotes the formation of plasma, and can also increase the deposition rate and the density of the film. Preferably, the first bias voltage is 1000V.
[0054] S12, placing the die-casting mold body and the graphite target in a cathode vacuum arc plasma device, wherein a die-casting cavity is opened on the die-casting mold body.
[0055] The die-casting mold body is the substrate (object) to be deposited.
[0056] Among them, the graphite target stone is of high purity, which can ensure the stability of the deposition process and the uniformity of the coating. In processes such as physical vapor deposition (PVD) and sputtering, the graphite target releases carbon atoms or molecules from the surface of the target through the sputtering process and forms a coating on the main body of the die-casting mold. In addition, the high thermal conductivity and chemical stability of the graphite target ensure the thermal management of the target during the sputtering process, while the chemical stability ensures the purity of the deposited coating and the service life of the target.
[0057] Among them, in the cathode vacuum arc plasma equipment, the distance between the die casting mold body and the target material ranges from 200mm to 250mm. This distance will affect the energy and deposition rate of the sputtered particles reaching the die casting mold body, which can reduce the deposition rate and improve the uniformity of the coating. Preferably, the distance between the die casting mold body and the target material is 230mm.
[0058] S13, lowering the air pressure in the vacuum ballast chamber of the cathode vacuum arc plasma equipment from a first air pressure value to a second air pressure value, and lowering the pulse bias voltage of the graphite target from a first bias voltage value to a second bias voltage value, wherein the second bias voltage ranges from 100V to 700V.
[0059] Different gas pressures affect the behavior of plasma and sputtering efficiency. Reducing the gas pressure in the vacuum chamber to the second gas pressure value can optimize the sputtering process, help increase the deposition rate or improve the microstructure of the coating. In addition, excessive gas pressure may reduce the ion energy in the plasma and reduce the sputtering efficiency. By reducing the gas pressure to the second gas pressure value, this situation can be avoided to ensure the effective sputtering of the graphite target. In addition, reducing the gas pressure can also reduce the wear on the cathode vacuum arc plasma equipment, extend the service life of the cathode vacuum arc plasma equipment, and reduce potential safety risks, such as avoiding failure or explosion of the cathode vacuum arc plasma equipment caused by high gas pressure.
[0060] The second pressure value range is 4.9×10 -3 Pa~5.1×10 -3 Pa. It can be understood that the second air pressure value can be 4.9×10 -3 Pa, 4.95×10 -3 Pa, 5.0×10 -3 Pa, 5.05×10 -3 Pa, 5.1×10 -3Pa. By precisely controlling the gas pressure to the range of the second gas pressure value, the density and energy of the plasma can be finely controlled. At a lower gas pressure, the collision between ions in the plasma and gas molecules is reduced, thereby increasing the proportion of particles reaching the die-casting mold body and increasing the sputtering yield; and lowering the gas pressure helps to reduce the collision between gas molecules and deposited atoms, reduce gas inclusions in the F-DLC coating, and thus improve the quality and purity of the F-DLC coating; because excessive gas pressure may lead to undesirable chemical reactions, such as excessive fluorination reactions, this situation can be avoided by setting a lower second gas pressure value. In addition, lowering the gas pressure can also reduce potential safety risks caused by high gas pressure. Preferably, the second gas pressure value is 5.0×10 - 3 Pa.
[0061] The second bias voltage may be 100 V, 220 V, 340 V, 460 V, 580 V, or 700 V. By setting the second bias voltage to the above range, on the one hand, sufficient energy can be provided to break the chemical bonds in the graphite target; on the other hand, in the cathode vacuum arc plasma device, the pulse bias voltage helps to form plasma, and the ions, electrons, and neutral particles in the plasma can bombard the graphite target, promoting the sputtering and dissociation of graphite; on the third hand, sp 2 Hybridized carbon and sp 3 The proportion of hybrid carbon will affect the physical and chemical properties of the coating. By adjusting the bias value, the sp in the F-DLC coating can be improved to a certain extent. 3 The atomic percentage content of hybridized carbon can control the hardness, elastic modulus and other properties of the coating; fourthly, setting a suitable bias value can prevent excessive sputtering, which may cause undesirable holes or unevenness in the coating, and help optimize the adhesion, uniformity, density and other physical and chemical properties of the coating; fifthly, the upper and lower limits of the bias value are also related to the operational safety of the cathode vacuum arc plasma equipment. Excessive bias may pose risks to the cathode vacuum arc plasma equipment or operators.
[0062] Understandable, sp 2 Hybridized carbon refers to the carbon atom in which three of the four valence electrons participate in the formation of hybrid orbitals, and the remaining electron remains in the original 2p orbital; in sp 2 In hybridization, one 2s orbital mixes with two 2p orbitals to form three equivalent sp 2 Hybrid orbital. sp 3 Hybridized carbon refers to the situation where three of the four valence electrons of a carbon atom participate in the formation of hybrid orbitals, and one 2p orbital electron does not participate in hybridization, but may be used to form π bonds or remain as a lone pair of electrons; in SP3 hybridization, one 2s orbital and three 2p orbitals are mixed to form four equivalent sp3 Hybrid orbital.
[0063] S14, introducing fluorine-containing gas into the cathode vacuum arc plasma equipment to form an F-DLC coating on the surface of the die-casting cavity, thereby obtaining a die-casting mold.
[0064] The fluorine-containing gas may be C2F4 (tetrafluoroethylene). It is understood that in other embodiments, the fluoride may also be other components, such as CF4, but is not limited thereto.
[0065] By introducing fluorine-containing gas into the cathode vacuum arc plasma equipment, the fluorine atoms in the fluorine-containing gas will form carbon chain bonds with the broken chemical bonds in the graphite, and form an F-DLC coating on the surface of the die-casting cavity. Since the F-DLC coating contains fluorine atoms, which are hydrophobic, the solidification of the semi-solid metal can be delayed during die-casting, so that the semi-solid metal can fill the die-casting cavity of the die-casting mold and be die-cast. The yield of the obtained die-casting is high and the die-casting is not prone to cracking.
[0066] Among them, the time range for forming the F-DLC coating is 15min to 25min. It can be understood that the time for forming the F-DLC coating can be 15min, 16min, 17min, 18min, 19min, 20min, 21min, 22min, 23min, 24min, 25min. Different deposition times may affect the microstructure of the F-DLC coating, such as grain size, porosity, etc. By controlling the time for forming the F-DLC coating to 15min to 25min, the thickness of the coating can be accurately controlled, which helps to obtain an ideal coating structure, and can ensure uniform deposition of the coating on the entire substrate, avoiding local over-thickness or unevenness. In addition, too long deposition time may cause cracks, excessive stress or other defects in the F-DLC coating. The appropriate time range helps to prevent these problems. Under the premise of ensuring the quality of the F-DLC coating, selecting a suitable deposition time can improve production efficiency, reduce energy consumption and material waste, and avoid potential safety risks caused by too long operation time, such as equipment overheating. Preferably, the time for forming the F-DLC coating is 20min.
[0067] Depend on Figure 2 and Figure 3 It can be seen that when the pulse bias voltage of the graphite target is adjusted to 700 V, the sp 3 The percentage content of hybrid carbon reaching the peak during the bonding process is greater than the sp in the F-DLC coating when the pulse bias voltage of the graphite target is adjusted to 100V. 3 The percentage content of hybrid carbon when it reaches the peak during the bonding process indicates that when the pulse bias voltage of the graphite target is adjusted to 700V, the sp 3The percentage of hybrid carbon is high. When the pulse bias voltage of the graphite target is adjusted to 100V, the sp 3 The percentage of hybrid carbon is low. Figure 4 It can be seen that when the first bias voltage is 100 V, 220 V, 340 V, 460 V, 580 V and 700 V respectively, the percentage content of fluorine atoms in the F-DLC coating gradually increases.
[0068] Among them, the F-DLC coating includes sp 3 Hybridized carbon and sp 2 Hybridized carbon, sp 3 Hybridized carbon with sp 2 The ratio of hybrid carbon ranges from 4% to 72%. 3 Hybridized carbon with sp 2 When the ratio of hybrid carbon is in this ratio range, the F-DLC coating has higher hardness and better wear resistance, and has certain toughness.
[0069] Among them, the F-DLC coating includes F elements and C elements, and the ratio of F elements to C elements ranges from 1% to 10%. Fluorine doping can significantly change the surface energy and friction coefficient of the DLC coating, affecting its wear resistance, corrosion resistance and biocompatibility. When the fluorine content is in this ratio range, the hydrophobicity of the coating can be improved.
[0070] Among them, the water contact angle of the F-DLC coating ranges from 103° to 159°. When the water contact angle is in this range, the surface of the F-DLC coating has better hydrophobicity, which has important application value in the fields of self-cleaning, anti-icing and drag reduction in water.
[0071] The roughness of the F-DLC coating ranges from 50.8 nm to 55.6 nm. The roughness will affect the hydrophobicity of the coating. When the roughness is within this range, the hydrophobicity of the F-DLC coating will increase with the increase of the roughness.
[0072] Among them, the grain size in the F-DLC coating ranges from 4.7μm to 53.2μm. The grain size affects the microstructure and mechanical properties of the coating. When the grain size is in this range, the hardness and wear resistance of the F-DLC coating can be improved.
[0073] Please refer to Table 1, which shows the composition ratio of the F-DLC coating obtained at different pulse bias values, sp 3 Hybridized carbon with sp 3 The proportion of hybrid carbon, as well as the water contact angle, roughness, and grain size of the corresponding F-DLC coating. The unit of pulse bias voltage is V, and the unit of F-DLC coating composition ratio is %, sp 3Hybridized carbon with sp 3 The unit of the ratio of hybridized carbon is %, the unit of the water contact angle is °, the unit of the roughness is nm, and the unit of the grain size is μm.
[0074] Table 1
[0075] Pulse bias F-DLC coating composition ratio / (F / C) <![CDATA[sp 3 / sp 2 ]]> Water contact angle Roughness Grain size 100 1 4 103 50.8 4.7 220 2 16 117 51.3 5.3 340 4 28 135 54.5 12.3 460 6 40 150 54.6 18.6 580 8 57 153 55.6 27.5 700 10 72 159 50.9 53.2
[0076] It can be seen from Table 1 that by adjusting the pulse bias of cathode vacuum arc plasma deposition, the F / C and sp in the F-DLC coating can be controlled simultaneously. 3 / sp 2 Due to the high ratio of fluorine to sp 3 The percentage content of hybrid carbon atoms can effectively improve the thermal insulation and lubricity of the die-casting mold coated with F-DLC coating. 3 Hybridized carbon / sp 2 The preferred proportion of hybrid carbon is 57%. Here, the F-DLC coating has the best matching degree of fluidity of the soup (semi-solid pre-pressed material) in the die casting mold under the condition of thermal insulation and the influence of grain size.
[0077] From the water drop angle characteristics of the F-DLC coating, it can be seen that as the fluorine ratio increases, the water drop angle trend also increases, while the surface roughness has no obvious upward and downward trend. Among them, the best result is when the F / C ratio is 8%. The die casting obtained under this ratio is full of molds, and there is no cracking on the surface of the die castings, which means that the F-DLC coating can provide good soup sliding and insulation, so that the heat field in the die casting cavity of the die casting mold is uniform and a single heat source is maintained to prolong the fluidity of the soup.
[0078] Please refer to Table 2, which shows the composition ratio of the F-DLC coating and the corresponding roughness. The unit of the composition ratio of the F-DLC coating is %, and the unit of the roughness is nm.
[0079] Table 2
[0080] F-DLC coating composition ratio (F / C) Test 1 Test 2 Test Three Test 4 average 2 55.6 50.7 45.1 53.9 51.3 4 54.1 55.7 50.8 57.5 54.5 6 37.3 59.6 71.6 49.7 54.6 8 56.7 58.4 47.1 60.0 55.6 10 42.7 59.8 46.0 55.0 50.9
[0081] See also Figure 5 , Figure 5 The metallographic image of the F-DLC coating obtained in one embodiment of the present application. Figure 5 By measuring any four test points in the F-DLC coating in multiple embodiments, a set of data in Table 2 can be obtained. It can be seen from Table 2 that in different F-DLC coating composition ratios (F / C), the average roughness of the F-DLC coating surface is 53nm.
[0082] In addition, by analyzing the grain size, it was found that the F / C ratio was 8% and sp 3 Hybridized carbon / sp 2 When the proportion of hybrid carbon is 57%, the grain size is 27.5μm, which can achieve the saturated mold condition, indicating that the spherical crystal structure can reach the balance point between the flow of semi-solid soup and the solidification growth of grains at this grain size.
[0083] See also Figure 6 In a second aspect of an embodiment of the present application, a die-casting mold 100 is provided, comprising a die-casting mold body 10 and the F-DLC coating 20 as described above, a die-casting cavity 11 is opened on the die-casting mold body 10, and the F-DLC coating 20 is arranged on the cavity wall of the die-casting cavity 11 of the die-casting mold body 10.
[0084] In this embodiment, the F-DLC coating 20 can improve the surface conditions of the die-casting cavity 11 of the die-casting mold body 10, such as: low surface energy, low surface roughness, high surface hardness, thermal stability, etc., and can be extended to many industrial processing fields, such as: stamping, aluminum extrusion, CNC, etc.
[0085] See also Figure 7 A fourth aspect of the present application provides a die-casting method, comprising the following steps:
[0086] S21, obtaining a semi-solid pre-pressed material.
[0087] Among them, see Figure 8 The step of obtaining the semi-solid pre-pressed material comprises:
[0088] S211, obtaining a pre-pressed blank, wherein the pre-pressed blank comprises, by mass percentage: 0.4% silicon, 0.5% iron, 1.5% copper, 2.5% magnesium, 0.2% chromium, 5.5% zinc, 0.2% titanium, 0.3% manganese, and the remainder aluminum;
[0089] S212, heating the pre-pressed blank to 850° C. to 950° C. to melt the pre-pressed blank;
[0090] S213, homogenizing the melted pre-pressed blank for 35 minutes to 45 minutes;
[0091] S214, cooling the homogenized pre-pressed blank to a semi-solidification point to obtain a semi-solid pre-pressed blank.
[0092] In this embodiment, the pre-pressed blank is heated to 900° C., homogenized for 40 minutes, and then cooled to a semi-solidification point to increase a spherical crystal structure, so as to obtain a semi-solid pre-pressed blank.
[0093] S22, injecting a semi-solid pre-pressed material into the F-DLC coating surface on the cavity wall of the die-casting cavity of the die-casting mold as above, and obtaining a die-casting part after die-casting.
[0094] Specifically, the semi-solid pre-pressed material is first mixed and poured into a titanium eddy current resonance container, and then the titanium eddy current resonance container resonates at a frequency of 20 Hz. The resonated slurry is then injected into a die-casting machine. The die-casting machine then punches the semi-solid metal into the F-DLC coating surface on the cavity wall of the die-casting cavity of the die-casting mold at a stroke rate of 10 cm / s, and the die-casting is obtained after die-casting by the die-casting machine.
[0095] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, from any point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claim involved. In addition, it is obvious that the word "comprising" does not exclude other units or steps, and the singular does not exclude the plural.
[0096] Finally, it should be noted that the above implementation modes are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the preferred implementation modes, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention.
Claims
1. A method for preparing a die-casting mold, It is characterized in that The following steps are involved: Evacuating a vacuum ballast chamber of a cathode vacuum arc plasma device to adjust the air pressure in the vacuum ballast chamber to a first air pressure value, and adjusting the cathode pulse bias voltage to a first bias voltage value; Placing a die-casting mold body and a graphite target in the cathode vacuum arc plasma equipment, wherein a die-casting cavity is provided on the die-casting mold body; The gas pressure in the vacuum ballast chamber of the cathode vacuum arc plasma device is lowered from the first gas pressure value to a second gas pressure value, and the pulse bias voltage of the graphite target is lowered from the first bias voltage value to a second bias voltage value, wherein the second bias voltage value is in the range of 100V to 700V; Fluorine-containing gas is introduced into the cathode vacuum arc plasma device to form an F-DLC coating on the surface of the die-casting cavity, thereby obtaining a die-casting mold.
2. The preparation method according to claim 1, It is characterized in that The F-DLC coating includes sp 3 Hybridized carbon and sp 2 Hybridized carbon, the sp 3 Hybridized carbon with the sp 2 The ratio of hybrid carbon ranges from 4% to 72%.
3. The preparation method according to claim 1, It is characterized in that The F-DLC coating includes F element and C element, and the ratio of the F element to the C element ranges from 1% to 10%.
4. The preparation method according to claim 1, It is characterized in that The first air pressure value has a value range of 5.9×10 - 3 Pa~6.1×10 -3 Pa, the value range of the second air pressure value is 4.9×10 -3 Pa~5.1×10 -3 Pa, the first bias voltage value ranges from 950V to 1050V, and the time for forming the F-DLC coating after the pulse bias of the graphite target is reduced from the first bias voltage value to the second bias value ranges from 15min to 25min.
5. The preparation method according to claim 1, It is characterized in that The water contact angle of the F-DLC coating ranges from 103° to 159°.
6. The preparation method according to claim 1, It is characterized in that The roughness of the F-DLC coating ranges from 50.8 nm to 55.6 nm.
7. The preparation method according to claim 1, It is characterized in that The grain size of the F-DLC coating ranges from 4.7 μm to 53.2 μm.
8. A die casting mold, It is characterized in that include: A die-casting mold body, wherein a die-casting cavity is formed on the die-casting mold body; The F-DLC coating according to any one of claims 1 to 7, wherein the F-DLC coating is provided on the cavity wall of the die-casting cavity of the die-casting mold body.
9. A die casting method, It is characterized in that The following steps are involved: Obtaining a semi-solid pre-pressed material; The pre-pressed material is injected into the F-DLC coating surface on the cavity wall of the die-casting cavity of the die-casting mold according to claim 8 to obtain a die-casting part after die-casting.
10. The die casting method according to claim 9, It is characterized in that The step of obtaining the semi-solid pre-pressed material comprises: Obtaining a pre-pressed blank, wherein the pre-pressed blank comprises, by mass percentage: 0.4% silicon, 0.5% iron, 1.5% copper, 2.5% magnesium, 0.2% chromium, 5.5% zinc, 0.2% titanium, 0.3% manganese, and the remainder aluminum; Heating the pre-pressed blank to 850° C. to 950° C. to melt the pre-pressed blank; Homogenize the melted pre-pressed blank for 35 to 45 minutes; The homogenized pre-pressed blank is cooled to a semi-solidification point to obtain a semi-solid pre-pressed blank.