Coating method of high-corrosion-resistance infrared optical film for optical parts

By plating multi-layer high-corrosion-resistant infrared optical films on ship-based infrared optical equipment, the problems of oxidation and corrosion of light windows in high temperature, high humidity and high salt spray environments in the prior art are solved, and higher transparency is achieved Over-rate and corrosion resistance extend the service life of the equipment and improve optical performance.

CN118996347APending Publication Date: 2024-11-22KUNMING KAIHANG PHOTOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311008020.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-08-11
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing ship-based infrared optical equipment is prone to oxidation and corrosion in high temperature, high humidity and high salt spray environments, resulting in a degradation of light window performance and it is difficult to meet the technical requirements of ship-based equipment.

Method used

Using a highly corrosion-resistant infrared optical film coating method, multi-layer film structures are plating on the surface of optical parts such as fluorine glass and zinc sulfide, including materials such as JG, ZnS, HfO2, SiO2 and FSM, and ion beam sputtering deposition technology, Optimize the coating thickness and structural order to improve the film's transmittance and corrosion resistance.

Benefits of technology

It significantly improves the transmittance and corrosion resistance of infrared optical films, allowing them to work stably in harsh marine environments for a long time, extend the service life of optical windows and enhance their optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996347A_ABST
    Figure CN118996347A_ABST
Patent Text Reader

Abstract

The invention discloses a high-corrosion-resistance infrared optical film coating method for optical parts, and relates to the technical field of optical film preparation. The method comprises the following steps of: pre-treating an optical part which is qualified after surface smoothness inspection; and then plating the high-corrosion-resistance infrared optical thin film, sequentially loading corresponding film materials and parts into a crucible according to a first layer of JG, a second layer of ZnS, a third layer of JG, a fourth layer of HfO2, a fifth layer of SiO2, a sixth layer of HfO2, a seventh layer of HfO2, an eighth layer of SiO2, a ninth layer of JG and a tenth layer of FSM, and placing the crucible in a vacuum chamber. The invention provides the infrared optical film which has the advantages of high transmission, multiband, wide spectrum, good environmental adaptability and capability of resisting damage of severe environments such as high-temperature, high-salt and high-humidity sandstone in a photoelectric system under a marine environment condition, an optical window is protected, the optical window is enabled to have relatively long service life, the optical performance of the optical window is improved, the coverage range of a transmission band is relatively wide, and the transmission efficiency is relatively high. The purpose of enhancing the optical window performance is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical film preparation, and in particular relates to a highly corrosion-resistant infrared optical film coating method for optical parts. Background Art

[0002] At present, due to its special deployment location, the environmental conditions that shipborne infrared optical equipment is subjected to during parking, take-off and landing are very different from those of land-based equipment. The infrared optical equipment, external process conditions and deck support equipment installed on it will also be subjected to the test of special environmental conditions. It needs to adapt to the most extreme climate environment and special shipborne environment in my country's waters and even the world's waters, and needs to work stably for a long time in the marine atmospheric environment of high temperature, high humidity and high salt fog.

[0003] Since the existing infrared optical equipment has oxidation and corrosion in the optical window after a few months, it is difficult to meet the technical indicators of shipborne optical equipment. Therefore, it is necessary to improve the technology to solve the above problems. Summary of the invention

[0004] The purpose of the present invention is to provide a method for coating optical parts with a high corrosion resistance infrared optical film. By providing a high-transmittance and high-corrosion resistance infrared optical film suitable for shipborne infrared optical windows, the problems of poor environmental adaptability and poor transmittance performance of existing shipborne infrared windows are solved.

[0005] In order to solve the above technical problems, the present invention is achieved through the following technical solutions: The present invention is a method for coating a highly corrosion-resistant infrared optical thin film for optical parts, which is coated on the surface of optical parts such as oxyfluoride glass, zinc sulfide, and sapphire. The structural sequence and film thickness of the film and the coating method specifically include the following steps: (1) Pre-treat the optical parts that have passed the surface finish inspection; (2) For the coating of highly corrosion-resistant infrared optical films, the details are as follows: ① Load the corresponding film materials and parts into the crucible in the order of the first layer of JG, the second layer of ZnS, the third layer of JG, the fourth layer of HfO2, the fifth layer of SiO2, the sixth layer of HfO2, the seventh layer of HfO2, the eighth layer of SiO2, the ninth layer of JG, and the tenth layer of FSM, and place it in the vacuum chamber; ② Vacuum to 4.0x10 -4 Pa±2x10 -4 Pa, keep it for more than 2h, baking temperature: 150℃±10℃, baking time: 30 minutes, ion source bombards the surface of the part for 5 minutes, beam current: 100mA, Ar: 15sccm.

[0006] ③ Using ion beam sputtering deposition process, when coating the first and second layers of the film, the temperature is set to 200℃, the heating rate is 7℃ / min, the constant temperature time is greater than 60min after reaching the set temperature, the ion source bombardment is 10min, the beam current is 150mA, Ar: 15sccm, the physical thickness is: 150nm for the first layer and 123nm for the second layer, and the correction coefficients are 84 and 44 respectively; After the deposition of the first and second layers is completed, the surface of the part is bombarded with an ion beam for 5 minutes, with a beam current of 100 mA and an Ar of 15 sccm. After the bombardment, three to nine layers are plated in sequence, with an open source beam current of 150 mA and an Ar of 15 sccm. The physical thickness is: 98 nm for the third layer, 67.9 nm for the fourth layer, 234.7 nm for the fifth layer, 21.4 nm for the sixth layer, 161.8 nm for the seventh layer, 93.3 nm for the eighth layer, and 50 nm for the ninth layer. The hafnium oxide plating process is oxygenated at 95 sccm, namely the fourth, sixth and seventh layers.

[0007] After the ninth layer is deposited, the vacuum is pumped to 6.0x10 -4 Below Pa, beam current 100 mA, Ar: 15 sccm, temperature does not rise, ion source is turned off, rate setting 4, power setting 6, physical thickness 70 nm.

[0008] After plating is completed, turn off the ion source, bake, cool naturally to below 100°C, close the high valve, reduce the vacuum chamber temperature to below 60°C, and open the door to take out the parts.

[0009] Furthermore, when the optical parts are pretreated in step (1), the optical parts before coating are first soaked in gasoline for 2 hours and then in alcohol for 2 hours.

[0010] Furthermore, when the optical parts are pre-treated in step (1), the parts are wiped and the cleanliness of the parts surface is tested by the breath method. After the parts are wiped clean, they are plated with a highly corrosion-resistant infrared optical film.

[0011] Furthermore, when pre-treating the optical parts in step (1), check whether the oxygen and argon gases are sufficient before plating.

[0012] Furthermore, when the optical parts are pretreated in step (1), the conditions in the vacuum chamber and the water temperature of the water cooling system should be frequently observed during the plating process.

[0013] Furthermore, when the optical parts are pre-processed in step (1), the vacuum chamber is cleaned, and the ion source, filament, etc. are inspected and cleaned.

[0014] Furthermore, when the highly corrosion-resistant infrared optical film is plated in step (2), the entire process lasts for about 20 to 24 hours.

[0015] Furthermore, when the highly corrosion-resistant infrared optical film is plated in step (2), the infrared optical film can be applied to infrared optical materials such as oxyfluoride glass, zinc sulfide, and sapphire, and can increase the substrate transmittance by more than 20% @ 0.9-1.7 μm, 3.6-4.8 μm, and meet the requirements of high temperature, high humidity, high salt, and high corrosion resistance environment tests at sea.

[0016] The present invention has the following beneficial effects: the present invention provides an infrared optical film with high transmittance, wide spectrum, good environmental adaptability and resistance to damage from harsh environments for an infrared photoelectric system under marine environmental conditions, thereby protecting the optical window, making the optical window have a longer service life, improving its optical performance and making the transmission band coverage wider, thereby achieving the purpose of enhancing the performance of the optical window. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0018] Figure 1 This is a schematic diagram of the structure of infrared optical high-temperature, high-humidity, high-salt and high-corrosion-resistant optical thin film layer; Figure 2 This is the test chart of the transmittance @0.9~1.7μm of infrared optical film in high temperature, high humidity, high salt and high corrosion resistance environment; Figure 3 This is the test chart of the transmittance @3.8~4.8μm of infrared optical film in high temperature, high humidity, high salt and high corrosion resistance environment; Implementation

[0019] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0020] See also Figure 1-2 As shown, the present invention is a method for coating a highly corrosion-resistant infrared optical thin film for optical parts, which is coated on the surface of optical parts such as oxyfluoride glass, zinc sulfide, and sapphire. The structural sequence and film thickness of the film and the coating method specifically include the following steps: (1) Pre-process the optical parts that have passed the surface finish inspection as follows: ① Soak the optical parts in gasoline for 2 hours and alcohol for 2 hours before coating; ② Wipe the surface of the parts and use the breath method to detect the cleanliness of the surface. After wiping, the parts will be plated with a highly corrosion-resistant infrared optical film; Before plating, check that there is enough oxygen and argon. During the plating process, you should often observe the conditions in the vacuum chamber (such as the temperature in the vacuum chamber, whether the film material is sputtering, whether the parts hanging plate revolves and rotates normally, etc.), and observe the water temperature of the water cooling system; Clean the vacuum chamber, check and clean the ion source, filament, etc.; (2) For the coating of highly corrosion-resistant infrared optical films, the details are as follows: ① Load the corresponding film materials and parts into the crucible in the order of the first layer of JG, the second layer of ZnS, the third layer of JG, the fourth layer of HfO2, the fifth layer of SiO2, the sixth layer of HfO2, the seventh layer of HfO2, the eighth layer of SiO2, the ninth layer of JG, and the tenth layer of FSM, and place it in the vacuum chamber; ② Vacuum to 4.0x10 -4 Pa±2x10 -4 Pa, keep for more than 2 hours, baking temperature: 150℃±10℃, baking time: 30 minutes, ion source bombards the surface of parts for 5 minutes, beam current: 100mA, Ar: 15sccm; ③ Using ion beam sputtering deposition process, when coating the first and second layers of the film, the temperature is set to 200℃, the heating rate is 7℃ / min, the constant temperature time is greater than 60min after reaching the set temperature, the ion source bombardment is 10min, the beam current is 150mA, Ar: 15sccm, the physical thickness is: 150nm for the first layer and 123nm for the second layer, and the correction coefficients are 84 and 44 respectively; After the deposition of the first and second layers is completed, the surface of the part is bombarded with an ion beam for 5 minutes, with a beam current of 100 mA and an Ar of 15 sccm. After the bombardment, three to nine layers are plated in sequence, with an open source beam current of 150 mA and an Ar of 15 sccm. The physical thickness is: 98 nm for the third layer, 67.9 nm for the fourth layer, 234.7 nm for the fifth layer, 21.4 nm for the sixth layer, 161.8 nm for the seventh layer, 93.3 nm for the eighth layer, and 50 nm for the ninth layer. The hafnium oxide plating process is oxygenated at 95 sccm, namely the fourth, sixth and seventh layers.

[0021] After the ninth layer is deposited, the vacuum is pumped to 6.0x10 -4 Below Pa, beam current 100 mA, Ar: 15 sccm, temperature does not rise, ion source is turned off, rate setting 4, power setting 6, physical thickness 70 nm.

[0022] After plating is completed, turn off the ion source, bake, cool naturally to below 100°C, close the high valve, reduce the vacuum chamber temperature to below 60°C, and open the door to take out the parts.

[0023] The whole process lasts about 20 to 24 hours. The infrared optical film can be applied to infrared optical materials such as oxyfluoride glass and zinc sulfide. It can increase the transmittance of the substrate by more than 20% @ 0.9-1.7μm and 3.6-4.8μm, and meet the test requirements of high temperature, high humidity, high salt and high corrosion resistance environment at sea.

[0024] The above are only preferred embodiments of the present invention and do not limit the present invention. Any modification to the technical solutions recorded in the aforementioned embodiments, any equivalent replacement of some of the technical features therein, and any modification, equivalent replacement, and improvement made are all within the protection scope of the present invention.

Claims

1. A method for coating an infrared optical thin film with high corrosion resistance for optical parts, characterized in that: The film is plated on the surface of optical parts such as oxyfluoride glass, zinc sulfide, sapphire, etc. The structural sequence and film thickness of the film and the plating method specifically include the following steps: (1) Pre-treat the optical parts that have passed the surface finish inspection; (2) For the coating of highly corrosion-resistant infrared optical films, the details are as follows: ① Load the corresponding film materials and parts into the crucible in the order of the first layer of JG, the second layer of ZnS, the third layer of JG, the fourth layer of HfO2, the fifth layer of SiO2, the sixth layer of HfO2, the seventh layer of HfO2, the eighth layer of SiO2, the ninth layer of JG, and the tenth layer of FSM, and place it in the vacuum chamber; ② Vacuum to 4.0x10 -4 Pa±2x10 -4 Pa, keep for more than 2h, baking temperature: 150℃±10℃, baking time: 30min, ion source bombards the surface of parts for 5min, beam current: 100mA, Ar: 15sccm; ③ Using ion sputtering deposition process, when coating the first and second layers of the film, the temperature is set to 200℃, the heating rate is 7℃ / min, the constant temperature time is greater than 60min after reaching the set temperature, the ion source bombardment is 10min, the beam current is 150mA, Ar: 15sccm, the physical thickness is: 150nm for the first layer and 123nm for the second layer, and the correction coefficients are 84 and 44 respectively; After the first and second layers are deposited, the surface of the parts is bombarded with ion beams for 5 minutes, with a beam current of 100 mA and an Ar of 15 sccm. After the bombardment, the third to ninth layers are plated in sequence, with an open source throughout the process, a beam current of 150 mA and an Ar of 15 sccm. The physical thickness is: 98 nm for the third layer, 67.9 nm for the fourth layer, 234.7 nm for the fifth layer, 21.4 nm for the sixth layer, 161.8 nm for the seventh layer, 93.3 nm for the eighth layer, and 50 nm for the ninth layer. The hafnium oxide plating process is oxygenated at 95 sccm, i.e. the fourth, sixth and seventh layers. After the ninth layer is deposited, the vacuum is pumped to 6.0x10 -4 Pa or less, beam current 100 mA, Ar: 15 sccm, temperature does not rise, ion source is turned off, rate setting 4, power setting 6, physical thickness 70 nm; After plating is completed, turn off the ion source, bake, cool naturally to below 100°C, close the high valve, reduce the vacuum chamber temperature to below 60°C, and open the door to take out the parts.

2. The method for coating an optical component with a highly corrosion-resistant infrared optical thin film according to claim 1, characterized in that: When pre-treating the optical parts in step (1), the optical parts before coating are first soaked in gasoline for 2 hours and then in alcohol for 2 hours.

3. The method for coating an optical component with a highly corrosion-resistant infrared optical thin film according to claim 1, characterized in that: When the optical parts are pretreated in step (1), the parts are wiped and the cleanliness of the parts surface is tested by the breath method. After wiping, the parts are plated with a highly corrosion-resistant infrared optical film.

4. The method for coating an optical component with a highly corrosion-resistant infrared optical thin film according to claim 1, characterized in that: When pre-treating the optical parts in step (1), check that there is sufficient oxygen and argon before plating.

5. The method for coating an optical component with a highly corrosion-resistant infrared optical thin film according to claim 1, characterized in that: When pre-treating the optical parts in step (1), the conditions in the vacuum chamber and the water temperature of the water cooling system should be frequently observed during the plating process.

6. The method for coating an optical component with a highly corrosion-resistant infrared optical thin film according to claim 1, characterized in that: When pre-treating the optical parts in step (1), clean the vacuum chamber, and check and clean the ion source, filament, etc.

7. The method for coating an optical component with a highly corrosion-resistant infrared optical thin film according to claim 1, characterized in that: When the highly corrosion-resistant infrared optical film is plated in step (2), the whole process lasts about 20 to 24 hours.

8. The method for coating an optical component with a highly corrosion-resistant infrared optical thin film according to claim 1, characterized in that: When the highly corrosion-resistant infrared optical film is plated in step (2), the infrared optical film can be applied to infrared optical materials such as oxyfluoride glass, zinc sulfide, and sapphire, and can increase the substrate transmittance by more than 20% @ 0.9-1.7 μm, 3.6-4.8 μm, and meet the requirements of high temperature, high humidity, high salt, and high corrosion resistance environment tests at sea.