WNiX sputtering target

The WNiX sputtering target was produced by powder metallurgy method, and the mixed phase structure of W, Ni and X was used to solve the ferromagnetic and microstructure roughness of the sputtering target in the prior art, achieving uniform sputtering behavior and high mechanical properties .

CN118996352APending Publication Date: 2024-11-22PLANSEE SHANGHAI HIGH PERFORMANCE MATERIAL +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310549498.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing sputtering targets have ferromagnetic pure nickel parts in magnetron sputtering, resulting in unstable coating rate and unevenness of the deposition layer. The microstructure of the target materials produced by the melt metallurgy method is rough, making it easy to see relief and Problem of brittle cracks.

Method used

WNiX sputtering targets are produced by powder metallurgy method, using W, Ni and metal X of Group 5 or Group 6 of the periodic table. A pure W phase and a mixed phase of NiWX, NiW and NiX appear in the microstructure to ensure the target material The uniformity and magnetic properties of the product are used to compact, sinter and forming steps to achieve high density and low oxygen content.

Benefits of technology

The uniformity in chemical composition and layer thickness distribution is achieved, the appearance of ferromagnetic Ni phase is avoided, the uniformity of sputtering behavior and the mechanical properties of the target are ensured, and undesired local melting and brittleness problems are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996352A_ABST
    Figure CN118996352A_ABST
Patent Text Reader

Abstract

The present invention relates to a sputtering target manufactured by a powder metallurgy method comprising tungsten (W), nickel (Ni) and a further metal X selected from the group comprising Group 5 or Group 6 of the periodic table, and unavoidable impurities, in which the sputtering target has a two-phase microstructure in which one phase is pure W and the other phase is a mixed phase selected from the group comprising NiWX, NiW, NiX and mixtures thereof. The invention also relates to a method for producing a WNiX sputtering target by means of powder metallurgy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a WNiX sputtering target produced by powder metallurgy, wherein X is selected from the group comprising Group 5 or Group 6 of the periodic table of elements. The present invention also relates to a method for producing a WNiX sputtering target by powder metallurgy. Background Art

[0002] Sputtering, also known as cathode atomization, is a physical process in which atoms are detached from a sputtering target and enter the gas phase by bombardment with high-energy ions.

[0003] Sputtering targets composed of Ni, W and optionally one or more further metals X, in particular selected from the group of refractory metals, in particular NiWCr and NiWTa, are known in the prior art.

[0004] However, a problem of the prior art is that the use of nickel powder as a starting material for the manufacture of the target material results in the presence of pure nickel in the target material which exhibits ferromagnetic properties. This means that ferromagnetic pure Ni parts or Ni phases appear in the microstructure of such a sputtering target. Ferromagnetic properties are disadvantageous for magnetron sputtering, since they lead to different and unstable coating rates and therefore have an adverse effect on the uniformity of the possible deposited layers to be formed. In comparison with the above-described "simple" cathode atomization, a magnetic field is additionally generated in the case of magnetron sputtering. The superposition of electric and magnetic fields prolongs the path of the charge carriers and increases the number of collisions per electron.

[0005] For example, EP3825427A1 relates to a sputtering target comprising Ni, W and optionally one or more other metals X selected from refractory metals (e.g., Ti, V, Cr, Mn, Zr, Nb, etc.), Sn, Al and Si. In this application, the sputtering target has a normalized peak intensity ratio of 0.40 or more, which includes a pure Ni portion.

[0006] CN104646930A relates to a method for manufacturing a NiWCr alloy target, including smelting, ingot casting, forging, primary heat treatment, hot rolling, cold rolling and secondary heat treatment. CN102534308A discloses a NiWCr alloy target with 15-35% by weight of W and 5-15% by weight of Cr constituents. The material is also prepared by melting, casting, hot forging, cold rolling and recrystallization annealing steps. JP2010-133001A teaches a method for manufacturing a Ni alloy target, wherein the Ni alloy target contains 10 to 30% by mass of one or more selected from (Cr, Mo, W), the balance being Ni, wherein the target is obtained by melting, casting, plastic working and recrystallization treatment. However, the sputtering target produced by melt metallurgy shows the disadvantage of a rough microstructure after the casting step, which leads to the formation of relief by uneven erosion during the sputtering process or cracks due to the brittleness of the coarse grain microstructure. This problem can be solved by a powder metallurgy production process. Sputtering targets manufactured by powder metallurgy show a very uniform fine-grained microstructure after sintering, which subsequently ensures uniform erosion and optimized thin layers during sputtering. Although some of the above patent applications mention fine and uniform grain size in the target, this grain size is achieved by an additional production step after casting.

[0007] WO2010 / 009829 discloses a sputtering target made of a NiWCr alloy containing 1-20 atomic % W and 1-20 atomic % Cr, with the remainder being Ni. The sputtering target can be manufactured by casting or powder metallurgy production. However, the document does not mention the microstructure of the alloy target. Therefore, it is not obvious whether there is a pure Ni portion in the microstructure of the sputtering target.

[0008] JP2009-155722A teaches a sintered target material containing 3 to 15 atomic % W, 20 atomic % or less Cr, and the balance being Ni. The microstructure is described as a face-centered cubic structure. The present application provides a sputtering target having more than 15 atomic % W.

[0009] The sputtering targets described in the prior art do not meet the increasing requirements with regard to layer homogeneity, homogeneity of the sputtering behavior and avoidance of undesired local partial melting. Local partial melting is caused, for example, by arc processes (local formation of an arc). Summary of the invention

[0010] The object of the present invention is to provide a WNiX sputtering target with which layers which are very homogeneous both in terms of chemical composition and layer thickness distribution can be produced, wherein the microstructure contains no pure (or elemental) Ni phases. In addition, the sputtering target should have a homogeneous sputtering behavior. Here, homogeneous sputtering behavior means that the individual phases in the microstructure of the sputtering target can be ablated at the same rate.

[0011] Another object of the present invention is to provide a method for producing a WNiX sputtering target having the above-mentioned properties in a simple, reproducible and inexpensive manner.

[0012] This object is achieved by the independent claim. Advantageous embodiments are indicated in the dependent claims.

[0013] The sputtering target of the present invention comprises tungsten (W), nickel (Ni), one other metal X selected from the group including Group 5 or Group 6 of the periodic table, and inevitable impurities. The sputtering target has the following characteristics: measured at the cross section of the target material, the microstructure shows a two-phase microstructure, one phase is pure W (i.e., W grains), and the other phase is a mixed phase selected from the group including NiWX, NiW, NiX and mixtures thereof.

[0014] For the purposes of the present invention, “microstructure” is understood to mean the microstructure of the sputtering target, which can be analyzed in a simple manner familiar to the person skilled in the art by means of metallographically polished sections and evaluation under an optical microscope or a scanning electron microscope.

[0015] The presence of pure W phases as well as mixed phases in the sputtering targets according to the invention can be very easily confirmed or excluded by X-ray diffraction (XRD) (taking into account the respective X-ray detection limits) using JCPDS (Joint Committee on Powder Diffraction Standards) cards. A mixed phase refers to a phase that occurs in a binary or ternary component system, which is different from the pure elemental components used as starting elements. They generally have a crystal structure that deviates from the crystal structure of the pure components, and the mixed phase is characterized by a composition with inexact (meaning that the valence does not directly correspond to the valence of the pure components) valences.

[0016] The two-phase microstructure of the sputtering target refers to the presence of a pure W phase and a mixed phase, but other additional phases, such as oxides or pores, may also be present therein. However, the proportion of these additional phases should be as small as possible, since they may have a negative impact on the sputtering behavior, in particular its homogeneity. Thus, oxides, for example, can promote the occurrence of local incipient melting (arcing).

[0017] The presence of mixed phases is not detrimental to the magnetic properties of the sputtering target according to the invention, since the Ni-containing phases that occur in the WNiX system, ie NiWX, NiW or NiX, are not ferromagnetic.

[0018] The term "inevitable impurities" refers to production-related contamination with gases or associated elements, which originate from the raw materials used. In the sputtering target of the present invention, the proportion of these impurities is preferably below 350 μg / g (equivalent to ppm) for gases (C, H, N, O) and below 300 μg / g for other elements (Al, Ca, Cd, Cu, Fe, K, Li, Mg, Mn, Na, P, Pb, S, Zr). Suitable methods for known chemical element analysis depend on the chemical elements to be analyzed. The chemical analysis of the inevitable impurities of the present invention is carried out by thermal extraction analysis of the elements of O, N, H, or by combustion analysis of the elements of C and S, or using ICP-MS (inductively coupled plasma mass spectrometry) or ICP-OES (inductively coupled plasma optical emission spectroscopy).

[0019] Chemical analysis of W, Ni, and X, which are main components in the sputtering target of the present invention, is performed using XRF (X-ray fluorescence analysis).

[0020] In a preferred embodiment of the present invention, the other metal X is a metal selected from the elements Cr, Mo, Nb or Ta, more preferably the other metal X is Cr or Ta.

[0021] The high electrical conductivity of molybdenum, tungsten, tantalum, niobium and chromium in particular is advantageous for use as conductor tracks or lines. The low thermal expansion coefficient, in particular of molybdenum, tungsten, tantalum, niobium and chromium, ensures good adhesion and low layer stress of the deposited layer when deposited on a substrate.

[0022] Preferably, the sputtering target according to the present invention contains 38-70 wt. % W, 25-50 wt. % Ni, 5-22 wt. % X and the maximum proportion of unavoidable impurities is ≤650 μg / g. It is obvious to a person skilled in the art that the total amount of W+Ni+X+ impurities is 100 wt. %. When the W content is less than 38 wt. %, a ferromagnetic Ni phase may be produced in the sputtering target. If the W content is higher than 70 wt. %, the hardness of the target material is too high to ensure optimal and economical processing performance. When the above-mentioned W content is 38-70 wt. %, the appearance of a mixed phase consisting of a NiWX phase, an optional NiW phase, an optional NiX phase or an optional mixture thereof is very advantageous. The preferred composition of the sputtering target includes 40-67 wt. % W, 26-46 wt. % Ni, and 6-21 wt. % X. Preferably, according to the present invention, the maximum proportion of unavoidable impurities is less than or equal to 300 μg / g. Also in this case, it is obvious that the total amount of W+Ni+X+ impurities is 100 wt. %.

[0023] The sputtering target according to the invention preferably has a relative density of greater than 85%. A relative density of greater than 90% is particularly advantageous. The density of the sputtering target is highly dependent on the element X in the WNiX target, in particular the O content in the element X powder. The higher the density of the target, the more favorable its properties. Targets with a low relative density have a relatively high proportion of pores, which can be actual leaks and / or sources of impurities and particles during the sputtering process. In addition, targets with a low density tend to absorb water or other impurities, which can lead to difficult-to-control process parameters. In addition, during the sputtering process, the ablation rate of a material that has been densified to only a low degree is lower than the ablation rate of a material with a higher relative density.

[0024] As is known, the absolute density can be easily determined by the buoyancy method using Archimedes' principle. The relative density can be determined, for example, by microscopic photographs.

[0025] The sputtering target according to the invention preferably has an oxygen content of less than 350 μg / g, preferably less than 100 μg / g, more preferably less than 75 μg / g, even more preferably less than 30 μg / g. By having such a low oxygen content, undesirable arc processes during sputtering can be reliably avoided.

[0026] The oxygen content can be determined in a simple manner by thermal extraction analysis.

[0027] The sputtering target according to the invention is characterized by a hardness of preferably less than 400 HV10 after the pressing and sintering steps. It has been found that a satisfactory toughness of the target material can be best ensured at a hardness of less than 400 HV10. This simplifies handling during the manufacturing process, for example in an optional mechanical forming step. During use, especially as a one-piece tubular target in one embodiment, a hardness of less than 400 HV10 significantly simplifies handling. By carrying out one or more forming steps after pressing and sintering, the hardness of the sputtering target according to the invention can be increased to 600 HV10.

[0028] For the purposes of the present invention, the HV10 hardness (Vickers hardness) is the arithmetic mean determined from 5 hardness measurements.

[0029] The installation of the sputtering target according to the invention in various coating devices and for coating substrates with different geometries places various geometric demands on the sputtering target according to the invention. Thus, a target of this type can be in the form of a planar sputtering target, such as a plate or disk, or in the form of a tubular sputtering target. In addition, other target forms are also within the scope of the invention, for example, a rod or a body with another complex shape.

[0030] The sputtering target according to the present invention may be a multi-component sputtering target or a one-piece sputtering target.

[0031] With regard to the design as a one-piece tubular sputtering target, this enables the deposition of particularly uniform layers on large-area substrates, since there are no discontinuities (e.g. joints, undercuts, residues of solder material, impurities in the joint area) between the individual pieces (segments) of the target.

[0032] Compared to multi-component tubular targets, the design as a one-piece tubular target makes it possible to avoid movement of individual components of the target due to different temperatures or temperature cycles during the coating process. In addition, the homogeneity of the target material in terms of chemical purity or microstructure is better in the case of a one-piece tubular target than in the case of a multi-component tubular target.

[0033] However, the sputtering target according to the invention can be configured not only as a one-piece tubular target. As described above, it can also exist as a multi-part tubular target or have various regions with different outer diameters or relative densities over its length ("dog bone" target). Such an embodiment can reduce or greatly avoid, for example, uneven ablation of the sputtering target at the end of the target material ("cross angle effect"). Targets with regions of different diameters can also be constructed as one-piece targets and multi-part targets.

[0034] The sputtering target according to the present invention preferably has an area ratio of the W phase measured on the cross section of the target material of 5% to 50%, preferably 15% to 45%.

[0035] An area ratio of the W phase of less than 5% may be associated with an increase in the proportion of the ferromagnetic Ni phase, thus resulting in poor sputtering behavior. An area ratio of the W phase exceeding 50% has an adverse effect on the hardness and processing properties of the target.

[0036] The area ratio of the W phase is determined by appropriate evaluation of a metallographically polished section. A metallographically polished section is a two-dimensional section of a three-dimensional target. Regional analysis can be performed on a micrograph produced in this way by commercially available image analysis software. This is performed by image analysis (usually by contrasting the phases to be distinguished) in order to determine the proportions of the individual phases in the above-mentioned microstructure. The average area ratio is calculated as the arithmetic mean of 5 area ratio measurements measured on 5 image areas with a size of 600×500 μm of a metallographically polished section, recorded at a magnification of 200:1.

[0037] The sputtering target according to the present invention preferably has an average grain size of the W phase of less than 40 μm, more preferably less than 30 μm.

[0038] The average grain size of the W phase is less than 40 μm, more preferably less than 30 μm, resulting in a particularly uniform sputtering behavior and thus in the deposition of a particularly uniform layer with a particularly uniform thickness. In addition, the notch effect of the W phase is kept low in this way, as a result of which a satisfactory toughness of the target material is optimally ensured.

[0039] The diameter of the aggregates of a plurality of crystal grains of the W phase may exceed 40 μm, but in the sputtering target of the present invention, these aggregates cannot be considered as single crystal grains of the W phase.

[0040] The average grain size of the W phase can be determined in a simple manner on a metallographically polished cross section by the wire section method as shown, for example, in ASTM E112-12.

[0041] The method for manufacturing a WNiX sputtering target by a powder metallurgy route according to the present invention is characterized in that the method comprises at least the following steps:

[0042] - A compacting step in which a mixed powder of W powder, Ni powder and X powder is compacted by applying pressure, heat, or pressure and heat to obtain a blank.

[0043] The compaction step as part of the method for manufacturing a WNiX sputtering target according to the present invention results in compacting and densifying a suitable powder mixture by applying pressure, heat or pressure and heat to form a blank. This can be done by various process steps, for example by pressing and sintering, cold isostatic pressing, hot isostatic pressing, hot pressing or spark plasma sintering (SPS) or a combination of these methods or other methods of compacting the powder mixture.

[0044] The manufacture of a powder mixture that can be used in the method according to the invention is preferably achieved by mixing appropriate amounts of W powder, Ni powder and X powder. These powders are filled into a suitable mixing device and mixed until a uniform distribution of the components in the powder mixture is ensured. For the purposes of the present invention, the expression powder mixture may include a pre-alloyed or partially alloyed powder containing the components W, Ni and X.

[0045] In a preferred embodiment, the mixing of the powders is performed in an inert atmosphere, for example by using the inert gases argon or nitrogen.

[0046] The powder mixture produced in this way is preferably introduced into a mold for carrying out the compaction step. Suitable molds here are molds or flexible tubes of a cold isostatic press, molds of a hot press or spark plasma sintering equipment, or capsules in the case of hot isostatic pressing.

[0047] It has been found that in the method according to the invention for producing a WNiX sputtering target, it is particularly advantageous to implement the compaction step by sintering at a temperature of 1100 to 1450° C. Preferably, the sintering temperature is in the range of 1250 to 1400° C. Here, sintering is a sintering method known as pressureless sintering at a pressure of less than 2 MPa, preferably at a pressure below atmospheric pressure.

[0048] Compacting at these temperatures optimally ensures that solid phase sintering or liquid phase sintering to very high relative densities occurs in the powder mixture present. In the case of compacting below 1100° C., the achievable density may be too low, while at temperatures above 1450° C. a reduction in the mechanical stability of the target may occur. In the case of compacting in the temperature range indicated, an optimal combination of high density achieved and optimal mechanical properties is ensured, and low oxygen contents can be achieved.

[0049] Sintering is advantageously carried out under vacuum, in an inert atmosphere and / or a reducing atmosphere. For the purposes of the present invention, an inert atmosphere is a gaseous medium that does not react with the alloy components, such as a noble gas. A suitable reducing atmosphere is in particular hydrogen.

[0050] The blank obtained by the method according to the invention can then be subjected to a forming step to possibly produce advantageous properties, such as a further increase in density and / or a further homogenization of the microstructure. Suitable methods for implementing the forming step for the purposes of the invention are, for example, rolling, extrusion and forging. Preferably, rolling or forging is used as a suitable forming step.

[0051] The forming step for the purposes of the present invention can be carried out as a single-stage or multi-stage process. A combination of a plurality of suitable methods is also possible. Thus, the forming process can comprise one or more sub-steps.

[0052] By means of a forming process comprising at least one forging step or rolling step, a defined degree of deformation can be introduced into the target material in a particularly targeted manner. In this way, for example, excessive reinforcement and thus exceeding the deforming forces that can be applied can be avoided.

[0053] By means of a forming process which includes at least one rolling step or forging step, textures can be introduced into the target material in a targeted manner, and these textures can in turn have a positive influence on the mechanical properties and sputtering properties of the target material.

[0054] Furthermore, by using one or more rolling steps or forging steps, the thickness of the shaped material can be varied over its length and set in a targeted manner. This thickness can be used, among other things, to increase the sputtering efficiency (regions with different outer diameters over the length, "dog-bone" targets).

[0055] In addition, rolling can be used to obtain a uniform surface quality that is beneficial for further machining, and forging or rolling can achieve straightness and good roundness.

[0056] The method for manufacturing a sputtering target according to the present invention may further include the following steps:

[0057] -Heat treatment.

[0058] After compaction by pressure, heat or pressure and heat, and after any forming step, it is advantageous to heat treat the blank. Depending on the chemical composition of the sputtering target, the temperature employed may be in the range of 1000 to 1200° C. Moreover, the effect of this heat treatment may come from the exclusive dissipation of stresses, up to the modification of the microstructure by the movement of small and / or large angle grain boundaries.

[0059] After the compaction step, after the optional shaping step or after the optional heat treatment step, it may be desirable or necessary to mechanically process the blank or target obtained. Such mechanical processing, for example by cutting, grinding or polishing, enables the final geometry to be set or made more precise and, for example, a particularly desired surface quality to be set. These processing steps can be configured as dry or wet processing steps.

[0060] The sputtering target produced by the method according to the invention can also be applied, for example, by a bonding step, to one or more suitable support elements. Such support elements can be, for example, backing plates of various geometries or, in the preferred case of tubular sputtering targets, in particular monolithic tubular targets, support tubes or support elements which do not extend through the entire tube, such as ports, flanges or other connecting parts or multi-part support tubes or support elements.

[0061] Such a support element may be made, for example, of stainless steel, Cu, a Cu alloy, Ti or a Ti alloy. However, other materials may also be used to manufacture such a support element.

[0062] For the bonding step, preferably elements or alloys with a low melting point are used, such as indium. Furthermore, adhesives, such as Ni, can optionally be used to ensure better wettability. Instead of the bonding step, the application to a suitable support element can also be performed by means of welding or adhesive bonding or by mechanical locking, such as by screwing or clamping.

[0063] In the method according to the invention for producing a WNiX sputtering target, as a further step, a corrosion-resistant protective device, for example in the form of a paint or varnish or a polymer coating, can also be applied to at least part of the inner diameter of the target material.

[0064] In a preferred case, a sputtering target is produced by the method according to the invention for producing a WNiX sputtering target, the sputtering target containing 38-70 wt. % W, 25-50 wt. % Ni, 5-22 wt. % X, and the maximum proportion of unavoidable impurities is ≤ 650 μg / g. In this case, the method according to the invention is used to ensure that the microstructure of the WNiX sputtering target has two phases, one of which is a pure W phase and the other is a mixed phase selected from NiWX, NiW, NiX and mixtures thereof (measured by XRD).

[0065] The method for producing a W-NiX sputtering target according to the invention makes it possible to ensure a relative density greater than 85% in the WNiX sputtering target produced by the method. In a particularly preferred embodiment of the invention, a relative density greater than 90% can be achieved.

[0066] By means of the method according to the invention for producing a WNiX sputtering target, the purity and the mechanical properties of the resulting target material are also optimized.

[0067] Therefore, the method of the present invention leads to a very low impurity content in the sputtering target prepared therefrom, for example, a preferred oxygen content of less than 350 μg / g, particularly preferably less than 100 μg / g, more preferably less than 75 μg / g, and even more preferably less than 30 μg / g.

[0068] In a preferred case, a sputtering target containing 38-70 wt. % W, 25-50 wt. % Ni, 5-22 wt. % X and unavoidable impurities is produced by means of the method according to the invention for producing a WNiX sputtering target. In this case, a hardness of less than 400 HV10 is preferably obtained by means of the method according to the invention after a compaction step, such as pressing and sintering.

[0069] In a preferred case, a sputtering target containing 38-70 wt % W, 25-50 wt % Ni, 5-22 wt % X and inevitable impurities is produced by means of the method for producing a WNiX sputtering target according to the present invention. In this case, by means of the method according to the present invention, the area ratio of the W phase measured on the cross section of the target material reaches 5%-50%.

[0070] In a preferred case, a sputtering target containing 38-70 wt. % W, 25-50 wt. % Ni, 5-22 wt. % X and unavoidable impurities is produced by means of the method according to the invention for producing a WNiX sputtering target. In this case, the average grain size of the W phase achieved by the method according to the invention is less than 40 μm, more preferably less than 30 μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] The accompanying drawings show:

[0072] Figure 1 is an X-ray diffraction pattern of a WNiMo sputtering target sample according to the present invention;

[0073] Figure 2 is an X-ray diffraction pattern of a WNiCr sputtering target sample according to the present invention;

[0074] Figure 3 is the microstructure (optical microscope) of the WNiMo sputtering target according to the present invention;

[0075] Figure 4 : is the microstructure (optical microscope) of the WNiCr sputtering target according to the present invention. DETAILED DESCRIPTION

[0076] The invention is explained below with the aid of production examples and the accompanying drawings.

[0077] Examples

[0078] Example 1 (Manufacture of WNiMo tube):

[0079] The particle size of the W metal powder was determined by Fisher's method to be 4 μm, the particle size of the Ni metal powder was determined by Fisher's method to be 4.2 μm, and the particle size of the Mo metal powder was determined by Fisher's method to be 4.6 μm. The powders were added to a closed container at a ratio of 42 wt% W, 47 wt% Ni and 11 wt% Mo, and mixed in an oscillator for 1 hour.

[0080] A steel mandrel with a diameter of 141 mm was placed in the middle of a rubber tube with a diameter of 300 mm and one end was closed. The powder mixture was introduced into the intermediate space between the steel core and the rubber wall, and the rubber tube was closed at the open end of the rubber tube by a rubber cap. The closed rubber tube was placed in a cold isostatic press and pressed at a pressure of 200 MPa to obtain a disc-shaped green body with a relative density of about 59% and an outer diameter of 242 mm.

[0081] The green body produced in this way was sintered in an indirect sintering furnace in a hydrogen atmosphere at a temperature of about 1250° C. The relative density after sintering was about 80%.

[0082] The hardness of the target material was 126 HV10. The oxygen content was measured to be 190 μg / g.

[0083] Figure 1 The X-ray diffraction pattern of this example is shown. In order to evaluate the diffraction pattern, JCPDS cards 00-004-0806 (W) (corresponding to W phase), 01-071-9764 (Mo1.08Ni2.92), 01-072-2652 (Ni0.85W0.15) (corresponding to mixed phase) are used. It can be clearly seen from the figure that there is no pure Ni phase (appearing at 2θ=44.5°) in the X-ray spectrum. The peak at 2θ=40.2° refers to the pure W phase.

[0084] Microstructure Figure 3 For optical microscopy images, samples such as tubes were cut into approximately 15x15x15mm 3, which is then placed in an embedding mold and filled with plastic granules. In the press, pressure and temperature are used to melt the granules; after cooling, the sample is embedded in the plastic. The surface to be examined is then polished with sandpaper from coarse to fine grit and finally with a diamond suspension. The sample is then directly ready for examination under an optical microscope. The W grains (dark grey) are located in a mixture of NiWMo (bright colours). The black colour shows the pores resulting from the manufacturing via a powder metallurgy route.

[0085] Example 2 (Manufacture of WNiCr plate):

[0086] Also in this case, W metal powder having a particle size of 4 μm determined by the Fisher method, Ni metal powder having a particle size of 4.2 μm determined by the Fisher method, and Cr metal powder (sieved to less than 45 μm) were used as raw materials. The powders were introduced into a closed container in a ratio of 67 wt % W, 26 wt % Ni and 7 wt % Cr and mixed in an oscillator for 1 hour.

[0087] The powder mixture was introduced into a flexible rubber tube which was closed at its open end by a rubber cap. The closed rubber tube was placed in a cold isostatic press and pressed at a pressure of 200 MPa to obtain a plate-like green body with a relative density of about 64.9%.

[0088] The green body thus prepared was sintered in an indirect sintering furnace in a hydrogen atmosphere at about 1400° C. for 4 hours. The relative density after sintering was about 90%. The plate had a size of 268×48.7×343 mm 3 The target material has an approximate size of 189 HV10 and an oxygen content of 50 μg / g.

[0089] Figure 2 The X-ray diffraction pattern of this example is shown. To evaluate the diffraction pattern, JCPDS cards 00-004-0806 (W), 03-065-5108 (Cr4Ni 15 W), 01-071-7594 (CrNi), 03-065-6291Cr2Ni3 and 01-077-3140 (Ni9W) 0.4. It can be clearly seen from the figure that there is no pure Ni phase (appearing at 2θ = 44.5°) in the X-ray spectrum. The peak at 2θ = 40.2° refers to the pure W phase.

[0090] Microstructure Figure 4 A sample of this plate was prepared as described in Example 1.

[0091] W grains (dark grey) are located in a mixture of NiWCr (light colour). Black shows the porosity resulting from the manufacturing via the powder metallurgy route.

Claims

1. A sputtering target manufactured by a powder metallurgy method, wherein the sputtering target comprises tungsten (W), nickel (Ni) and one other metal X selected from the group consisting of Group 5 or Group 6 of the periodic table, and inevitable impurities, wherein the sputtering target has a two-phase microstructure, wherein one phase is pure W and the other phase is a mixed phase selected from the group consisting of NiWX, NiW, NiX and a mixture thereof.

2. The sputtering target according to claim 1, wherein The other metal X is a metal selected from the elements Cr, Mo, Nb or Ta.

3. The sputtering target according to claim 1 or 2, wherein: The sputtering target comprises the following composition: 38-70 wt% W, 25-50 wt% Ni, 5-22 wt% X, and the maximum proportion of unavoidable impurities is ≤ 650 μg / g, so that the sum of W+Ni+X+impurities is 100 wt%.

4. The sputtering target according to any one of claims 1 to 3, wherein: The density of the sputtering target is at least 85%.

5. The sputtering target according to any one of claims 1 to 4, characterized in that: The oxygen content is less than 350μg / g.

6. The sputtering target according to claim 5, characterized in that The oxygen content is less than 100μg / g.

7. The sputtering target according to any one of claims 1 to 6, characterized in that: The sputtering target is a tubular sputtering target.

8. The sputtering target according to any one of claims 1 to 6, characterized in that: The sputtering target is a planar sputtering target.

9. The sputtering target according to any one of claims 1 to 8, characterized in that: The sputtering target has an area ratio of the W phase measured at a cross section of the target material of 5% to 50%.

10. The sputtering target according to any one of claims 1 to 9, characterized in that: The average grain size of the W phase of the sputtering target is less than 40 μm.

11. A method for manufacturing a WNiX sputtering target by a powder metallurgy process, characterized in that: The method comprises at least the following steps: - A compacting step in which a mixed powder of W powder, Ni powder and X powder is compacted by applying pressure, heat, or pressure and heat to obtain a blank.

12. The method for manufacturing a WNiX sputtering target according to claim 11, characterized in that: The compacting step is achieved by sintering at a temperature of 1100 to 1450°C.

13. The method for manufacturing a WNiX sputtering target according to claim 11 or 12, characterized in that: The method comprises a forming step after the pressing step.

14. The method according to claim 13, characterized in that Forming is done by rolling or forging.

15. The method according to claim 13 or 14, wherein: The forming step is followed by a heat treatment.

Citation Information

Patent Citations

  • Method for improving moisture and heat resistance of Cr-Si high resistance film resistor based on electro-catalytic property

    CN104485190A

  • W-Ni sputter target

    CN105849633A

  • Ni-W BASED SINTERED TARGET MATERIAL

    JP2009155722A