Preparation method and application of composite PdS self-supporting electrode material
By using composite PdS self-supporting electrode materials regulated by S element in electrocatalytic reactions, the problems of complex peracetic acid preparation process and high energy consumption in the prior art are solved, and efficient and stable peracetic acid generation is achieved, with a wide range of industrial application potential.
Patent Information
- Application Number
- CN202410931602.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The existing peracetic acid preparation process is complex and has high energy consumption, which limits its wide application in biopharmaceuticals, food processing, livestock and poultry breeding, and the stability and reaction selectivity of the catalyst are insufficient.
The composite PdS self-supporting electrode material is prepared by simple impregnation and calcination. Through the precise regulation of S element, the Pd active site is improved, and the efficient electrocatalytic synthesis of peracetic acid is achieved. PdS nanoparticles are used to catalyze the formation of peracetic acid in electrocatalytic reaction. .
It has achieved efficient and excellent stability of peracetic acid production, reduced production costs, simplified process flow, conformed to the concept of environmental protection and sustainable development, and has good industrial prospects.
Smart Images

Figure CN118996446A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrocatalytic material preparation, and specifically relates to a preparation method and application of a composite PdS self-supporting electrode material Background Art
[0002] As a strong oxidant, peracetic acid has strong oxidizing and bleaching effects, and plays an important role in the biopharmaceutical field, food processing industry, and livestock and poultry farming. Among them, in terms of disinfection performance, peracetic acid is known for its efficient bactericidal ability. It can quickly kill a variety of microorganisms such as bacterial propagules, mycobacteria, bacterial spores, fungi, algae and viruses, and its bactericidal effect is enhanced with the increase of concentration and the extension of action time. At the same time, peracetic acid also has good stability and can maintain its disinfection effect for a long time under certain conditions.
[0003] At present, the main preparation processes of peracetic acid are acetic acid oxidation and acetaldehyde oxidation, which are oxidized under the action of catalysts to generate peracetic acid. The reaction is usually carried out under reduced pressure and high temperature, and the catalyst is sulfuric acid or other inorganic acid and ion exchange resin, which is often limited by cumbersome process flow and high energy consumption cost, restricting its wider application and development.
[0004] In recent years, the rapid rise of electrocatalytic technology has become the focus of scientific research and industrial circles. Its green environmental protection, significant cost-effectiveness and high efficiency are remarkable. In the process of electrocatalytic technology, how to develop efficient and stable catalysts to optimize the production process of peracetic acid and improve reaction selectivity and yield has become a key problem to be solved. The present invention shows a preparation method and application of a composite PdS self-supporting electrode material. The catalyst precisely regulates the Pd active site through S doping, realizes efficient electrocatalytic synthesis of peracetic acid, and has important practical application value and market prospects. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation and application of a composite PdS self-supporting electrode material. A composite PdS self-supporting electrode material is synthesized by a simple impregnation and roasting method. The composite PdS self-supporting electrode material has the advantages of simple operation, easy repeatability, and efficient synthesis. The composite PdS self-supporting electrode material has excellent stability, durability and electrocatalytic performance, and has good industrial prospects in the application of electrocatalytic production of peracetic acid.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A method for preparing a composite PdS self-supporting electrode material comprises the following steps:
[0008] 1) Dispersing the Pd source and the S source in ethanol and homogenizing by ultrasonication;
[0009] 2) fully immersing the gas-repellent electrode support material in the solution dispersed by ultrasonication in step 1) for a single immersion time of 0.5-3 minutes, and then placing the electrode support material in an oven for drying to completely remove ethanol; repeating the immersion and drying steps 10-25 times, each time ensuring that the electrode support material is evenly immersed in the solution;
[0010] 3) placing the electrode support material treated in step 2) in a tube furnace and calcining it in an inert gas Ar atmosphere to form PdS nanoparticles on the electrode support material, and then cooling it to room temperature to obtain a composite PdS self-supporting electrode.
[0011] Furthermore, the palladium salt in step 1) is one of palladium chloride PdCl2, chloropalladic acid H2[PdCl6], potassium chloropalladate K2PdCl4 and sodium chloropalladate Na2PdCl4, the S source is one of thiourea, sodium sulfide and sulfur powder, and the dispersed concentration of the S source in the ultrasonically dispersed solution of step 1) is 3-7mmol / L, preferably 4-5mmol / L.
[0012] Furthermore, in step 1), the molar ratio of the Pd source to the S source is 0.3-1:1, preferably 0.7-1:1.
[0013] Furthermore, the self-supporting electrode material needs to be selected from electrodes with good stability, gas repellency and certain deformation resistance, such as carbon felt, titanium felt, nickel felt, foam copper, foam iron, etc., preferably carbon felt.
[0014] Furthermore, in step 3), the calcination temperature is 300-700° C., preferably 400-500° C., and the calcination time is 1-5 h, preferably 3 h.
[0015] The present invention also provides an application of the composite PdS self-supporting electrode material in electrocatalytic production of peracetic acid, wherein the composite PdS self-supporting electrode material is used as a cathode working electrode; the electrocatalytic reaction process is carried out in a gas diffusion flow cell, comprising an anode chamber and a cathode chamber, wherein the anode chamber and the cathode chamber are separated by a proton exchange membrane, the anode adopts a platinum mesh electrode, the cathode adopts the cathode working electrode, and the cathode divides the cathode chamber into two left and right chambers, the chamber close to the proton exchange membrane is recorded as a cathode liquid chamber, and the other chamber is a cathode air chamber, and the cathode working electrode is located between the cathode liquid chamber and the cathode air chamber; the anode and the cathode are respectively connected to a constant current meter through wires;
[0016] The anode electrolyte is an H2SO4 aqueous solution, acetic acid is used as a reaction substrate in the cathode liquid chamber, and the aqueous solution of the reaction substrate is used as the cathode electrolyte. Air or oxygen is introduced into the cathode air chamber, and a constant current instrument is energized to perform an electrocatalytic reaction. The air or oxygen diffuses to the surface of the cathode working electrode to contact the PdS nanoparticle catalyst component, and a reaction occurs at the cathode under the action of the catalyst to generate peracetic acid.
[0017] Furthermore, the concentration of the H2SO4 aqueous solution is 0.05-1 mol / L, preferably 0.5 mol / L.
[0018] Furthermore, the device for the electrocatalytic reaction also includes an anode liquid storage tank, a cathode liquid storage tank, a circulation pump 1 and a circulation pump 2. When the electrocatalytic reaction is carried out, the circulation pump 1 is started to allow the cathode electrolyte to circulate between the cathode liquid storage tank and the cathode liquid chamber; at the same time, the circulation pump 2 is started to allow the anode electrolyte to circulate between the anode chamber and the anode liquid storage tank.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] 1) The raw materials are easy to obtain, the cost is low, the electrocatalyst preparation steps are simple, and it is easy to prepare and scale up in batches;
[0021] 2) The electrocatalytically produced peracetic acid has a high concentration and good stability;
[0022] 3) The preparation method and application of the composite PdS self-supporting electrode material prepared by the above technology, PdS is loaded on the self-supporting material substrate by simple infiltration and calcination. The present invention uses S element doping to regulate the active sites of Pd, greatly enhancing its electrocatalytic production of peracetic acid concentration. Secondly, peracetic acid is produced by electrochemical means without excessive waste liquid, and its production process is more in line with the concept of environmental protection and sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the SEM image of the catalyst on the surface of the material in Example 2;
[0024] Figure 2 This is a cyclic performance diagram of the electrocatalyst material performance test of Example 2 of the present invention;
[0025] Figure 3 It is a schematic diagram of the explosion structure of a gas diffusion flow cell according to an application embodiment of the present invention. DETAILED DESCRIPTION
[0026] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0027] The model of the carbon felt used in the embodiment of the present invention is KFD 2.5T, and its porosity is 94%. Such rich porosity means that there can be sufficient gas-liquid contact, which is conducive to the reaction.
[0028] Example 1: Preparation of a composite PdS self-supporting electrode material comprising the following steps (molar ratio Pd:S=0.5:1)
[0029] 1) Add 0.05 mmol palladium chloride and 0.1 mmol thiourea to 20 mL ethanol, sonicate until uniformly distributed, and stir at room temperature for 15 min;
[0030] 2) 3×3cm 2 The carbon felt is immersed in the evenly dispersed solution in step 1), and then placed in an oven for drying to completely remove the ethanol; the immersion and drying steps are repeated 20 times, with a single immersion time of 1 minute, each time ensuring that all electrode materials are evenly immersed in the solution.
[0031] 3) placing the self-supporting electrode treated in step 2) in a tubular furnace, heating the temperature from room temperature to 400°C at a heating rate of 5°C / min in an inert gas Ar atmosphere, and then calcining at a constant temperature for 3 hours to form PdS nanoparticles. After the procedure is completed, the temperature is cooled to room temperature to obtain a self-supporting electrode with composite PdS.
[0032] Example 2: Preparation of a composite PdS self-supporting electrode material (molar ratio Pd:S=0.7:1)
[0033] The preparation steps of the electrode material in Example 2 are repeated in Example 1, with the only difference being that "the amount of palladium chloride in step 1) is replaced by 0.07 mmol", and other conditions remain unchanged, thereby obtaining a self-supporting electrode of composite PdS.
[0034] Example 3: Preparation of a composite PdS self-supporting electrode material (molar ratio Pd:S=1:1)
[0035] The preparation steps of the electrode material in Example 3 are repeated in Example 1, with the only difference being that "the amount of palladium chloride in step 1) is replaced by 0.1 mmol", and other conditions remain unchanged, thereby obtaining a self-supporting electrode of composite PdS.
[0036] Example 4: Preparation of a composite PdS self-supporting electrode material (molar ratio Pd:S=0.7:1)
[0037] The preparation steps of the electrode material of Example 4 are repeated in Example 2, with the only difference being that "in step 3), the calcination temperature is replaced from 400° C. to 300° C.", and other conditions remain unchanged, thereby obtaining a self-supporting electrode of composite PdS.
[0038] Example 5: Preparation of a composite PdS self-supporting electrode material (molar ratio Pd:S=0.7:1)
[0039] The preparation steps of the electrode material in Example 5 are repeated in Example 2, with the only difference being that the calcination temperature in "step 3) is replaced from 400°C to 500°C", and other conditions remain unchanged, thereby obtaining a self-supporting electrode of composite PdS.
[0040] Example 6: Preparation of a composite PdS self-supporting electrode material (molar ratio Pd:S=0.7:1)
[0041] The preparation steps of the electrode material of Example 6 are repeated in Example 2, with the only difference being that the calcination temperature in "step 3) is replaced from 400°C to 600°C", and other conditions remain unchanged, thereby obtaining a self-supporting electrode of composite PdS.
[0042] Example 7: Preparation of a composite PdS self-supporting electrode material (molar ratio Pd:S=0.7:1)
[0043] The preparation steps of the electrode material of Example 7 are repeated in Example 2, with the only difference being that the calcination temperature in "step 3) is replaced from 400°C to 700°C", and other conditions remain unchanged, thereby obtaining a self-supporting electrode of composite PdS.
[0044] Example 8: Preparation of a composite PdS self-supporting electrode material (molar ratio Pd:S=0.7:1)
[0045] The preparation steps of the electrode material of Example 8 are repeated in Example 2, with the only difference being that "in step 3), the calcination temperature is replaced from 400° C. to 800° C.", while other conditions remain unchanged, and a self-supporting electrode of composite PdS can be obtained.
[0046] Example 9: Preparation of a composite PdS self-supporting electrode material (molar ratio Pd:S=0.7:1)
[0047] The preparation steps of the electrode material of Example 9 are repeated in Example 2, with the only difference being that "in step 3), the calcination temperature is replaced from 400° C. to 900° C.", and other conditions remain unchanged, thereby obtaining a self-supporting electrode of composite PdS.
[0048] Comparative Example 1: Preparation of a composite PdS self-supporting electrode material comprising the following steps (molar ratio Pd:P=0.7:1)
[0049] 1) Dissolve 0.07 mmol palladium chloride and 0.1 mmol sodium hypophosphite in 20 mL ethanol mixed solution and sonicate until uniformly distributed, and stir at room temperature for 15 min.
[0050] 2) 3×3cm 2The carbon felt is immersed in the solution dispersed in step 1), and then placed in an oven for drying to completely remove the ethanol; the immersion and drying steps are repeated 20 times, with a single immersion time of 1 minute, each time ensuring that all electrode materials are evenly immersed in the solution.
[0051] 3) placing the self-supporting electrode treated in step 2) in a tubular furnace, heating the temperature from room temperature to 600°C at a heating rate of 5°C / min in an inert gas Ar atmosphere, and then calcining at a constant temperature for 3 hours to form PdP nanoparticles. After the procedure is completed, the temperature is cooled to room temperature to obtain a self-supporting electrode with composite PdP.
[0052] Comparative Example 2: Preparation of a composite PdS self-supporting electrode material comprises the following steps
[0053] 1) Dissolve 0.07 mmol palladium chloride and 0.1 mmol urea in 20 mL ethanol mixed solution and sonicate until uniformly distributed, then stir at room temperature for 15 min.
[0054] 2) 3×3cm 2 The carbon felt is immersed in the solution dispersed in step 1), and then placed in an oven for drying to completely remove the ethanol; the immersion and drying steps are repeated 20 times, with a single immersion time of 1 minute, each time ensuring that all electrode materials are evenly immersed in the solution.
[0055] 3) After the reaction is completed, the self-supporting electrode of step 2) is placed in a tubular furnace, and in an inert gas atmosphere, the temperature is increased from room temperature to 600°C at a heating rate of 5°C / min, and then calcined at a constant temperature for 3 hours to form PdN nanoparticles. After the program is completed, the temperature is cooled to room temperature to obtain a self-supporting electrode of composite PdN.
[0056] Comparative Example 3: Preparation of a composite PdSe self-supporting electrode material comprising the following steps (molar ratio Pd:Se=0.7:1)
[0057] 1) Disperse 0.07 mmol palladium chloride and 0.1 mmol Se powder in 20 mL ethanol mixed solution by ultrasonication until uniform distribution, and stir at room temperature for 15 min.
[0058] 2) 3×3cm 2 The carbon felt is immersed in the solution dispersed in step 1), and then placed in an oven for drying to completely remove the ethanol; the immersion and drying steps are repeated 20 times, with a single immersion time of 1 minute, each time ensuring that all electrode materials are evenly immersed in the solution.
[0059] 3) After the reaction is completed, the self-supporting electrode of step 2) is placed in a tubular furnace, and in an inert gas atmosphere, the temperature is increased from room temperature to 600°C at a heating rate of 5°C / min, and then calcined at a constant temperature for 3 hours to form PdSe nanoparticles. After the procedure is completed, the temperature is cooled to room temperature to obtain a self-supporting electrode of composite PdSe.
[0060] Application Example 1: Experimental steps for testing the performance of a composite PdS self-supporting electrode material in electrocatalytic production of peracetic acid:
[0061] 1) The prepared composite PdS self-supporting electrode material is assembled as a cathode working electrode in a gas diffusion flow cell for testing.
[0062] 2) Commercial 3×3cm 2 The platinum mesh was used as the anode electrode, the anode electrolyte was 1L 0.5mol / L H2SO4 aqueous solution, the cathode electrolyte was 1L 5mol / L CH3COOH aqueous solution, the air flow rate into the cathode gas collector 3 was 20mL / min, the cathode and anode electrodes were connected to the negative and positive poles of the constant current meter respectively, the electrocatalytic reaction was carried out at 180mA for 3h, and then the concentration of peracetic acid produced by the cathode electrolyte was detected.
[0063] The gas diffusion flow cell comprises an anode chamber and a cathode chamber, the anode chamber and the cathode chamber are separated by a proton exchange membrane, the anode adopts a platinum mesh electrode, the cathode adopts the cathode working electrode, and the cathode divides the cathode chamber into two left and right chambers, the chamber close to the proton exchange membrane is recorded as the cathode liquid chamber, and the other chamber is the cathode air chamber, and the cathode working electrode is located between the cathode liquid chamber and the cathode air chamber; the anode and the cathode are respectively connected to a constant current meter through wires.
[0064] The exploded structure diagram of the gas diffusion flow cell in this application is as follows Figure 3 As shown, the cathode and anode chambers are separated by a proton exchange membrane, including an end plate 1, a stainless steel conductive plate 2, a cathode gas collector 3, a cathode gas diffusion electrode 4, a cathode flow cell 5, a proton exchange membrane 6, an anode electrode 7, an anode flow cell 8 and an end plate 1, which are arranged from left to right. Fluororubber gaskets can be clamped between two adjacent module plates for sealing. All these modules can be assembled and fixed by bolts to form a stacked structure as a whole.
[0065] Among them, a hollow hole is arranged in the center of the anode electrode 7, an air inlet and an air outlet are arranged at both ends of the cathode gas collector 3, and a liquid inlet and an outlet are arranged at both ends of the cathode flow pool 5 and the anode flow pool 8, which are respectively connected to the cathode and anode liquid storage tanks through hoses to form a loop; a proton exchange membrane 6 is arranged between the cathode flow pool 5 and the anode flow pool 8, and its area is larger than the area of the hollow area in the center of the cathode and anode flow pools.
[0066] According to the test method of Application Example 1, the electrocatalysts prepared in Examples 1-9 and Comparative Examples 1-3 were tested respectively. The experimental results are shown in Table 1.
[0067] Table 1 Concentration of peracetic acid produced by different electrocatalyst tests
[0068] Catalyst Grouping Peracetic acid concentration (ppm) Example 1 1207 Example 2 1714 Example 3 1296 Example 4 1407 Example 5 1503 Example 6 1321 Example 7 1435 Example 8 1308 Example 9 1056 Comparative Example 1 118 Comparative Example 2 80 Comparative Example 3 640 Control 1: Carbon black 150 Comparison 2: Carbon nanotubes 136 Control 3: Pd / C catalyst 208
[0069] From the catalytic test results of the electrocatalysts of Examples 1-3 in Table 1, it can be seen that by changing the ratio of the Pd source to the S source to regulate the electronic effect of the S element on the Pd, the best effect of producing peracetic acid is achieved when the molar ratio is Pd:S=0.7:1. The SEM image of the catalyst on the surface of the material of Example 2 is as follows: Figure 1 As shown, it is obvious that particles are loaded on the surface of the carbon felt fiber and are in a uniformly dispersed state; this highly distributed PdS nanoparticle helps to adsorb the reactants and desorb the product peracetic acid in time, and the high concentration of peracetic acid comes from this. In addition, the Pd loading was tested by ICP-MS. The actual Pd loading in the electrocatalyst prepared in Example 2 was 0.373% (the Pd loading in the electrocatalyst prepared in Example 1 was 0.233%, and the Pd loading in the electrocatalyst prepared in Example 3 was 0.56%); Examples 4-9 explored the effect of stability on its catalytic activity during calcination, and the activity was best when calcined at 400°C; in order to further explore the electronic regulation effect of different anions on Pd, different anion precursors (P, N and Se sources) were used for doping in Comparative Examples 1-3, and the performance test results were all better than those of the S source, highlighting the unique electronic regulation effect of the S element on Pd.
[0070] In addition, commercial carbon black, carbon nanotubes or Pd / C catalyst (Pd loading 1%) were used as control catalysts, further demonstrating the excellent performance of the composite PdS self-supporting electrode material in the electrocatalytic production of peracetic acid.
[0071] The durability and stability of the catalyst are important factors in evaluating its industrial application. The electrocatalyst material of Example 2 was subjected to a cyclic application experiment. After each experiment, the electrocatalytic reaction was carried out at 180 mA for 3 hours, and then the cathode and anode electrolytes were replaced with fresh electrolytes, and then the next electrocatalyst application experiment was carried out. The cyclic application performance results of the electrocatalyst material performance test of Example 2 are shown in FIG. Figure 2 As shown, the composite PdS self-supporting electrode material was used for 50 cycles in the electrocatalytic production of peracetic acid, and its peracetic acid concentration did not show obvious attenuation, indicating its excellent durability and stability, and has certain industrial application and market potential for expansion.
Claims
1. A method for preparing a composite PdS self-supporting electrode material, characterized in that The following steps are involved: 1) Dispersing the Pd source and the S source in ethanol and homogenizing by ultrasonication; 2) fully immersing the gas-repellent electrode support material in the solution dispersed by ultrasonication in step 1) for a single immersion time of 0.5-3 minutes, and then placing the electrode support material in an oven for drying to completely remove ethanol; repeating the immersion and drying steps 10-25 times, each time ensuring that the electrode support material is evenly immersed in the solution; 3) placing the electrode support material treated in step 2) in a tube furnace and calcining it in an inert gas Ar atmosphere to form PdS nanoparticles on the electrode support material, and then cooling it to room temperature to obtain a composite PdS self-supporting electrode.
2. The method for preparing a composite PdS self-supporting electrode material according to claim 1, characterized in that The palladium salt in step 1) is one of palladium chloride PdCl2, chloropalladic acid H2[PdCl6], potassium chloropalladate K2PdCl4 and sodium chloropalladate Na2PdCl4, the S source is one of thiourea, sodium sulfide and sulfur powder, and the dispersion concentration of the S source in the ultrasonically dispersed solution of step 1) is 3-7mmol / L, preferably 4-5mmol / L.
3. The method for preparing a composite PdS self-supporting electrode material according to claim 1, characterized in that In step 1), the molar ratio of the Pd source to the S source is 0.3-1:1, preferably 0.7-1:
1.
4. The method for preparing a composite PdS self-supporting electrode material according to claim 1, characterized in that The self-supporting electrode substrate material used includes carbon felt, nickel felt, titanium felt, foamed copper or foamed iron, preferably carbon felt.
5. The method for preparing a composite PdS self-supporting electrode material according to claim 1, characterized in that In step 3), the calcination temperature is 300-700° C., preferably 400-500° C., and the calcination time is 1-5 h, preferably 3 h.
6. A composite PdS self-supporting electrode material prepared by the method according to any one of claims 1 to 5.
7. Use of the composite PdS self-supporting electrode material as claimed in claim 6 in electrocatalytic production of peracetic acid.
8. The use according to claim 7, characterized in that The composite PdS self-supporting electrode material is used as a cathode working electrode; the electrocatalytic reaction process is carried out in a gas diffusion flow cell, including an anode chamber and a cathode chamber, the anode chamber and the cathode chamber are separated by a proton exchange membrane, the anode uses a platinum mesh electrode, the cathode uses the cathode working electrode, and the cathode divides the cathode chamber into two left and right chambers, the chamber close to the proton exchange membrane is recorded as the cathode liquid chamber, and the other chamber is the cathode air chamber, and the cathode working electrode is located between the cathode liquid chamber and the cathode air chamber; the anode and the cathode are respectively connected to a constant current instrument through wires; The anode electrolyte is an H2SO4 aqueous solution, acetic acid is used as a reaction substrate in the cathode liquid chamber, and the aqueous solution of the reaction substrate is used as the cathode electrolyte. Air or oxygen is introduced into the cathode air chamber, and a constant current instrument is energized to perform an electrocatalytic reaction. The air or oxygen diffuses to the surface of the cathode working electrode to contact the PdS nanoparticle catalyst component, and a reaction occurs at the cathode under the action of the catalyst to generate peracetic acid.
9. The use according to claim 8, characterized in that The concentration of the H2SO4 aqueous solution is 0.05-1 mol / L, preferably 0.5 mol / L.
10. The use according to claim 8, characterized in that The device for the electrocatalytic reaction also includes an anode liquid storage tank, a cathode liquid storage tank, a circulation pump 1 and a circulation pump 2. When the electrocatalytic reaction is carried out, the circulation pump 1 is started to allow the cathode electrolyte to circulate between the cathode liquid storage tank and the cathode liquid cavity; at the same time, the circulation pump 2 is started to allow the anode electrolyte to circulate between the anode chamber and the anode liquid storage tank.
Citation Information
Patent Citations
Preparation method and application of novel photocatalytic semiconductor C2N3 and verification of degradation mechanism of coupled peracetic acid
CN118162185A
Process method for electro-catalysis in-situ oxidation synthesis of peracetic acid based on stacked electrolytic cell device
CN118292001A
Method for preparing palladium catalyst solution forelectroless plate process and method for activatingthe same
KR1020060083006A