High-efficiency FeOOH-coated NiOOH electrocatalyst with stable Fe site and preparation method and application of high-efficiency FeOOH-coated NiOOH electrocatalyst

The Ni-ferrohydroxide treatment is carried out through cyclic voltammetry and constant current polarization to form FeOOH@NiOOH electrocatalyst, which solves the problem of poor stability of NiFe-based catalysts under high currents, significantly improving the efficiency and stability of hydrogen production by electrolyzing water , promotes the industrial application of electrolytic water.

CN118996508APending Publication Date: 2024-11-22SHANGHAI UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411232934.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing NiFe-based catalysts are difficult to maintain stability under high currents, resulting in high cost of hydrogen production by electrolyzing water and unstable iron site kinetics, affecting the long-term stability of the catalyst.

Method used

The nickel ferrohydroxide is treated by cyclic voltammetry scanning and constant current polarization to form a FeOOH@NiOOH electrocatalyst, which strengthens the binding energy of the Fe site and the high-index crystal surface on the surface, and enhances the catalytic activity and stability of the OER.

Benefits of technology

The stability of the Fe site and OER catalytic performance under large currents have been improved, the cost of hydrogen production by electrolyzing water is reduced, and the industrial application of electrolyzing water is promoted.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996508A_ABST
    Figure CN118996508A_ABST
Patent Text Reader

Abstract

The invention provides a high-efficiency FeOOH-coated NiOOH electrocatalyst with a stable Fe site, and a preparation method and application thereof, and belongs to the technical field of hydrogen production by electrolyzing water with an electrocatalyst. The preparation method provided by the invention comprises the following steps: scanning ferro-nickel hydroxide through a cyclic voltammetry until a cyclic voltammetry curve is stable, and then applying constant current to the ferro-nickel hydroxide after the cyclic voltammetry curve is stable for polarization to obtain the FeOOH-coated NiOOH electrocatalyst. According to the method, eFNO is subjected to surface in-situ reconstruction through strong current polarization, a high-index crystal face is exposed, and adsorption of reaction intermediates in the OER process is enhanced. In addition, the synergistic effect between NiOOH and FeOOH plays a beneficial role in adjusting peripheral electron arrangement and reducing the energy barrier of OER.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen production by electrolysis of water using an electrocatalyst, and in particular to a high-efficiency FeOOH@NiOOH electrocatalyst with a stable Fe site, and a preparation method and application thereof. Background Art

[0002] Water electrolysis is a promising technology for obtaining high-purity hydrogen energy, providing a green alternative to traditional hydrogen production methods. However, the biggest problem facing water electrolysis for hydrogen production is the high cost of hydrogen production. Water electrolysis involves two reactions: the cathode hydrogen evolution reaction (HER) and the anode oxygen evolution reaction (OER). Since the OER process involves four electron transfers and the HER is a two-electron transfer process, OER is generally more difficult to occur than HER. Therefore, the development of OER electrocatalysts with low overpotential has become the key to reducing the cost of water electrolysis for hydrogen production.

[0003] Recent research has been extensively focused on NiFe-based catalysts, which have great potential in achieving excellent OER catalytic performance. These catalysts have appropriate peripheral electron arrangements and are able to effectively adsorb and desorb intermediates during the OER process, making them comparable to precious metal catalysts such as Ir and Rh. However, NiFe-based catalysts still face some challenges. Although they have successfully achieved relatively ideal overpotential values ​​at low currents, it is still difficult to reduce their overpotential at high currents. In addition, the iron sites are easily lost due to kinetic instability at high currents, thereby destroying the catalyst structure and making their catalytic stability poor. Therefore, maintaining long-term stability at high currents remains a major obstacle for NiFe-based catalysts, hindering their industrial application. Summary of the invention

[0004] Based on the above content, the purpose of the present invention is to provide an efficient FeOOH@NiOOH electrocatalyst with stable Fe sites and a preparation method and application thereof. The binding energy of Fe in the FeOOH@NiOOH electrocatalyst provided by the present invention is higher than that of unphased FeNiOOH (5eFNO), so the stability of the Fe site is better; at the same time, the catalyst surface has more high-index crystal faces and exhibits better OER catalytic activity.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] One of the technical solutions of the present invention is a method for preparing an efficient FeOOH@NiOOH electrocatalyst with stable Fe sites, comprising the following steps:

[0007] The nickel iron hydroxide was scanned by cyclic voltammetry until the cyclic voltammetry curve was stable, and then constant current polarization was applied to the nickel iron hydroxide after the cyclic voltammetry curve was stable to obtain the FeOOH@NiOOH electrocatalyst.

[0008] Preferably, the scanning rate of the cyclic voltammetry is 5 mV / s, and the scanning voltage is in the range of -0.1V-0.8V.

[0009] Preferably, the constant current polarization current is 1.5Acm -2 , the polarization time is 10h.

[0010] The second technical solution of the present invention is a highly efficient FeOOH@NiOOH electrocatalyst with stable Fe sites prepared by the above preparation method.

[0011] The third technical solution of the present invention is the use of the above-mentioned efficient FeOOH@NiOOH electrocatalyst with stable Fe sites in water electrolysis.

[0012] The present invention discloses the technical effects:

[0013] The present invention reconstructs the surface of eFNO in situ by strong current polarization, exposing high-index crystal planes, which is beneficial to enhance the adsorption of reaction intermediates during the OER process. In addition, the synergistic effect between NiOOH and FeOOH plays a beneficial role in regulating the peripheral electron arrangement and reducing the energy barrier of OER.

[0014] The binding energy of Fe in FeOOH after phase separation and reconstruction is much higher than that in non-phase-separated 5eFNO, which plays a role in reinforcing the iron catalytic active sites and ensures that the Fe sites are not easily lost during high-current electrolysis to achieve excellent electrolytic water stability.

[0015] eFNO provided by the present invention L It exhibits excellent OER catalytic performance and stability in high-current alkaline water electrolysis, which has a positive role in promoting the industrial application of hydrogen production by water electrolysis.

[0016] The present invention uses high current polarization to carry out Fe 2 O 3 The phase transition to FeOOH has a simple preparation method and is conducive to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 The eFNO of Example 1 L Schematic diagram of the preparation process.

[0019] Figure 2 The eFNO of Example 1 L and eFNO of Comparative Example 3 S Voltage-time diagram during the polarization reconstruction process.

[0020] Figure 3 The eFNO of Example 1 L and X-ray diffraction spectra of eFNO of comparative example 1 and 5eFNO of comparative example 2, wherein a is eFNO of comparative example 1 and 5eFNO of comparative example 2, and b is eFNO of embodiment 1 L .

[0021] Figure 4 The eFNO of Example 1 L TEM images a and b are area Ⅰ in Figure a, and c is area Ⅱ in Figure a.

[0022] Figure 5 The eFNO of Example 1 L , eFNO of Comparative Example 1, 5eFNO of Comparative Example 2, and eFNO of Comparative Example 3 S OER polarization curve.

[0023] Figure 6 The eFNO of Example 1 L And the stability test time-voltage diagram of eFNO of comparative example 1 and 5eFNO of comparative example 2.

[0024] Figure 7 The eFNO of Example 1 L Polarization curves of fully decomposed water before and after stability testing.

[0025] Figure 8 The eFNO of Example 1 L Figure a shows the change of Fe element in the electrolyte before and after the complete decomposition of water for eFNO of comparative example 1 and 5eFNO of comparative example 2, and figure b shows the change of element ratio in the material. DETAILED DESCRIPTION

[0026] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0027] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0028] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0029] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0030] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0031] The present invention provides a method for preparing an efficient FeOOH@NiOOH electrocatalyst with stable Fe sites, comprising the following steps:

[0032] The nickel iron hydroxide was scanned by cyclic voltammetry until the cyclic voltammetry curve was stable, and then a constant current polarization was applied to the nickel iron hydroxide after the cyclic voltammetry curve was stable to obtain the FeOOH@NiOOH electrocatalyst (denoted as eFNO L catalyst).

[0033] In some embodiments of the present invention, the scan rate of the cyclic voltammetry is 5 mV / s, and the scan voltage is in the range of -0.1V-0.8V.

[0034] In some embodiments of the present invention, the number of cyclic voltammetry scans is 5 times.

[0035] In some embodiments of the present invention, the constant current polarization current is 1.5Acm -2 , the polarization time is 10h.

[0036] In the present invention, the reasons why cyclic voltammetry and constant current polarization are set to the above parameter ranges are as follows:

[0037] The present invention first scans nickel iron hydroxide by cyclic voltammetry until the cyclic voltammetry curve is stable. When the number of scans is too many, time is wasted. When the number of scans is small, impurities and some unstable substances are difficult to remove completely. Therefore, the preferred number of scans is 5 times until the material is stable.

[0038] Scanning rate and scanning voltage outside the above range are likely to damage the material structure.

[0039] If the current of constant current polarization is further increased, the material structure will also be destroyed.

[0040] In some embodiments of the present invention, the method for preparing nickel iron hydroxide (eFNO) comprises the following steps:

[0041] Nickel foam (NF) was placed in a metal precursor solution and Fe 2 O 3 @Ni(OH) 2 Precursor (denoted as FNO precursor);

[0042] The Fe 2 O 3 @Ni(OH) 2 The precursor is etched in a sodium hydroxide solution to obtain the nickel iron hydroxide (eFNO).

[0043] In some embodiments of the present invention, before placing the nickel foam (NF) in the metal precursor solution, a process of pre-treating the nickel foam is also included; the pre-treatment is: ultrasonically cleaning the nickel foam with 3M hydrochloric acid, anhydrous ethanol, and water in sequence to remove surface impurities and oxide layers.

[0044] In some embodiments of the present invention, the metal precursor solution includes nickel, iron and urea; the molar ratio of the nickel, iron and urea is (0.6-0.7):(0.3-0.4):1, preferably 0.67:0.33:1; the nickel is Ni(NO 3 ) 2 6H 2 O is provided; the iron element is provided by Fe(NO 3 ) 3 9H 2 O provided.

[0045] The present invention successfully obtains phase-separated eFNOL by controlling the amount of urea, which provides a basis for the in-situ conversion of high-index crystal planes and the fixation of Fe sites in the later stage. In the present invention, if the molar ratio of nickel to iron exceeds the parameter range, the sheet structure of the product will collapse. If Ni(NO 3 ) 2 6H 2 O and Fe(NO 3 ) 3 9H 2 O is replaced by other nickel salts and iron salts, which will also cause the flaky structure of the product to disappear. Therefore, the molar ratio of the nickel salt, iron salt, and nickel element, iron element, and urea is preferably the above parameters.

[0046] In some embodiments of the present invention, the metal precursor solution is composed of Ni(NO in a molar volume ratio of 0.6-0.7mmol:0.3-0.4mmol:1mmol:30mL, preferably 0.67mmol:0.33mmol:1mmol:30mL. 3 ) 2 6H 2 O, Fe(NO 3 ) 3 9H 2 O, urea and water.

[0047] In some embodiments of the present invention, the reaction temperature of the one-pot hydrothermal method is 140° C. and the reaction time is 9 h.

[0048] In some embodiments of the present invention, after the one-pot hydrothermal reaction is completed, the steps of washing and drying the FNO precursor obtained by the reaction are also included; the washing is carried out using anhydrous ethanol; and the drying is carried out at 60° C. for 12 hours.

[0049] In some embodiments of the present invention, the concentration of the sodium hydroxide solution is 5 M; the etching temperature is 60° C. and the etching time is 3 h. The present invention converts part of the divalent metal into a trivalent metal by etching.

[0050] In some embodiments of the present invention, after the etching is completed, the steps of washing and drying the etching product in sequence are also included; the washing is carried out using anhydrous ethanol; and the drying is carried out by vacuum drying at 60° C. for 12 hours.

[0051] The principle of the present invention is as follows:

[0052] The present invention uses high current polarization to perform in-situ surface reconstruction of eFNO. High current polarization not only fixes the Fe site, but also promotes the 2 O 3It is converted into FeOOH with high-index crystal faces, thus forming an OER catalyst with excellent catalytic performance and good stability. It is worth noting that the binding energy of Fe in the phase-separated eFNOL is much higher than that of the non-phase-separated 5eFNOL, which ensures that the Fe sites are not easily lost during high-current electrolysis. In addition, high-current polarization exposes FeOOH with high-index crystal faces, which are more suitable for the adsorption of intermediates in the OER process, so that eFNOL has a high catalytic performance and good stability at 500mAcm -2 The overpotential is only 271.9 mV. This work highlights the importance of fixed iron sites during high current electrolysis and provides a new strategy for designing efficient and stable Ni-Fe-based catalysts.

[0053] The present invention also provides a high-efficiency FeOOH@NiOOH electrocatalyst with stable Fe sites prepared by the above preparation method.

[0054] The present invention also provides the use of the above-mentioned high-efficiency FeOOH@NiOOH electrocatalyst with stable Fe sites in water electrolysis.

[0055] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0056] Example 1

[0057] This embodiment provides a FeOOH@NiOOH electrocatalyst, and the preparation steps are as follows:

[0058] Step 1: First, a piece of nickel foam (NF, 3cm*3cm) was ultrasonically cleaned with 3M hydrochloric acid, anhydrous ethanol, and deionized water for 15 minutes to remove surface impurities and oxide layer.

[0059] Step 2: Place the NF obtained in step 1 in 30 ml of metal precursor solution (the metal precursor solution consists of Ni(NO 3 ) 2 6H 2 O (0.67 mmol), Fe (NO 3 ) 3 9H 2 O (0.33 mmol), CH 4 N 2 O (1 mmol) and 30 mL of water), and FNO was prepared by a one-pot hydrothermal method at 140 °C in a hydrothermal reactor for 9 h. The deep red FNO was then washed with anhydrous ethanol and dried in an oven at 60 °C for 12 h.

[0060] Step 3: The FNO obtained in step 2 was etched in a 5M NaOH solution at 60°C for 3 hours to convert part of the divalent metal into a trivalent state. After the etching was completed, the etched product was cleaned with anhydrous ethanol and then vacuum dried at 60°C for 12 hours to obtain eFNO.

[0061] Step 4: Use the eFNO obtained in step 3 as an anode to carry out a constant current polarization process to obtain eFNO L Cyclic voltammetry was performed five times to scan the curve until it was stable (scan rate was 5 mV / s in the range of -0.1 V to 0.8 V), and then 1.5 A cm -2 The FeOOH@NiOOH electrocatalyst was obtained by constant current polarization for 10 h and was denoted as eFNO L catalyst.

[0062] Comparative Example 1

[0063] This comparative example provides an eFNO catalyst, and the preparation steps are as follows:

[0064] Step 1: First, a piece of nickel foam (NF, 3cm*3cm) was ultrasonically cleaned with 3M hydrochloric acid, anhydrous ethanol, and deionized water for 15 minutes to remove surface impurities and oxide layer.

[0065] Step 2: Place the NF obtained in step 1 in 30 ml of metal precursor solution (the solution consists of Ni(NO 3 ) 2 6H 2 O (0.67 mmol), Fe (NO 3 ) 3 9H 2 O (0.33 mmol), CH 4 N 2 O (1 mmol) and 30 mL of water), and FNO was prepared by a one-pot hydrothermal method at 140 °C in a hydrothermal reactor for 9 h. The deep red FNO was then washed with anhydrous alcohol and dried in an oven at 60 °C for 12 h.

[0066] Step 3: The FNO obtained in step 2 was etched in 5M NaOH at 60°C for 3 hours. After the etching was completed, the etched product was washed with anhydrous ethanol and then vacuum dried at 60°C for 12 hours to obtain an eFNO catalyst. (Compared with Example 1, step 4 was omitted).

[0067] Comparative Example 2

[0068] This comparative example provides a 5eFNO catalyst, and the preparation steps are as follows:

[0069] Step 1: First, a piece of nickel foam (NF, 3cm*3cm) was ultrasonically cleaned with 3M hydrochloric acid, anhydrous ethanol, and deionized water for 15 minutes to remove surface impurities and oxide layer.

[0070] Step 2: Place the NF obtained in step 1 in 30 ml of metal precursor solution (the metal precursor solution consists of Ni(NO 3 ) 2 6H 2 O (0.67 mmol), Fe (NO 3 ) 3 9H 2 O (0.33 mmol), CH 4 N 2 O (5 mmol) and 30 mL of water), and FNO was prepared by a one-pot hydrothermal method at 140 °C in a hydrothermal reactor for 9 h. The deep red FNO was then washed with anhydrous ethanol and dried in an oven at 60 °C for 12 h.

[0071] Step 3: The FNO obtained in step 2 was etched in 5M NaOH at 60°C for 3 hours. After the etching was completed, the etched product was washed with anhydrous ethanol and then vacuum dried at 60°C for 12 hours to obtain a 5eFNO catalyst.

[0072] Comparative Example 3

[0073] This comparative example provides an eFNO S The catalyst is prepared as follows:

[0074] Step 1: First, a piece of nickel foam (NF, 3cm*3cm) was ultrasonically cleaned with 3M hydrochloric acid, anhydrous ethanol, and deionized water for 15 minutes to remove surface impurities and oxide layer.

[0075] Step 2: Place the NF obtained in step 1 in 30 ml of metal precursor solution (the metal precursor solution consists of Ni(NO 3 ) 2 6H 2 O (0.67 mmol), Fe (NO 3 ) 3 9H 2 O (0.33 mmol), CH 4 N 2 O (1 mmol) and 30 mL of water), and FNO was prepared by a one-pot hydrothermal method at 140 °C in a hydrothermal reactor for 9 h. The deep red FNO was then washed with anhydrous ethanol and dried in an oven at 60 °C for 12 h.

[0076] Step 3: The FNO obtained in step 2 was etched in 5M NaOH at 60°C for 3 hours to convert part of the divalent metal into a trivalent state. After the etching was completed, the etched product was cleaned with anhydrous ethanol and then vacuum dried at 60°C for 12 hours to obtain eFNO.

[0077] Step 4: Use the eFNO obtained in step 3 as an anode to carry out a small current polarization process to obtain eFNO L Cyclic voltammetry was performed five times to scan the curve until it was stable (scan rate was 5 mV / s in the range of -0.1 V to 0.8 V), and then 10 mA cm -2 eFNO was obtained by constant current polarization for 10 h. S Catalyst. (Compared with Example 1, the difference is that the current during constant current polarization is changed from 1.5Acm -2 Reduced to 10mAcm -2 ).

[0078] Figure 1 The preparation flow chart of Example 1 is as follows. The precursor is first obtained by a one-pot hydrothermal method and then alkali etching, and then 1.5Acm -2 eFNO was obtained by constant current polarization for 10 h. L catalyst.

[0079] Figure 2 The time-voltage diagram of the polarization reconstruction process of Example 1 and Comparative Example 3 (in the figure, eFNO L Example 1, eFNO s In Comparative Example 3), the voltage gradually decreases with the occurrence of surface reconstruction during high current polarization, while the voltage gradually increases with the loss of iron sites during low current polarization. Since the reconstruction rate of iron sites is greater than the loss rate of iron sites under high current, the iron sites are fixed.

[0080] Figure 3 Figure b is the XRD spectrum of Example 1, which confirms that its main substances are NiOOH and FeOOH, and the FeOOH shows more high-index crystal planes. Figure 3 a is the XRD spectrum of comparative example 1 and comparative example 2, and it can be confirmed that the main phase of comparative example 1 is Fe 2 O 3 and Ni(OH) 2 , the main phase of Comparative Example 2 is FeNiOOH.

[0081] Figure 4 a is the eFNO of Example 1 LTEM images, b and c are regions Ⅰ and Ⅱ in figure a, respectively. It can be observed that the surface of Example 1 is composed of phase-separated NiOOH and FeOOH, and FeOOH has more high-index crystal faces, which is beneficial to the improvement of catalytic activity and the fixation of Fe sites during OER catalysis.

[0082] Figure 5 The eFNO of Example 1 L and the eFNO of Comparative Example 1, the 5eFNO of Comparative Example 2, and the eFNO of Comparative Example 3 S OER polarization curves, where at 100 mA cm -2 Next, the eFNO of Example 1 L and the eFNO of Comparative Example 1, the 5eFNO of Comparative Example 2, and the eFNO of Comparative Example 3 S The OER overpotentials are 234mV, 281mV, 286mV, and 340mV respectively. -2 Next, the eFNO of Example 1 L , eFNO of Comparative Example 1, 5eFNO of Comparative Example 2, and eFNO of Comparative Example 3 S The OER overpotentials are 272 mV, 353 mV, 393 mV, and 523 mV, respectively. Compared with the comparative example, Example 1 having a high-index crystal face after high current polarization exhibits excellent catalytic performance.

[0083] Figure 6 The eFNO of Example 1 L The stability test time-voltage diagrams of eFNO of Comparative Example 1 and 5eFNO of Comparative Example 2 show that Example 1 exhibits excellent stability, while Comparative Examples 1 and 2 have poor stability due to the loss of iron sites under high current.

[0084] Figure 7 The eFNO of Example 1 L The polarization curve of water splitting before and after the stability test. After 100 hours of stability test, the attenuation of the polarization curve of water splitting is still small, indicating that after the large current polarization stabilizes the iron site, the eFNO of Example 1 L The stability has been greatly improved.

[0085] Figure 8 The eFNO of Example 1 L Figure a shows the change of Fe element in the electrolyte before and after the complete decomposition of water for eFNO of comparative example 1 and 5eFNO of comparative example 2, and figure b shows the change of element ratio in the material (in the figure, 5eFNO||Pt represents comparative example 2, eFNO L ||Pt represents Example 1, and eFNO||Pt represents Comparative Example 1). Figure a shows eFNO of Example 1. LThe iron content in the electrolyte is the lowest during the complete water splitting process, indicating that the Fe element in the catalyst is lost the least, and therefore the stability is the best. Figure b shows that the element ratio in the material before and after 100 hours of complete water splitting also corresponds to the result in Figure a, once again indicating that the improvement in stability is due to the fixation of the Fe sites.

[0086] In summary, at 25 °C in 1 M KOH, for 500 mA cm -2 ,eFNO L The overpotential for catalytic OER is 272 mV. In addition, when 500 mA cm -2 The overpotential obtained when the water is completely split is 1.68 V. Due to the strengthening of the iron site, the material shows excellent stability. -2 After 100 hours of water electrolysis with two electrodes in 1M KOH, the performance was still maintained at 98.5%. The present invention emphasizes the important role of the relative stability of the iron sites in nickel-iron-based catalysts during water electrolysis. By reinforcing the iron sites, the stability can be significantly enhanced, thus providing a promising method for the precise design of efficient and stable electrocatalyst materials.

[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an efficient FeOOH@NiOOH electrocatalyst with stable Fe sites, characterized in that: The following steps are involved: The nickel iron hydroxide was scanned by cyclic voltammetry until the cyclic voltammetry curve was stable, and then constant current polarization was applied to the nickel iron hydroxide after the cyclic voltammetry curve was stable to obtain the FeOOH@NiOOH electrocatalyst.

2. The method for preparing the efficient FeOOH@NiOOH electrocatalyst with stable Fe sites according to claim 1, characterized in that: The scanning rate of the cyclic voltammetry is 5 mV / s, and the scanning voltage is in the range of -0.1V-0.8V.

3. The method for preparing the efficient FeOOH@NiOOH electrocatalyst with stable Fe sites according to claim 1, characterized in that: The constant current polarization current is 1.5Acm -2 , the polarization time is 10h.

4. The method for preparing the efficient FeOOH@NiOOH electrocatalyst with stable Fe sites according to claim 1, characterized in that: The preparation method of the nickel-iron hydroxide comprises the following steps: The nickel foam was placed in a metal precursor solution and the Fe2O3@Ni(OH)2 precursor was prepared by a one-pot hydrothermal method. The Fe2O3@Ni(OH)2 precursor is etched in a sodium hydroxide solution to obtain the nickel-iron hydroxide.

5. The method for preparing the efficient FeOOH@NiOOH electrocatalyst with stable Fe sites according to claim 4, characterized in that: The metal precursor solution includes nickel, iron and urea; the molar ratio of the nickel, iron and urea is (0.6-0.7):(0.3-0.4):1; the nickel is provided by Ni(NO3)2·6H2O; and the iron is provided by Fe(NO3)3·9H2O.

6. The method for preparing the efficient FeOOH@NiOOH electrocatalyst with stable Fe sites according to claim 4, characterized in that: The reaction temperature of the one-pot hydrothermal method is 140° C. and the reaction time is 9 h.

7. The method for preparing the efficient FeOOH@NiOOH electrocatalyst with stable Fe sites according to claim 4, characterized in that: The concentration of the sodium hydroxide solution is 5M; the etching temperature is 60° C., and the etching time is 3 hours.

8. An efficient FeOOH@NiOOH electrocatalyst with stable Fe sites prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the efficient FeOOH@NiOOH electrocatalyst with stable Fe sites as claimed in claim 8 in water electrolysis.

Citation Information

Cited By

  • Dead-weight configuration oxygen evolution electrode, preparation method and application

    CN121472864A

  • Heterojunction catalyst with reconstructed surface as well as preparation method and application of heterojunction catalyst

    CN121896674A

  • A surface-reconstructed heterojunction catalyst and a preparation method and application thereof