A method for continuously producing water-soluble solid ammonium polyphosphate

By adopting continuous production methods and partition temperature control of a dual-shaft conveyor in ammonium polyphosphate production, a stable crystal structure is formed, and the ammonia volatility loss and high transportation cost in water-soluble solid ammonium polyphosphate production in the prior art is solved. Problem, efficient and stable production of water-soluble solid products has been achieved.

CN118771924BActive Publication Date: 2024-11-19SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411260694.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-19
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

In the prior art, the production of water-soluble solid ammonium polyphosphate mainly uses batch method, resulting in serious ammonia volatility loss and high transportation costs, and lacks excellent water-soluble solid products.

Method used

By using continuous production method, urea and monoammonium phosphate are heated to the molten state and then synergists are added. Through the partition temperature control and stirring process of the biaxial conveyor, a stable crystal structure is formed, which improves the water solubility and stability of ammonium polyphosphate. .

Benefits of technology

It realizes efficient production of water-soluble solid ammonium polyphosphate, improves its stability and water solubility, facilitates large-scale production, and reduces transportation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771924B_ABST
    Figure CN118771924B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for continuously producing water-soluble solid ammonium polyphosphate, which belongs to the technical field of compound fertilizers. When preparing solid ammonium polyphosphate, the present invention adds a synergist to the raw materials, which can introduce SO4 into the system. 2‑ Mg 2+ , K + , Ca 2+ , Fe 2+ Plasma, the presence of these ions can not only promote the formation of crystal nuclei, thereby improving the quality of solid products, but also change the surface charge and polarity of ammonium polyphosphate molecules, thereby improving its water solubility; the present invention divides the extrusion molding process into three different stages, and controls the temperature of the three stages to rise in sequence. Through the change of temperature, the synergistic ions can be evenly distributed in the ammonium polyphosphate crystals, further optimizing the product quality. The method for continuously producing water-soluble solid ammonium polyphosphate in the present invention is simple in process and is convenient for large-scale production of solid ammonium polyphosphate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of compound fertilizers, and in particular relates to a method for continuously producing water-soluble solid ammonium polyphosphate. Background Art

[0002] Ammonium polyphosphate (APP) is a polyphosphate containing nitrogen and phosphorus. It is a long-chain compound composed of -POP- chains. Its molecular formula is (NH 4 ) n+2 P n O 3n+1 , when n is large enough, it can be written as (NH 4 PO 3 ) n Type I or amorphous APP often has a lower degree of polymerization and exhibits good water solubility. It is often used as a high-concentration fertilizer containing nitrogen and phosphorus elements. APP products have the following advantages:

[0003] 1. The pH is neutral, which can improve soil agglomeration and compaction, and can also adjust the pH of the soil to maintain the pH within the ideal range required for crop growth;

[0004] 2. It has good water solubility and high solubility, and can be used to prepare high-concentration liquid fertilizer, and can also be used in water-fertilizer integrated agricultural facilities;

[0005] 3. It has a chelating effect on trace elements, and is not easily fixed and precipitated by soil iron, calcium and other ions, making phosphorus move longer in the soil and more easily reach the roots of crops, thus promoting the absorption and utilization of phosphorus and trace elements by crops;

[0006] 4. The polyphosphorus components contained in it are gradually hydrolyzed into orthophosphorus under the conditions of temperature, pH, enzymes and other factors before they can be absorbed and utilized by crops, and have a slow-release and long-lasting effect.

[0007] Since the 1960s, the United States has used 10-34-0 (NP 2 O 5 -K 2 The fully water-soluble NPK suspension fertilizer prepared with APP containing 10-11-0 (0.04-0) or 11-37-0 as the basic liquid fertilizer has been widely used in agricultural fertilization. However, there are few reports on the research and products of low-molecular-weight water-soluble solid APP.

[0008] There is a long history of research and utilization of water-soluble APP abroad. It mainly uses hot or wet phosphoric acid concentration to prepare superphosphoric acid, and then uses a tubular reactor to prepare 10-34-0 or 11-37-0 liquid fertilizer products. This tubular reactor method for preparing water-soluble APP is mostly continuous, but it has high quality requirements for phosphoric acid and the transportation cost of liquid products is also high. In China, wet phosphoric acid is mostly used to purify and remove impurities to prepare industrial monoammonium phosphate, and then industrial monoammonium phosphate and urea are used as raw materials to prepare solid products of specifications such as 18-58-0 and 23-46-0. In addition, there is a method for preparing APP by phosphoric acid-urea condensation (CN105621381A) and a method for preparing solid APP by phosphoric acid ammoniation (CN108002357A). However, these domestic methods for preparing APP all use intermittent production. Patent CN107176597A discloses a continuous production method for powdery water-soluble ammonium polyphosphate. A large amount of ammonia is volatilized and lost in the continuous conveyor belt polymerizer, and excess urea is required to ensure solidification. Summary of the invention

[0009] In view of the above-mentioned prior art, the present invention provides a method for continuously producing water-soluble solid ammonium polyphosphate to obtain a solid ammonium polyphosphate which is easy to store and transport and has excellent water solubility.

[0010] In order to achieve the above object, the technical solution adopted by the present invention is to provide a method for continuously producing water-soluble solid ammonium polyphosphate, comprising the following steps:

[0011] S1: heating urea and monoammonium phosphate to a molten state respectively, mixing the molten urea and monoammonium phosphate, adding a synergist to the mixture, stirring at 140-280° C. for 10-300 min, to obtain a reaction solution; the mass ratio of the molten monoammonium phosphate to the molten urea is 1:0.1-0.4; the synergist is at least one of magnesium salt, potassium salt, calcium salt, sulfate and iron salt;

[0012] S2: Feed the reaction liquid and powdered urea into the double-axis conveyor from the feeding end of the double-axis conveyor. The double-axis conveyor is divided into a mixing section, a fusion section and a reaction section from the feeding end to the discharging end. The temperature of the mixing section is 70~130℃, the temperature of the fusion section is 150~190℃, and the temperature of the reaction section is 200~280℃. Adjust the speed of the double-axis conveyor to 5~300rpm, collect the materials at the discharging end, cool and crush them, and obtain the product.

[0013] Based on the above technical solution, the present invention can also be improved as follows.

[0014] Furthermore, the heating temperature of urea in S1 is 135-160°C; the heating temperature of monoammonium phosphate is 195-215°C.

[0015] Furthermore, the mass ratio of the molten monoammonium phosphate to the synergist is 2 to 20:1.

[0016] Further, the magnesium salt is MgSO 4 Crystals, potassium salt is KCl crystals, calcium salt is CaCl 2 Crystal, iron salt is Fe 2 (SO 4 ) 3 Crystal.

[0017] Furthermore, the mass ratio of powdered urea to molten monoammonium phosphate is 0.1-0.4:1.

[0018] Furthermore, the particle size of the powdered urea is 0.8 to 1.2 mm.

[0019] Furthermore, the mixing section is divided into four temperature zones, which are 70°C, 90°C, 110°C and 130°C respectively according to the material flow temperature; the fusion section is divided into three temperature zones, which are 150°C, 170°C and 190°C respectively according to the material flow temperature; the reaction section is divided into five temperature zones, which are 200°C, 220°C, 240°C, 260°C and 280°C respectively according to the material flow temperature.

[0020] Furthermore, the residence time of the material in the mixing section is 30s~100min; the residence time in the fusion section is 30s~100min; and the residence time in the reaction section is 30s~100min.

[0021] Furthermore, the pitch of the mixing section is 12-20 mm, the pitch of the fusion section is 12-16 mm, and the pitch of the reaction section is 12-16 mm.

[0022] The beneficial effects of the present invention are:

[0023] 1. In the present invention, a synergist is added to the initial reaction of urea and monoammonium phosphate to introduce Mg into the system. 2+ , K + , Ca 2+ , Fe 2+ Plasma, these ions can be adsorbed around phosphate ions to form a stable crystal nucleus structure, thus serving as the center of crystal nucleation, reducing the energy barrier required for nucleation, and thus accelerating the formation of crystals; and after the crystal nucleus is formed, these ions can also promote the growth of crystals in three-dimensional space, making the crystal structure of ammonium polyphosphate more complete and dense, thereby improving the stability of ammonium polyphosphate. In addition, these ions can coordinate with the phosphate ions in the ammonium polyphosphate molecules, thereby changing the surface charge and polarity of the ammonium polyphosphate molecules, that is, they can affect the dissolution equilibrium of ammonium polyphosphate through ionic effects, making it more soluble in water.

[0024] 2. The present invention divides the extrusion molding process into three different stages, and controls the temperature of the three stages to rise in sequence. Through the change of temperature, the synergistic ions can be evenly distributed in the ammonium polyphosphate crystals, which can not only optimize the internal structure of the crystals, thereby improving the crystal quality, but also allow more synergistic ions to participate in the dissolution process, thereby improving the water solubility of ammonium polyphosphate.

[0025] 3. The method for continuously producing water-soluble solid ammonium polyphosphate in the present invention has a simple process and is convenient for large-scale production of solid ammonium polyphosphate. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a structural schematic diagram of a double-axis conveyor;

[0027] Figure 2 The polymerization degree distribution diagram of five kinds of ammonium polyphosphate obtained in Example 1;

[0028] Among them, 1. Mixing section; 2. Fusion section; 3. Reaction section; 4. First section; 5. Second section; 6. Third section; 7. Fourth section; 8. Fifth section. DETAILED DESCRIPTION

[0029] The focus of the present invention is on the process steps of ammonium polyphosphate production and the control of process parameters in the steps, and the double-axis conveyor is only a conventional production tool used to achieve the process purpose of the present invention. The double-axis conveyor in the present invention is essentially a twin-screw extruder, and the design of twin-screw extruders in the prior art is very mature (such as the SHJ series twin-screw extruders produced by Nanjing Shengchi Rubber and Plastic Machinery Manufacturing Co., Ltd.); based on this, the applicant of the present invention combined with the production process and commissioned Zhonglan Chenguang Chemical Research and Design Institute Co., Ltd. to redesign the conventional twin-screw extruder. The main structure is the same as the existing twin-screw extruder, and only the temperature partition and the screw pitch are adjusted to enable it to meet the production requirements of water-soluble solid ammonium polyphosphate, as shown in the specific embodiments.

[0030] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0031] Example 1

[0032] A method for continuously producing water-soluble solid ammonium polyphosphate comprises the following steps:

[0033] S1: Heat urea to a molten state at 160°C, and heat industrial-grade monoammonium phosphate to a molten state at 200°C; then mix the molten urea and the molten monoammonium phosphate according to the mass ratio in Table 1, and then add CaCl 2 Crystals, added CaCl 2The mass ratio of the crystal to the molten monoammonium phosphate is 0.1:1; then stirring at 220° C. for 45 minutes to obtain a reaction solution;

[0034] S2: Feed the reaction liquid and powdered urea with a particle size of about 1 mm into the double-axis conveyor from the feeding end of the double-axis conveyor. The structural diagram of the double-axis conveyor is shown in Figure 1 As shown, the double-axis conveyor is divided into a mixing section 1, a fusion section 2 and a reaction section 3 from the feed end to the discharge end, wherein the mixing section 1 is divided into four temperature zones, which are 70°C, 90°C, 110°C and 130°C in order according to the material flow temperature, the fusion section 2 is divided into three temperature zones, which are 150°C, 170°C and 190°C in order according to the material flow temperature, and the reaction section 3 is divided into five temperature zones, which are 200°C, 220°C, 240°C, 260°C and 280°C in order according to the material flow temperature; the screw of the double-axis conveyor is divided into a first section 4, a second section 5, a third section 6, a fourth section 7 and a fifth section 8, wherein the first section 4 is located in the mixing section 1, and its pitch is 20mm, and the second section 5 spans the mixing section 1 and the fusion section 2 (the portion located in the fusion section 2 accounts for 1 / 5 of the total length of the second section 5) , its pitch is 16mm, the third section 6 spans the fusion section 2 and the reaction section 3 (the part located in the reaction section 3 accounts for 1 / 3 of the total length of the third section 6), and its pitch is 12mm, the fourth section 7 and the fifth section 8 are located in the reaction section 3, and the pitches are 16mm and 12mm respectively; the proportioning relationship between powdered urea and the reaction liquid is shown in Table 1 (the mass ratio of powdered urea to molten monoammonium phosphate), the speed of the double-axis conveyor screw is adjusted to 10rpm, and the residence time of the mixed material in the mixing section 1 is controlled to be 5min; the residence time in the fusion section 2 is 10min; the residence time in the reaction section 3 is 30min; then the material is collected at the discharge end, air-cooled to room temperature, and crushed into particles with a particle size of about 2mm to obtain water-soluble solid ammonium polyphosphate.

[0035] Table 1 Ingredients relationship

[0036]

[0037] The degree of polymerization of the obtained water-soluble solid ammonium polyphosphate was analyzed, and the results were as follows: Figure 2 As shown in the figure, Pn represents n-polyammonium phosphate, such as P1 is orthophosphate, and P3 is tripolyammonium phosphate. It can be seen from the figure that the obtained water-soluble solid ammonium polyphosphate can achieve a relatively wide distribution of polymerization degree (the product with serial number C has a peak of hexapolyammonium phosphate, indicating that the highest degree of polymerization can reach hexapolyphosphate).

[0038] In addition, the polymerization rate, solubility, phosphorus content, nitrogen content, etc. of the obtained water-soluble solid ammonium polyphosphate were measured. The results are shown in Table 2.

[0039] Table 2 Characteristics of different water-soluble solid ammonium polyphosphates

[0040]

[0041] As can be seen from Table 2, if powdered urea (ammonium polyphosphate with serial number A) is not added during the extrusion molding stage, the resulting product not only cannot be cured well, but also shows low solubility and low nitrogen content. However, when urea is added in equal amounts at the front and rear ends (ammonium polyphosphate with serial number C), the degree of curing, polymerization rate, degree of polymerization distribution and solubility all reach a better level.

[0042] Example 2

[0043] A method for continuously producing water-soluble solid ammonium polyphosphate comprises the following steps:

[0044] S1: Heat urea to a molten state at 135°C, and heat industrial-grade monoammonium phosphate to a molten state at 195°C; then mix the molten urea and the molten monoammonium phosphate in a mass ratio of 1:0.18, and then add MgSO 4 Crystals, the added MgSO 4 The mass ratio of the crystal to the molten monoammonium phosphate is 0.2:1; then stirring at 200° C. for 60 minutes to obtain a reaction solution;

[0045] S2: Feed the reaction liquid and powdered urea with a particle size of about 1 mm into the double-axis conveyor from the feeding end of the double-axis conveyor. The structural diagram of the double-axis conveyor is shown in Figure 1As shown, the double-axis conveyor is divided into a mixing section 1, a fusion section 2 and a reaction section 3 from the feed end to the discharge end, wherein the mixing section 1 is divided into four temperature zones, which are 70°C, 90°C, 110°C and 130°C in order according to the material flow temperature, the fusion section 2 is divided into three temperature zones, which are 150°C, 170°C and 190°C in order according to the material flow temperature, and the reaction section 3 is divided into five temperature zones, which are 200°C, 220°C, 240°C, 260°C and 280°C in order according to the material flow temperature; the screw of the double-axis conveyor is divided into a first section 4, a second section 5, a third section 6, a fourth section 7 and a fifth section 8, wherein the first section 4 is located in the mixing section 1, and its pitch is 20 mm, the second section 5 spans the mixing section 1 and the fusion section 2 (the portion located in the fusion section 2 accounts for 1% of the total length of the second section 5). / 5), the pitch of which is 16mm, the third section 6 spans the fusion section 2 and the reaction section 3, the pitch of which is 12mm, the fourth section 7 and the fifth section 8 are located in the reaction section 3 (the part located in the reaction section 3 accounts for 1 / 3 of the total length of the third section 6), and the pitches are 16mm and 12mm respectively; the mass ratio of powdered urea to reaction liquid is 0.18:1 calculated based on the powdered urea and the original monoammonium phosphate, the speed of the screw of the double-axis conveyor is adjusted to 10rpm, and the residence time of the mixed material in the mixing section 1 is controlled to be 5min; the residence time in the fusion section 2 is 10min; the residence time in the reaction section 3 is 30min; then the material is collected at the discharge end, air-cooled to room temperature, and crushed into particles with a particle size of about 2mm to obtain water-soluble solid ammonium polyphosphate.

[0046] Example 3

[0047] A method for continuously producing water-soluble solid ammonium polyphosphate comprises the following steps:

[0048] S1: Heat urea to a molten state at 160°C, and heat industrial-grade monoammonium phosphate to a molten state at 215°C; then mix the molten urea and the molten monoammonium phosphate in a mass ratio of 1:0.18, and then add Fe 2 (SO 4 ) 3 Crystals, the added Fe 2 (SO 4 ) 3 The mass ratio of the crystal to the molten monoammonium phosphate is 0.05:1; then stirring at 280° C. for 10 minutes to obtain a reaction solution;

[0049] S2: Feed the reaction liquid and powdered urea with a particle size of about 1 mm into the double-axis conveyor from the feeding end of the double-axis conveyor. The structural diagram of the double-axis conveyor is shown in Figure 1As shown, the double-axis conveyor is divided into a mixing section 1, a fusion section 2 and a reaction section 3 from the feed end to the discharge end, wherein the mixing section 1 is divided into four temperature zones, which are 70°C, 90°C, 110°C and 130°C in order according to the material flow temperature, the fusion section 2 is divided into three temperature zones, which are 150°C, 170°C and 190°C in order according to the material flow temperature, and the reaction section 3 is divided into five temperature zones, which are 200°C, 220°C, 240°C, 260°C and 280°C in order according to the material flow temperature; the screw of the double-axis conveyor is divided into a first section 4, a second section 5, a third section 6, a fourth section 7 and a fifth section 8, wherein the first section 4 is located in the mixing section 1, and its pitch is 20mm, the second section 5 spans the mixing section 1 and the fusion section 2 (the portion located in the fusion section 2 accounts for 1 / 2 of the total length of the second section 5 5), the pitch is 16mm, the third section 6 spans the fusion section 2 and the reaction section 3 (the part located in the reaction section 3 accounts for 1 / 3 of the total length of the third section 6), and the pitch is 12mm, the fourth section 7 and the fifth section 8 are located in the reaction section 3, and the pitches are 16mm and 12mm respectively; the mass ratio of powdered urea to reaction liquid is 0.18:1 calculated based on the powdered urea and the original monoammonium phosphate, the speed of the screw of the double-axis conveyor is adjusted to 200rpm, and the residence time of the mixed material in the mixing section 1 is controlled to be 5min; the residence time in the fusion section 2 is 10min; the residence time in the reaction section 3 is 30min; then the material is collected at the discharge end, air-cooled to room temperature, and crushed into particles with a particle size of about 2mm to obtain water-soluble solid ammonium polyphosphate.

[0050] Comparative Example 1

[0051] A method for continuously producing water-soluble solid ammonium polyphosphate comprises the following steps:

[0052] S1: heating urea to a molten state at 160° C., and heating industrial-grade monoammonium phosphate to a molten state at 200° C.; then mixing the molten urea and the molten monoammonium phosphate in a mass ratio of 1:0.18; and then stirring at 220° C. for 45 minutes to obtain a reaction solution;

[0053] S2: Feed the reaction liquid and powdered urea with a particle size of about 1 mm into the double-axis conveyor from the feeding end of the double-axis conveyor. The structural diagram of the double-axis conveyor is shown in Figure 1As shown, the double-axis conveyor is divided into a mixing section 1, a fusion section 2 and a reaction section 3 from the feed end to the discharge end, wherein the mixing section 1 is divided into four temperature zones, which are 70°C, 90°C, 110°C and 130°C in order according to the material flow temperature, the fusion section 2 is divided into three temperature zones, which are 150°C, 170°C and 190°C in order according to the material flow temperature, and the reaction section 3 is divided into five temperature zones, which are 200°C, 220°C, 240°C, 260°C and 280°C in order according to the material flow temperature; the screw of the double-axis conveyor is divided into a first section 4, a second section 5, a third section 6, a fourth section 7 and a fifth section 8, wherein the first section 4 is located in the mixing section 1, and its pitch is 20 mm, the second section 5 spans the mixing section 1 and the fusion section 2 (the portion located in the fusion section 2 accounts for 1% of the total length of the second section 5). / 5), the pitch of which is 16mm, the third section 6 spans the fusion section 2 and the reaction section 3 (the portion located in the reaction section 3 accounts for 1 / 3 of the total length of the third section 6), and the pitch of which is 12mm, the fourth section 7 and the fifth section 8 are located in the reaction section 3, and the pitches are 16mm and 12mm respectively; the mass ratio of powdered urea to reaction liquid is 0.18:1 calculated based on the powdered urea and the original monoammonium phosphate, the speed of the screw of the double-axis conveyor is adjusted to 10rpm, and the residence time of the mixed material in the mixing section 1 is controlled to be 5min; the residence time in the fusion section 2 is 10min; the residence time in the reaction section 3 is 30min; then the material is collected at the discharge end, air-cooled to room temperature, and crushed into particles with a particle size of about 2mm to obtain water-soluble solid ammonium polyphosphate.

[0054] Comparative Example 2

[0055] A method for continuously producing water-soluble solid ammonium polyphosphate comprises the following steps:

[0056] S1: Heat urea to a molten state at 160°C, and heat industrial-grade monoammonium phosphate to a molten state at 200°C; then mix the molten urea and the molten monoammonium phosphate in a mass ratio of 1:0.18, and then add CaCl 2 Crystals, added CaCl 2 The mass ratio of the crystal to the molten monoammonium phosphate is 0.1:1; then stirring at 220° C. for 45 minutes to obtain a reaction solution;

[0057] S2: Feed the reaction liquid and powdered urea with a particle size of about 1 mm into the double-axis conveyor from the feeding end of the double-axis conveyor. The structural diagram of the double-axis conveyor is shown in Figure 1As shown, the double-axis conveyor is divided into a mixing section 1, a fusion section 2 and a reaction section 3 from the feeding end to the discharging end, wherein the temperature of the mixing section 1 is 90°C, the temperature of the fusion section 2 is 170°C, and the temperature of the reaction section 3 is 220°C; the screw of the double-axis conveyor is divided into a first section 4, a second section 5, a third section 6, a fourth section 7 and a fifth section 8, wherein the first section 4 is located in the mixing section 1, and its pitch is 20mm, the second section 5 spans the mixing section 1 and the fusion section 2 (the portion located in the fusion section 2 accounts for 1 / 5 of the total length of the second section 5), and its pitch is 16mm, the third section 6 spans the fusion section 2 and the reaction section 3 (the portion located in the reaction section 3 accounts for 6 1 / 3 of the total length), the pitch of which is 12mm, the fourth section 7 and the fifth section 8 are located in the reaction section 3, and the pitches are 16mm and 12mm respectively; the mass ratio of powdered urea to reaction liquid is 0.18:1 calculated based on the powdered urea and the original monoammonium phosphate, the speed of the screw of the double-axis conveyor is adjusted to 10rpm, the residence time of the mixed material in the mixing section 1 is controlled to be 5min; the residence time in the fusion section 2 is 10min; the residence time in the reaction section 3 is 30min; then the material is collected at the discharge end, air-cooled to room temperature, and crushed into particles with a particle size of about 2mm to obtain water-soluble solid ammonium polyphosphate.

[0058] Comparative Example 3

[0059] A method for continuously producing water-soluble solid ammonium polyphosphate comprises the following steps:

[0060] S1: Heat urea to a molten state at 160°C, and heat industrial-grade monoammonium phosphate to a molten state at 200°C; then mix the molten urea and the molten monoammonium phosphate in a mass ratio of 1:0.18, and then add CaCl 2 Crystals, added CaCl 2 The mass ratio of the crystal to the molten monoammonium phosphate is 0.1:1; then stirring at 220° C. for 45 minutes to obtain a reaction solution;

[0061] S2: Feed the reaction liquid and powdered urea with a particle size of about 1 mm into the double-axis conveyor from the feeding end of the double-axis conveyor. The structural diagram of the double-axis conveyor is shown in Figure 1As shown, the double-axis conveyor is divided into a mixing section 1, a fusion section 2 and a reaction section 3 from the feeding end to the discharging end, wherein the temperatures of the mixing section 1, the fusion section 2 and the reaction section 3 are all 220°C; the screw of the double-axis conveyor is divided into a first section 4, a second section 5, a third section 6, a fourth section 7 and a fifth section 8, wherein the first section 4 is located in the mixing section 1, and its pitch is 20 mm, the second section 5 spans the mixing section 1 and the fusion section 2 (the portion located in the fusion section 2 accounts for 1 / 5 of the total length of the second section 5), and its pitch is 16 mm, the third section 6 spans the fusion section 2 and the reaction section 3 (the portion located in the reaction section 3 accounts for 1 / 3 of the total length of the third section 6 ), the pitch of which is 12mm, the fourth section 7 and the fifth section 8 are located in the reaction section 3, and the pitches are 16mm and 12mm respectively; the mass ratio of powdered urea to reaction liquid is 0.18:1 calculated based on the powdered urea and the original monoammonium phosphate, the speed of the screw of the double-axis conveyor is adjusted to 10rpm, and the residence time of the mixed material in the mixing section 1 is controlled to be 5min; the residence time in the fusion section 2 is 10min; the residence time in the reaction section 3 is 30min; then the material is collected at the discharge end, air-cooled to room temperature, and crushed into particles with a particle size of about 2mm to obtain water-soluble solid ammonium polyphosphate.

[0062] The polymerization rate, solubility, phosphorus content, nitrogen content, etc. of the water-soluble solid ammonium polyphosphate obtained in Examples 2 to 3 and Comparative Examples 1 to 3 were measured. The results are shown in Table 3.

[0063] Table 3 Characteristics of different water-soluble solid ammonium polyphosphates

[0064]

[0065] It can be seen from Table 3 that the solid ammonium polyphosphate prepared by the process of the present invention (Examples 2-3) not only has a good polymerization rate, but also has a solubility of 155 g / 100 mL, and has excellent water solubility.

[0066] Compared with the ammonium polyphosphate with the serial number C in Example 1, the ammonium polyphosphate in Comparative Example 1 does not add the synergist CaCl during the preparation process. 2 During the formation of ammonium polyphosphate, the surface charge and polarity of the ammonium polyphosphate molecules cannot be effectively improved, which has an adverse effect on the dissolution equilibrium of ammonium polyphosphate, thereby deteriorating its water solubility.

[0067] Compared with the ammonium polyphosphate with serial number C in Example 1, the ammonium polyphosphate in Comparative Example 2 does not divide the mixing section 1, the fusion section 2 and the reaction section 3 into multiple temperature zones during the preparation process. Although the temperature is gradually rising, the temperature variation range is large, and the synergist cannot be evenly distributed in the ammonium polyphosphate crystals. The synergistic ions cannot effectively participate in the dissolution process, resulting in poor water solubility of the ammonium polyphosphate.

[0068] Compared with the ammonium polyphosphate with sequence number C in Example 1, the ammonium polyphosphate in Comparative Example 3 has the same temperature in the mixing section 1, the fusion section 2 and the reaction section 3 during the preparation process, and the temperature has been in a relatively high range, which is not conducive to the full mixing of the components, especially the synergist cannot be evenly distributed in the system, and the synergistic ions cannot effectively participate in the dissolution process, resulting in poor water solubility of the ammonium polyphosphate.

[0069] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for continuously producing water-soluble solid ammonium polyphosphate, characterized in that: The following steps are involved: S1: heating urea and monoammonium phosphate to a molten state respectively, mixing the molten urea and monoammonium phosphate, adding a synergist to the mixture, and stirring at 140-280° C. for 10-300 min to obtain a reaction solution; the mass ratio of the molten monoammonium phosphate to the molten urea is 1:0.1-0.4; the synergist is at least one of magnesium salt, potassium salt, calcium salt, sulfate and iron salt; S2: Feed the reaction liquid and powdered urea into the double-axis conveyor from the feed end of the double-axis conveyor. The double-axis conveyor is divided into a mixing section, a fusion section and a reaction section from the feed end to the discharge end. The mixing section is divided into four temperature zones, and the material flow temperatures are 70°C, 90°C, 110°C and 130°C respectively; the fusion section is divided into three temperature zones, and the material flow temperatures are 150°C, 170°C and 190°C respectively; the reaction section is divided into five temperature zones, and the material flow temperatures are 200°C, 220°C, 240°C, 260°C and 280°C respectively; adjust the speed of the double-axis conveyor to 5-300rpm, collect the material at the discharge end, cool and crush it, and obtain it.

2. The method for continuously producing water-soluble solid ammonium polyphosphate according to claim 1, characterized in that: The heating temperature of urea in S1 is 135~160℃; the heating temperature of monoammonium phosphate is 195~215℃.

3. The method for continuously producing water-soluble solid ammonium polyphosphate according to claim 1, characterized in that: The mass ratio of the molten monoammonium phosphate to the synergist is 2-20:

1.

4. The method for continuously producing water-soluble solid ammonium polyphosphate according to claim 1, characterized in that: The magnesium salt is MgSO4 crystal, the potassium salt is KCl crystal, the calcium salt is CaCl2 crystal, and the iron salt is Fe2(SO4)3 crystal.

5. The method for continuously producing water-soluble solid ammonium polyphosphate according to claim 1, characterized in that: The mass ratio of the powdered urea to the molten monoammonium phosphate is 0.1-0.4:

1.

6. The method for continuously producing water-soluble solid ammonium polyphosphate according to claim 1 or 5, characterized in that: The particle size of the powdered urea is 0.8-1.2 mm.

7. The method for continuously producing water-soluble solid ammonium polyphosphate according to claim 1, characterized in that: The material stays in the mixing section for 30s~100min; the material stays in the fusion section for 30s~100min; and the material stays in the reaction section for 30s~100min.

8. The method for continuously producing water-soluble solid ammonium polyphosphate according to claim 7, characterized in that: The pitch of the mixing section is 12-20 mm, the pitch of the fusion section is 12-16 mm, and the pitch of the reaction section is 12-16 mm.