Low-density irregular metal porous particle and preparation method thereof
By pretreatment of copper raw materials, detection and control of electrolyte, post-treatment, and pressing and sintering processes, the problems of cleanliness and morphology control in the preparation of porous metal particles were solved, and the preparation of high-quality, low-density, irregular porous metal particles was achieved, improving the stability and performance of the preparation process.
Patent Information
- Application Number
- CN202411108692.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
Existing technologies for preparing porous metal microparticles suffer from insufficient surface cleanliness and smoothness, and incomplete oxide removal, which affect the quality and performance of the preparation.
High-purity metallic copper is generated by mechanical pretreatment, pickling, ultrasonic cleaning, drying and oiling of copper raw materials, preparation and testing of electrolyte, electrolysis, and post-treatment such as rinsing, drying and grinding. Low-density irregular porous metal particles are prepared by combining pressing and sintering processes.
This ensured the cleanliness and smoothness of the raw material surface, controlled the morphology and structure of the particles, improved the uniformity and consistency of the particles, optimized the electrolysis efficiency, enhanced the stability and repeatability of the preparation process, and improved the performance and stability of the porous metal particles.
Smart Images

Figure CN118996543A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal porous particles, in particular to low-density irregular metal porous particles and a preparation method thereof. Background Art
[0002] The traditional preparation of metal porous particles has insufficient surface cleanliness and flatness, incomplete oxide removal, and may be deficient in deep cleaning and drying, which reduces the quality and performance of the metal porous particles. The preparation of metal porous particles in the present application can ensure the cleanliness and flatness of the raw material surface, remove oxides on the raw material surface, deeply clean and dry, and perform rust prevention protection, providing high-quality raw materials for the preparation of metal porous particles, thereby improving the performance and stability of the metal porous particles.
[0003] The defects of existing metal porous particle preparation are:
[0004] 1. Patent document JP6595808B2 discloses a magnesium metal fine particle and a method for preparing the magnesium metal fine particle. The document mainly considers how to inhibit the oxidation of the magnesium metal fine particle, but does not consider how to ensure the surface cleanliness and flatness of the raw material, remove the oxide on the surface of the raw material, deeply clean and dry it, and perform rust protection to provide high-quality raw materials for the preparation of metal porous particles, thereby improving the performance and stability of the metal porous particles;
[0005] 2. Patent document JP4293056B2 discloses a polymer metal particle. The document mainly considers how to provide a method for easily and cheaply producing materials, but does not consider how to solve the problems of controlling the morphology and structure of particles, regulating the density of particles, improving the uniformity and consistency of particles, and optimizing the electrolysis efficiency;
[0006] 3. Patent document JP5982156B2 discloses a metal microparticle dispersion. The document mainly considers how to obtain a low-resistance metal film with good adhesion to the glass substrate when the metal fine particle dispersion is coated on the surface of the glass substrate and fired, but does not consider how to provide a high-quality raw material basis for the subsequent preparation process, thereby indirectly solving the problem of raw material quality encountered in the preparation process;
[0007] 4. Patent document CN104550982B discloses a method for preparing ultrafine metal particles and the ultrafine metal particles prepared therefrom. The document mainly considers the problem of how to prevent the ultrafine metal particles from being exposed to air and oxidized during the preparation process, but does not consider how to solve the problems of controllability of porosity and structure, low density of particles, improvement of mechanical properties of particles, repeatability and stability of the process, and uniformity of pore distribution; Summary of the invention
[0008] The object of the present invention is to provide a low-density irregular metal porous particle and a preparation method thereof to solve the problems raised in the above background technology.
[0009] To achieve the above object, the present invention provides the following technical solution: a low-density irregular metal porous particle, and the preparation method of the irregular metal porous particle is as follows:
[0010] Step S1, pre-treating the copper raw material, the pre-treatment including mechanical pre-treatment, pickling, ultrasonic cleaning, drying and oil protection;
[0011] Step S2, preparing electrolyte;
[0012] Step S3, detecting electrolyte performance;
[0013] Step S4, electrolyzing to generate high-purity metallic copper;
[0014] Step S5, post-processing the high-purity metallic copper, the post-processing comprising washing, drying and grinding;
[0015] Step S6, preparing low-density irregular metal porous particles;
[0016] Step S7, measuring the porosity and compression performance of the porous metal particles;
[0017] In S1, the following steps are also included:
[0018] S11. Use a steel brush and a nylon brush to gently scrub the surface of the copper raw material, and use sandpapers of different roughness to polish it, starting from coarse sandpaper and gradually transitioning to fine sandpaper, to obtain a copper raw material with a smooth surface;
[0019] S12, using 0.2 mol / L dilute hydrochloric acid as a pickling agent, immersing the copper raw material in the pickling agent for 20 minutes for pickling, taking out the copper raw material after the pickling is completed, and washing the surface of the copper raw material with deionized water for 8 minutes;
[0020] S13, then put the copper raw material into an ultrasonic cleaning machine, add a cleaning solution for ultrasonic cleaning, put the cleaned copper raw material into a vacuum drying oven for drying, use a brush and a spray gun to evenly apply anti-rust oil on the surface of the copper raw material, and fully dry it to form a protective film.
[0021] Preferably, the cleaning solution is one of deionized water, acetone solution and ethanol solution.
[0022] Preferably, in S2, the following steps are also included:
[0023] S21. Slowly add copper sulfate powder into deionized water, stirring while adding until it is completely dissolved, add additives, adjust the pH value to 5.5-6.5, stir well, make the electrolyte to the fixed volume and filter.
[0024] Preferably, the additives include surfactants, corrosion inhibitors, grain refiners and electrolyte regulators.
[0025] Preferably, in S3, the following steps are also included:
[0026] S31, detecting the concentration, pH value and conductivity of the electrolyte, with a target concentration of 0.22-0.32 mol / L and a target conductivity of 50-200 S / m, and adjusting the electrolyte according to the test results;
[0027] S32. Adjusting the electrolyte includes adjusting the concentration, pH value and conductivity.
[0028] Preferably, the concentration adjustment includes increasing the concentration and decreasing the concentration, and the conductivity adjustment includes increasing the conductivity and decreasing the conductivity. If the detected concentration is lower than 0.22 mol / L or the conductivity is lower than 50 S / m, slowly add copper sulfate solution to the electrolyte. If the detected concentration is higher than 0.32 mol / L or the conductivity is higher than 200 S / m, add deionized water to dilute the electrolyte.
[0029] The pH adjustment includes increasing the pH and decreasing the pH. If the detected pH is lower than 5.5, sodium hydroxide is added to neutralize the acidic components in the electrolyte. If the detected pH is higher than 6.5, hydrochloric acid is added to lower the pH of the electrolyte.
[0030] Preferably, in S4, the following steps are also included:
[0031] S41, prepare an electrolytic cell, pour the electrolyte into the electrolytic cell, use the copper raw material as the anode, use a thin copper plate coated with wax as the cathode, turn on the power supply, and start electrolysis;
[0032] S42, monitoring and adjusting the parameters and electrolysis conditions of the electrolyte, wherein the parameters of the electrolyte include concentration, pH value and conductivity, and the electrolysis conditions include voltage, current and temperature;
[0033] S43. The cathode is taken out from the electrolytic cell, and the cathode is preheated to soften the wax layer. The wax layer is peeled off from the cathode surface using a scraper or gently to obtain high-purity metallic copper.
[0034] Preferably, in S5, the following steps are also included:
[0035] S51. Rinse the high-purity copper metal with deionized water and gently scrub the surface with a soft brush. Repeat the rinsing several times until the rinse liquid becomes clear.
[0036] S52, placing the cleaned high-purity metallic copper on a tray of a dryer for drying. After drying, turning off the power of the dryer, opening the dryer after cooling to room temperature, taking out the high-purity metallic copper, and grinding to obtain high-purity metallic copper powder with a purity greater than 99.9% and an average particle size of 80 μm.
[0037] Preferably, in S6, the following steps are also included:
[0038] S61. Using high-purity copper powder as the matrix material and soluble NaCl particles with an average particle size of 0.85 mm as the pore-forming agent, the high-purity copper powder and the soluble NaCl particles are uniformly mixed in different volume ratios, the volume proportions of the high-purity copper powder are 10%, 20%, 30% and 40% respectively, and the PILOTPRO pressure testing machine is used to press the green sheets at a pressure of 200 MPa, and the green sheets have a size of 20 mm×20 mm;
[0039] S62, put into TCXC1200T tubular muffle furnace, use argon as protective gas, raise the temperature to 600℃, 700℃, 800℃ and 900℃ at a heating rate of 10℃ / min, and the sintering time is 3h;
[0040] S63. After sintering is completed and cooled to room temperature, the upper and lower non-porous parts are removed and cut into 10mm×10mm. After being rinsed with deionized water at 70℃-80℃ for 30min, it is dried at 100℃ for 2h in a WGL-230B forced air drying oven to obtain low-density irregular metal porous particles.
[0041] Preferably, in S7, the following steps are also included:
[0042] S71. The density of the metal porous particles is measured by an XS225DU-Swiss Mettler-Toledo electronic density specific gravity analysis balance, and the porosity of the metal porous particles is calculated;
[0043] The calculation formula of porosity is: P = 1-(ρ measured - ρ actual);
[0044] Where: P is the porosity, ρmeasured is the measured density of the metal porous particles, and ρactual is the density of the non-porous metal copper;
[0045] S72, static compression test using a ZwickRoell static materials testing machine.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] 1. The present invention pre-treats the copper raw material, and the pre-treatment includes mechanical pre-treatment, pickling, ultrasonic cleaning, drying and oil protection. Through mechanical pre-treatment, the surface of the copper raw material is gradually polished using a steel brush, a nylon brush and sandpaper, which effectively removes dirt, oxides and uneven parts on the surface, making the surface of the copper raw material smooth, providing a basis for subsequent treatment. Pickling uses the corrosiveness of dilute hydrochloric acid to further remove oxides and other impurities on the surface of the copper raw material, ensuring the purity and activity of the copper raw material, which is conducive to promoting the electrolytic reaction. Ultrasonic cleaning uses the cavitation effect generated by high-frequency vibration waves in the cleaning liquid, which can penetrate into the tiny pores and cracks on the surface of the copper raw material, thoroughly remove residual dirt and impurities, and improve the cleanliness. The subsequent The vacuum drying treatment ensures that the copper raw material is subsequently processed in a completely water-free state, avoiding the influence of moisture on subsequent processes. A layer of rust-proof oil film is formed on the surface of the copper raw material, which effectively isolates air and moisture, prevents the copper raw material from oxidative corrosion when in contact with air, and extends the service life of the copper raw material. The pretreatment step provides high-quality copper raw materials for the subsequent preparation of metal porous particles. The smooth, clean and rust-proof surface of the copper raw material is conducive to the formation and uniform distribution of the porous structure. Therefore, it can solve the problem of how to ensure the cleanliness and flatness of the raw material surface, remove oxides on the raw material surface, deeply clean and dry, and perform rust-proof protection, thereby providing high-quality raw materials for the preparation of metal porous particles, thereby improving the performance and stability of metal porous particles.
[0048] 2. The present invention detects the performance of the electrolyte. The concentration, pH value and conductivity of the electrolyte directly affect the deposition rate and mode of copper ions during the electrolysis process, and further affect the morphology and structure of the final metal porous particles. By accurately adjusting these parameters, metal particles with irregular shapes and porous structures can be prepared. By adjusting the composition and conditions of the electrolyte, the density of the particles can be controlled to achieve the goal of low density. The stability and consistency of the electrolyte are crucial to the uniformity of the particles. By regularly detecting and adjusting the concentration, pH value and conductivity of the electrolyte, the stability of the electrolysis process can be ensured, thereby improving the uniformity and consistency of the particles. Suitable electrolyte conditions can significantly improve the electrolysis efficiency, reduce energy consumption and cost. By accurately controlling the parameters of the electrolyte, the electrolysis process can be optimized, and the yield and quality of the particles can be improved. Therefore, the problems of controlling the morphology and structure of the particles, regulating the density of the particles, improving the uniformity and consistency of the particles and optimizing the electrolysis efficiency can be solved.
[0049] 3. The present invention performs post-treatment on the high-purity metallic copper, and the post-treatment includes rinsing, drying and grinding. By using deionized water to rinse and gently scrub with a soft brush, impurities and pollutants on the surface of the high-purity metallic copper can be removed, the high purity and cleanliness of the raw materials can be ensured, the introduction of impurities can be avoided, and the quality of the porous metal particles can be improved. The grinding step processes the high-purity metallic copper into powder, and controls its average particle size to be 80 μm. Note the uniformity and consistency of the porous metal particles in the subsequent preparation process to avoid the degradation of the final morphology and performance due to inconsistent initial sizes. Rinsing, drying and grinding are pretreatment steps. High-quality raw materials are provided for the subsequent preparation of low-density irregular metal porous particles. These pretreatment steps help to ensure the stability and repeatability of the subsequent process, thereby improving the preparation efficiency and yield of the particles. By strictly controlling the purity, cleanliness and particle size of the raw materials, the controllability of the subsequent preparation process can be improved, which helps to reduce the uncertainty and variability in the preparation process, thereby obtaining more consistent and reliable low-density irregular metal porous particles. Therefore, it can provide a high-quality raw material basis for the subsequent preparation process, thereby indirectly solving the problem of raw material quality encountered in the preparation process.
[0050] 4. The present invention uses high-purity copper powder as a matrix material and soluble NaCl particles with an average particle size of 0.85 mm as a pore-forming agent to prepare low-density irregular metal porous particles, and measures the porosity and compression performance of the metal porous particles. By uniformly mixing high-purity copper powder and soluble NaCl particles and adopting a pressing and sintering process, it can ensure that the pores are evenly distributed inside the metal porous particles, which helps to avoid performance differences caused by excessively high or low local density. During the sintering process of the pressed green compact, an irregular pore structure is formed due to the dissolution and volatilization of NaCl particles. This irregular shape helps to increase the specific surface area of the particles and improve the performance of the metal porous particles in catalysis, adsorption and filtration. The performance of the surface is improved. At the same time, by using high-purity metallic copper powder and soluble NaCl particles in different volume ratios as pore-forming agents, the porosity of the final particles can be precisely controlled. The NaCl particles will dissolve and volatilize during the sintering process, leaving pores, thereby achieving controllable porosity. This controllability helps to adjust the physical and chemical properties of the particles. The method for preparing metal porous particles of the present application has clear steps and parameter settings, so that the preparation process has high repeatability and stability, which is helpful for large-scale production of metal porous particles with consistent performance. Therefore, the problems of controllability of porosity and structure, low density of particles, improvement of mechanical properties of particles, repeatability and stability of the process, and uniformity of pore distribution can be solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 It is the work flow chart of the present invention. DETAILED DESCRIPTION
[0052] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] Embodiment 1,
[0054] See also Figure 1 The present invention provides an embodiment: a low-density irregular metal porous particle, and the preparation method of the irregular metal porous particle is as follows:
[0055] Step S1, pre-treating the copper raw material, the pre-treatment including mechanical pre-treatment, pickling, ultrasonic cleaning, drying and oil protection;
[0056] In S1, the following steps are also included:
[0057] S11. Use a steel brush and a nylon brush to gently scrub the surface of the copper raw material, and use sandpapers of different roughness to polish it, starting from coarse sandpaper and gradually transitioning to fine sandpaper, to obtain a copper raw material with a smooth surface;
[0058] S12, using 0.2 mol / L dilute hydrochloric acid as a pickling agent, immersing the copper raw material in the pickling agent for 20 minutes for pickling, taking out the copper raw material after the pickling is completed, and washing the surface of the copper raw material with deionized water for 8 minutes;
[0059] S13, then put the copper raw material into an ultrasonic cleaning machine, add a cleaning solution for ultrasonic cleaning, put the cleaned copper raw material into a vacuum drying oven for drying, use a brush and a spray gun to evenly apply anti-rust oil on the surface of the copper raw material, and fully dry it to form a protective film.
[0060] The cleaning solution is one of deionized water, acetone solution and ethanol solution.
[0061] Further, a steel brush and a nylon brush are used to gently scrub the surface of the copper raw material. The two brushes are used to remove stubborn dirt and fine impurities respectively. The process starts with coarse sandpaper and gradually transitions to fine sandpaper. This process gradually refines the surface of the copper raw material and finally obtains a smooth and flawless surface. The smooth surface is conducive to the uniformity and effect of subsequent treatments.
[0062] 0.2 mol / L dilute hydrochloric acid was selected as the pickling agent. Dilute hydrochloric acid can effectively remove the oxide layer and slight corrosion on the copper surface without excessively corroding the copper matrix. The copper raw material was soaked in the pickling agent for 20 minutes to ensure sufficient reaction. After the pickling was completed, the surface of the copper raw material was rinsed with deionized water for 8 minutes to completely remove the residual acid and reaction products to prevent the subsequent treatment from being affected.
[0063] The copper raw material is placed in an ultrasonic cleaning machine, and a cleaning solution is added for ultrasonic cleaning. The high-frequency vibration of the ultrasonic wave can effectively remove the tiny particles and residues on the surface of the copper raw material, thereby improving the cleaning effect. The cleaned copper raw material is placed in a vacuum drying oven for drying to ensure that there is no moisture residue on the surface of the copper raw material to prevent rust.
[0064] Use a brush and a spray gun to evenly apply anti-rust oil on the surface of the copper raw material, and fully dry it to form a protective film. This protective film can isolate air and moisture to prevent the copper raw material from oxidation or corrosion during subsequent processing or storage. The above pretreatment can ensure that the surface of the copper raw material is clean, smooth and free of impurities, laying a good foundation for the subsequent preparation of irregular metal porous particles. At the same time, the oil protection step also effectively extends the service life and performance stability of the copper raw material.
[0065] Embodiment 2:
[0066] See also Figure 1 The present invention provides an embodiment: a low-density irregular metal porous particle, and the preparation method of the irregular metal porous particle is as follows:
[0067] Step S2, preparing electrolyte;
[0068] In S2, the following steps are also included:
[0069] S21. Slowly add copper sulfate powder into deionized water, stirring while adding until it is completely dissolved, add additives, adjust the pH value to 5.5-6.5, stir well, make the electrolyte to the fixed volume and filter.
[0070] Additives include surfactants, corrosion inhibitors, grain refiners and electrolyte regulators.
[0071] Further, the copper sulfate powder is slowly added to the deionized water, stirring while adding, and the process is slow to ensure that the copper sulfate can be fully dissolved to avoid agglomeration or precipitation caused by excessive local concentration. Stirring helps to accelerate the dissolution process and make the solution more uniform. After the copper sulfate is completely dissolved, an additive is added to the solution;
[0072] Surfactants can reduce the surface tension of the solution and help to form smaller bubbles or particles, thereby affecting the morphology of porous metal particles. Corrosion inhibitors can slow down the corrosion rate of the electrode during electrolysis and protect the electrode surface. They can also help control the generation rate and morphology of porous metal particles. Grain refiners can promote grain refinement and help to form smaller porous metal particles. Electrolyte regulators are used to adjust the conductivity and pH value of the electrolyte to ensure the smooth progress of the electrochemical process and adjust the pH value of the electrolyte to within the range of 5.5-6.5.
[0073] After adding all the ingredients, use a stirrer to stir the electrolyte thoroughly to ensure that all ingredients are evenly mixed and avoid local concentration differences. The electrolyte is diluted to the specified volume. The pH value of the electrolyte after dilution should be checked again. Finally, the electrolyte is filtered to remove possible impurities and undissolved particles. The filtered electrolyte should be clear and transparent without suspended matter or sediment.
[0074] Embodiment 3,
[0075] See also Figure 1 The present invention provides an embodiment: a low-density irregular metal porous particle, and the preparation method of the irregular metal porous particle is as follows:
[0076] Step S3, detecting electrolyte performance;
[0077] In S3, the following steps are also included:
[0078] S31, detecting the concentration, pH value and conductivity of the electrolyte, with a target concentration of 0.22-0.32 mol / L and a target conductivity of 50-200 S / m, and adjusting the electrolyte according to the test results;
[0079] S32. Adjusting the electrolyte includes adjusting the concentration, pH value and conductivity.
[0080] Concentration adjustment includes increasing concentration and decreasing concentration, conductivity adjustment includes increasing conductivity and decreasing conductivity. If the detected concentration is lower than 0.22 mol / L or the conductivity is lower than 50 S / m, slowly add copper sulfate solution to the electrolyte. If the detected concentration is higher than 0.32 mol / L or the conductivity is higher than 200 S / m, add deionized water to dilute the electrolyte.
[0081] The pH adjustment includes increasing the pH and decreasing the pH. If the detected pH is lower than 5.5, sodium hydroxide is added to neutralize the acidic components in the electrolyte. If the detected pH is higher than 6.5, hydrochloric acid is added to lower the pH of the electrolyte.
[0082] Furthermore, the concentration of the electrolyte is detected by titration or spectrophotometry, with a target concentration range of 0.22-0.32 mol / L. Too high or too low a concentration will affect the generation rate and morphology of the microparticles. The pH value of the electrolyte is measured by a pH meter, with a target range of 5.5-6.5. The pH value has an important influence on the stability of the electrolyte and the generation of microparticles. The conductivity of the electrolyte is measured by a conductivity meter, with a target range of 50-200 S / m. The conductivity reflects the ability of ions in the electrolyte to conduct current and has a direct impact on the efficiency of the electrochemical process.
[0083] According to the test results of concentration, pH value and conductivity, determine whether the electrolyte needs to be adjusted and formulate a corresponding adjustment plan;
[0084] Concentration adjustment: If the detected concentration is lower than 0.22 mol / L, it means that the solute concentration in the electrolyte is insufficient and the concentration needs to be increased. At this time, copper sulfate solution can be slowly added to the electrolyte while stirring until the concentration reaches the target range;
[0085] If the detected concentration is higher than 0.32 mol / L, it means that the electrolyte is too concentrated and needs to be reduced. At this time, deionized water can be added to dilute the electrolyte. It is also necessary to stir while adding to ensure uniform mixing.
[0086] Conductivity adjustment: Conductivity adjustment is usually carried out simultaneously with concentration adjustment. Adding copper sulfate solution can increase the concentration and conductivity of the electrolyte, while adding deionized water can reduce the concentration and conductivity of the electrolyte.
[0087] pH adjustment: If the detected pH value is lower than 5.5, it means that the electrolyte is acidic and needs to be increased. At this time, slowly add an appropriate amount of sodium hydroxide solution to neutralize the acidic components in the electrolyte, stirring while adding and monitoring the pH change;
[0088] If the detected pH value is higher than 6.5, it means that the electrolyte is alkaline and needs to be lowered. At this time, add an appropriate amount of hydrochloric acid solution to lower the pH value of the electrolyte. It is also necessary to stir while adding and monitor the pH value changes.
[0089] Embodiment 4:
[0090] See also Figure 1 The present invention provides an embodiment: a low-density irregular metal porous particle, and the preparation method of the irregular metal porous particle is as follows:
[0091] Step S4, electrolyzing to generate high-purity metallic copper;
[0092] In S4, the following steps are also included:
[0093] S41, prepare an electrolytic cell, pour the electrolyte into the electrolytic cell, use the copper raw material as the anode, use a thin copper plate coated with wax as the cathode, turn on the power supply, and start electrolysis;
[0094] S42, monitoring and adjusting the parameters and electrolysis conditions of the electrolyte, wherein the parameters of the electrolyte include concentration, pH value and conductivity, and the electrolysis conditions include voltage, current and temperature;
[0095] S43. The cathode is taken out from the electrolytic cell, and the cathode is preheated to soften the wax layer. The wax layer is peeled off from the cathode surface using a scraper or gently to obtain high-purity metallic copper.
[0096] Furthermore, the material of the electrolytic cell is ensured to be corrosion resistant and conductive, and the pre-prepared electrolyte is poured into the electrolytic cell, ensuring that the amount of electrolyte is appropriate to cover the effective working area of the anode and cathode. A high-purity copper raw material is used as the anode, which is fixed at one end of the electrolytic cell, and a thin copper plate coated with wax is used as the cathode, because the wax layer can prevent copper from being directly deposited on the cathode during the electrolysis process, thereby forming a porous structure;
[0097] Connect the electrolytic cell to the power supply, turn on the power supply to start electrolysis. During the electrolysis process, copper ions dissolve from the anode into the electrolyte and are reduced to metallic copper by electrons on the cathode surface. However, since the cathode surface is coated with a wax layer, metallic copper cannot be deposited directly on the cathode, but will be deposited in the pores or cracks of the wax layer, thus forming a porous structure.
[0098] Regularly test the concentration, pH value and conductivity parameters of the electrolyte. Changes in these parameters will affect the electrolysis efficiency and the purity of the copper metal. If the parameters are found to deviate from the preset range, they should be adjusted in time. According to the monitoring results, the concentration, pH value and conductivity of the electrolyte should be adjusted to the optimal range by adding appropriate amounts of solutes, acid-base regulators or deionized water;
[0099] At the same time, the voltage, current and temperature conditions during the electrolysis process are monitored. These conditions have an important influence on the electrolysis rate and the morphology of the metal copper. According to actual needs, the power supply voltage, current density or cooling system are adjusted to keep the electrolysis conditions within the optimal range;
[0100] After the electrolysis is completed, turn off the power supply and remove the cathode from the electrolytic cell. At this time, the wax layer on the surface of the cathode has been embedded with high-purity copper. The cathode is preheated to soften the wax layer. The preheating temperature should be moderate to avoid melting or deformation of the copper. The preheating treatment helps to weaken the bonding force between the wax layer and the copper, which is convenient for subsequent stripping.
[0101] Use a scraper or similar tool to gently peel off the wax layer from the cathode surface. During the peeling process, be careful to maintain uniform force to avoid damaging the surface of the copper metal. The wax layer after peeling contains most of the impurities that did not participate in the electrolysis and the residual electrolyte components, while the copper metal remains on the cathode to form a porous structure. The copper metal after peeling the wax layer should be cleaned to remove the residual electrolyte and impurities. After cleaning, it should be dried to prevent the copper metal surface from oxidation or moisture.
[0102] Embodiment 5,
[0103] See also Figure 1 The present invention provides an embodiment: a low-density irregular metal porous particle, and the preparation method of the irregular metal porous particle is as follows:
[0104] Step S5, post-processing the high-purity metallic copper, the post-processing comprising washing, drying and grinding;
[0105] In S1, the following steps are also included:
[0106] S51. Rinse the high-purity copper metal with deionized water and gently scrub the surface with a soft brush. Repeat the rinsing several times until the rinse liquid becomes clear.
[0107] S52, placing the cleaned high-purity metallic copper on a tray of a dryer for drying. After drying, turning off the power of the dryer, opening the dryer after cooling to room temperature, taking out the high-purity metallic copper, and grinding to obtain high-purity metallic copper powder with a purity greater than 99.9% and an average particle size of 80 μm.
[0108] Further, the high-purity copper metal is rinsed with deionized water, and the surface is gently scrubbed with a soft brush to remove dirt and oxides attached to the metal surface. The rinsing is repeated several times until the rinsing liquid becomes clear, indicating that the surface has been basically cleaned. The rinsed high-purity copper metal is placed on a tray of a dryer for drying. After drying, the power of the dryer is turned off and it is waited for to cool naturally to room temperature. After cooling, the dryer is opened to take out the copper metal to ensure that the material properties will not be affected by temperature changes in subsequent processing.
[0109] The dried metallic copper is ground using a grinding device to obtain high-purity metallic copper powder with a purity greater than 99.9% and an average particle size of 80 μm. The high purity ensures the stability of material properties in subsequent processing, and the particle size of 80 μm contributes to the formation of a porous structure.
[0110] Embodiment 6,
[0111] See also Figure 1The present invention provides an embodiment: a low-density irregular metal porous particle, and the preparation method of the irregular metal porous particle is as follows:
[0112] Step S6, preparing low-density irregular metal porous particles;
[0113] In S6, the following steps are also included:
[0114] S61. Using high-purity copper powder as the matrix material and soluble NaCl particles with an average particle size of 0.85 mm as the pore-forming agent, the high-purity copper powder and the soluble NaCl particles are uniformly mixed in different volume ratios, the volume proportions of the high-purity copper powder are 10%, 20%, 30% and 40% respectively, and the PILOTPRO pressure testing machine is used to press the green sheets at a pressure of 200 MPa, and the green sheets have a size of 20 mm×20 mm;
[0115] S62, put into TCXC1200T tubular muffle furnace, use argon as protective gas, raise the temperature to 600℃, 700℃, 800℃ and 900℃ at a heating rate of 10℃ / min, and the sintering time is 3h;
[0116] S63. After sintering is completed and cooled to room temperature, the upper and lower non-porous parts are removed and cut into 10mm×10mm. After being rinsed with deionized water at 70℃-80℃ for 30min, it is dried at 100℃ for 2h in a WGL-230B forced air drying oven to obtain low-density irregular metal porous particles.
[0117] Further, the measurement parameter table is as follows:
[0118]
[0119]
[0120] Embodiment 7,
[0121] See also Figure 1 The present invention provides an embodiment: a low-density irregular metal porous particle, and the preparation method of the irregular metal porous particle is as follows:
[0122] Step S7, measuring the porosity and compression performance of the porous metal particles;
[0123] In S7, the following steps are also included:
[0124] S71. The density of the metal porous particles is measured by an XS225DU-Swiss Mettler-Toledo electronic density specific gravity analysis balance, and the porosity of the metal porous particles is calculated;
[0125] The calculation formula of porosity is: P = 1-(ρ measured - ρ actual);
[0126] Where: P is the porosity, ρmeasured is the measured density of the metal porous particles, and ρactual is the density of the non-porous metal copper;
[0127] S72, static compression test using a ZwickRoell static materials testing machine.
[0128] Furthermore, under the same other conditions and different volume proportions of high-purity copper metal powder, the porosity measurement results are as follows:
[0129]
[0130] The porosity measurement results show that, under the same other conditions, the porosity gradually decreases with the increase of the volume proportion of metal copper powder.
[0131] When other conditions are the same and the sintering temperature is different, the porosity measurement results are as follows:
[0132]
[0133]
[0134] The porosity measurement results show that: under the same other conditions, with the increase of sintering temperature, the porosity decreases slightly at 600℃-700℃, because the increase in temperature promotes the viscosity and sintering growth stage of copper powder sintering process, making the gap between copper powder particles smaller, so that the porosity of the porous copper is slightly reduced. When the sintering temperature is 900℃, the porosity decreases significantly, because the temperature is too high to melt NaCl, and the metal porous particles lose support, causing local collapse and resulting in a decrease in porosity.
[0135] The static compression test results show that:
[0136] For the porous metal particles prepared at a sintering temperature of 800°C, as the porosity increases, the platform area of the porous copper compression curve gradually shortens, the platform stress increases, and the stress decreases when it begins to enter the dense zone.
[0137] For the porous metal particles prepared when the volume proportion of the metal copper powder is 10%, the compression performance is less affected by the change of the sintering temperature.
[0138] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A low-density irregular metal porous particle and a preparation method thereof, It is characterized in that The preparation method of irregular metal porous particles is as follows: Step S1, pre-treating the copper raw material, the pre-treatment including mechanical pre-treatment, pickling, ultrasonic cleaning, drying and oil protection; Step S2, preparing electrolyte; Step S3, detecting electrolyte performance; Step S4, electrolyzing to generate high-purity metallic copper; Step S5, post-processing the high-purity metallic copper, the post-processing comprising washing, drying and grinding; Step S6, preparing low-density irregular metal porous particles; Step S7, measuring the porosity and compression performance of the porous metal particles; In S1, the following steps are also included: S11. Use a steel brush and a nylon brush to gently scrub the surface of the copper raw material, and use sandpapers of different roughness to polish it, starting from coarse sandpaper and gradually transitioning to fine sandpaper, to obtain a copper raw material with a smooth surface; S12, using 0.2 mol / L dilute hydrochloric acid as a pickling agent, immersing the copper raw material in the pickling agent for 20 minutes for pickling, taking out the copper raw material after the pickling is completed, and washing the surface of the copper raw material with deionized water for 8 minutes; S13, then put the copper raw material into an ultrasonic cleaning machine, add a cleaning solution for ultrasonic cleaning, put the cleaned copper raw material into a vacuum drying oven for drying, use a brush and a spray gun to evenly apply anti-rust oil on the surface of the copper raw material, and fully dry it to form a protective film.
2. A low-density irregular metal porous particle and a preparation method thereof according to claim 1, Features: The cleaning solution is one of deionized water, acetone solution and ethanol solution.
3. A low-density irregular metal porous particle and a preparation method thereof according to claim 1, Features: In S2, the following steps are also included: S21. Slowly add copper sulfate powder into deionized water, stirring while adding until it is completely dissolved, add additives, adjust the pH value to 5.5-6.5, stir well, make the electrolyte to the fixed volume and filter.
4. A low-density irregular metal porous particle and a preparation method thereof according to claim 3, Features: Additives include surfactants, corrosion inhibitors, grain refiners and electrolyte regulators.
5. A low-density irregular metal porous particle and a preparation method thereof according to claim 1, Features: In S3, the following steps are also included: S31, detecting the concentration, pH value and conductivity of the electrolyte, with a target concentration of 0.22-0.32 mol / L and a target conductivity of 50-200 S / m, and adjusting the electrolyte according to the test results; S32. Adjusting the electrolyte includes adjusting the concentration, pH value and conductivity.
6. A low-density irregular metal porous particle and a preparation method thereof according to claim 5, Features: Concentration adjustment includes increasing concentration and decreasing concentration, conductivity adjustment includes increasing conductivity and decreasing conductivity. If the detected concentration is lower than 0.22 mol / L or the conductivity is lower than 50 S / m, slowly add copper sulfate solution to the electrolyte. If the detected concentration is higher than 0.32 mol / L or the conductivity is higher than 200 S / m, add deionized water to dilute the electrolyte. The pH adjustment includes increasing the pH and decreasing the pH. If the detected pH is lower than 5.5, sodium hydroxide is added to neutralize the acidic components in the electrolyte. If the detected pH is higher than 6.5, hydrochloric acid is added to lower the pH of the electrolyte.
7. A low-density irregular metal porous particle and a preparation method thereof according to claim 1, Features: In S4, the following steps are also included: S41, prepare an electrolytic cell, pour the electrolyte into the electrolytic cell, use the copper raw material as the anode, use a thin copper plate coated with wax as the cathode, turn on the power supply, and start electrolysis; S42, monitoring and adjusting the parameters and electrolysis conditions of the electrolyte, wherein the parameters of the electrolyte include concentration, pH value and conductivity, and the electrolysis conditions include voltage, current and temperature; S43. The cathode is taken out from the electrolytic cell, and the cathode is preheated to soften the wax layer. The wax layer is peeled off from the cathode surface using a scraper or gently to obtain high-purity metallic copper.
8. A low-density irregular metal porous particle and a preparation method thereof according to claim 6, Features: In S5, the following steps are also included: S51. Rinse the high-purity copper metal with deionized water and gently scrub the surface with a soft brush. Repeat the rinsing several times until the rinse liquid becomes clear. S52, placing the cleaned high-purity metallic copper on a tray of a dryer for drying. After drying, turning off the power of the dryer, opening the dryer after cooling to room temperature, taking out the high-purity metallic copper, and grinding to obtain high-purity metallic copper powder with a purity greater than 99.9% and an average particle size of 80 μm.
9. A low-density irregular metal porous particle and a preparation method thereof according to claim 6, Features: In S6, the following steps are also included: S61. Using high-purity copper powder as the matrix material and soluble NaCl particles with an average particle size of 0.85 mm as the pore-forming agent, the high-purity copper powder and the soluble NaCl particles are uniformly mixed in different volume ratios, the volume proportions of the high-purity copper powder are 10%, 20%, 30% and 40% respectively, and the PILOTPRO pressure testing machine is used to press the green sheets at a pressure of 200 MPa, and the green sheets have a size of 20 mm×20 mm; S62, put into TCXC1200T tubular muffle furnace, use argon as protective gas, raise the temperature to 600℃, 700℃, 800℃ and 900℃ at a heating rate of 10℃ / min, and the sintering time is 3h; S63. After sintering is completed and cooled to room temperature, the upper and lower non-porous parts are removed and cut into 10mm×10mm. After being rinsed with deionized water at 70℃-80℃ for 30min, it is dried at 100℃ for 2h in a WGL-230B forced air drying oven to obtain low-density irregular metal porous particles.
10. A low-density irregular metal porous particle and a preparation method thereof according to claim 1, Features: In S7, the following steps are also included: S71. The density of the metal porous particles is measured by an XS225DU-Swiss Mettler-Toledo electronic density specific gravity analysis balance, and the porosity of the metal porous particles is calculated; The calculation formula of porosity is: P = 1-(ρ measured - ρ actual); Where: P is the porosity, ρmeasured is the measured density of the metal porous particles, and ρactual is the density of the non-porous metal copper; S72, static compression test using a ZwickRoell static materials testing machine.