High-speed bright silver plating electroplating solution and application thereof

By combining the suitable electroplating conditions, silver nitrate and triazole compounds in high-speed bright silver plating solution, combined with suitable electroplating conditions, the problem of insufficient conductivity and oxidation resistance of molybdenum foil material is solved, and silver plating is realized on the surface of molybdenum metal Stable deposition and efficient combination enhance the overall performance of molybdenum foil.

CN118996553APending Publication Date: 2024-11-22JIANGMEN UBIS SEMICON MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411121314.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In high temperature environments, the conductive ability and damage resistance of molybdenum foil material are insufficient, and its oxidation properties are strong, which makes silver plated difficult to adhere, easily fall off, and it is difficult to form a stable plating layer on the surface of molybdenum metal.

Method used

Using a high-speed bright silver plating solution, including silver nitrate, ammonium citrate, triazole compounds, brighteners, pH adjusters, polypropylene glycol, sulfonates and potassium carbonate, through the complexation of triazole compounds The action and the conductivity of potassium carbonate improve the deposition flatness and binding ability of silver ions, and combine the appropriate plating temperature and current density to ensure the stable bond between the plating layer and molybdenum metal.

Benefits of technology

The uniform, flat and stable deposition of silver plating on the surface of molybdenum metal is achieved, the bonding force and stability of the plating are improved, the problem of plating falls off is avoided, and the conductivity and welding of the molybdenum foil is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004995175530000071
    Figure BDA0004995175530000071
  • Figure BDA0004995175530000081
    Figure BDA0004995175530000081
  • Figure BDA0004995175530000091
    Figure BDA0004995175530000091
Patent Text Reader

Abstract

The invention relates to the technical field of silver electroplating, and particularly discloses a high-speed bright silver electroplating solution and application thereof. The high-speed bright silver plating electroplating solution comprises the following raw materials in parts by weight: 20-30 parts of silver nitrate, 25-35 parts of ammonium citrate, 40-60 parts of a triazole compound, 10-30 parts of a brightener, 15-25 parts of a pH regulator, 10-15 parts of polypropylene glycol, 20-30 parts of sulfonate, 5-8 parts of potassium carbonate and the balance of water. The high-speed bright silver plating electroplating solution can be used for plating silver on the surface of molybdenum metal, and has the advantages that the high-speed bright silver plating electroplating solution is tightly combined with the molybdenum metal, and a plating layer is bright.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of silver electroplating, and more specifically, to a high-speed bright silver electroplating solution and its application. Background Art

[0002] Silver powder has the advantages of good conductivity, strong antioxidant ability, and stable chemical properties, but its high price limits its wide application. Plating silver on the surface of ordinary powder can save silver usage. If the surface coating is relatively complete, it can replace silver powder under certain circumstances. Moreover, these powders themselves have their own special properties, which can give full play to the role of the two materials. It is simple and environmentally friendly. Therefore, there is room for demand for chemical silver plating solution and it has been developed in the long run.

[0003] At present, the interconnection sheet materials used in aerospace mainly use molybdenum foil, molybdenum and molybdenum alloy metal high temperature resistant materials, which can maintain high strength at high temperatures, and also have high thermal conductivity and low thermal expansion coefficient. However, since spacecraft are often affected by various complex environmental factors such as high-altitude radiation, meteorites, ultra-high temperature, and ultra-low temperature during orbital flight, in order to enhance the conductivity of molybdenum foil and improve its anti-damage ability on a large scale, it is necessary to surface treat the existing molybdenum foil material, that is, electroplate a layer of protective metal silver. In addition, under high temperature environment, molybdenum itself will produce strong oxidation, and its weldability will deteriorate. The surface silver plating process will greatly improve its weldability. However, it is very difficult to silver-plated on molybdenum sheets, and the silver plating often does not adhere firmly, causing the coating to fall off. Therefore, it is necessary to prepare a coating that can be stably bonded to the surface of molybdenum metal. Summary of the invention

[0004] In order to improve the bonding ability between the coating and the molybdenum metal surface, the present application provides a high-speed bright silver plating solution and its application.

[0005] The present application provides a high-speed bright silver plating solution and its application, which adopts the following technical solution: In the first aspect, the present application provides a high-speed bright silver plating solution, which adopts the following technical solution: A high-speed bright silver plating solution comprises the following raw materials in parts by weight: 20-30 parts of silver nitrate, 25-35 parts of ammonium citrate, 40-60 parts of triazole compounds, 10-30 parts of brighteners, 15-25 parts of pH adjusters, 10-15 parts of polypropylene glycol, 20-30 parts of sulfonates, 5-8 parts of potassium carbonate, and the balance is water.

[0006] By adopting the above technical scheme, silver nitrate is used as the main salt, which is insensitive to light, heat, etc., thereby improving the stability of the electroplating solution. The triazole compound is used as a complexing agent in the electroplating solution. The water in the electroplating solution acts as a weak base reagent to remove a proton on the triazole ring to convert it into a triazole anion, which coordinates with the monovalent silver ion to form a complex. At the same time, the triazole substance has a strong adsorption on molybdenum, which helps the silver ions to be quickly deposited on the surface of the molybdenum metal while strengthening the bonding ability of the coating and the molybdenum metal. At the same time, because the triazole substances can be connected to form a chain structure through the triazole ligand, they have a good complexing property for silver ions, thereby improving the flatness of the silver coating deposited on the molybdenum metal.

[0007] Ammonium citrate can help remove molybdenum oxide and impurities on the metal surface, making the surface of the electroplated substrate cleaner. It can also reduce the surface tension of the electroplating solution, increase the wettability of the electroplating solution to molybdenum metal, and form a microfilm on the surface of the plated part during electroplating, thereby increasing the rate of electromagnetic induction and electrochemical reaction and improving the quality of electroplating. Potassium carbonate, as a conductive salt, can increase the conductivity of the plating solution, promote a more uniform distribution of current on the cathode surface, and facilitate the uniform deposition of silver ions on the cathode molybdenum sheet.

[0008] Optionally, the triazole compound is a mercaptotriazole compound.

[0009] By adopting the above technical solution, mercaptotriazole has multiple coordination sites and strong coordination ability. At the same time, the presence of mercapto groups further improves the complexing ability of the triazole compound with silver ions and improves the adsorption capacity with the base material metal molybdenum.

[0010] Optionally, the raw materials further include o-benzoylsulfonyl imide, the weight ratio of the o-benzoylsulfonyl imide to the brightener is 1:(3-9), and the total amount of the brightener and o-benzoylsulfonyl imide is 10-30 parts.

[0011] By adopting the above technical solution, the main function of the brightener is to refine the grains. Adding it can reduce the tensile stress of the coating, but it will cause the tensile stress of the coating to increase. The compressive stress of o-benzoylsulfonyl imide is helpful to offset the tensile stress formed by the brightener, improve the bonding strength between the coating and the substrate, and thus obtain a bright and level coating.

[0012] Optionally, the sulfonate substance is mercaptosulfonate, which is any one of sodium 3-mercaptopropane sulfonate or sodium 2-mercaptoethane sulfonate.

[0013] By adopting the above technical scheme, the sulfonate group has a strong hydrophilicity, and its addition can improve the wettability of the plating solution to the molybdenum metal surface, so that the stability of the silver plating solution and the coating is greatly improved. At the same time, the complexation of mercaptosulfonic acid substances with silver ions increases the reduction potential of silver ions, and it also has a good complexation effect on silver ions, which is beneficial to the stable deposition of the silver coating on the molybdenum metal surface.

[0014] Optionally, the pH adjuster is one of sodium bicarbonate, sodium hydroxide and ammonia water.

[0015] By adopting the above technical solution, the addition of sodium bicarbonate, sodium hydroxide and ammonia water will not react with silver ions, will not affect the normal operation of the electrolyte, and only plays a role in adjusting the pH of the electrolyte. The alkaline pH regulator adjusts the pH in the electrolyte to alkaline, providing a suitable working environment for the electrolyte.

[0016] Optionally, the pH of the electroplating solution is between 8.5 and 9.0.

[0017] By adopting the above technical solution, the pH of the electroplating solution is increased to between 8.5 and 9.0, which can improve the protonation of the lone electron pair coordinated N atoms in the complexing agent triazole substances, improve the adsorption capacity of silver ions, reduce the presence of free silver ions in the electroplating solution, and thus improve the stability of the coating.

[0018] In a second aspect, the present application provides an application of a high-speed bright silver plating solution, using the following technical solution: an application of a high-speed bright silver plating solution on a molybdenum metal coating, comprising the following steps: Clean the surface of the molybdenum sheet and immerse it in the above-mentioned high-speed bright silver plating solution, using the molybdenum sheet as the cathode and the silver plate as the anode. After the silver plating is completed, take out the plated part from the plating solution, clean the surface with distilled water, and dry it with cold air.

[0019] By adopting the above technical solution, the surface of the molybdenum sheet is cleaned and the grease on the metal surface is removed, providing a clean metal surface for electroplating, ensuring that the coating has no defects, peeling, blistering, stains, etc. After power is turned on, the cathode molybdenum sheet attracts silver ions to deposit, and a bright silver coating with good bonding ability with the molybdenum metal is obtained.

[0020] Preferably, the electroplating temperature is 20-30°C and the current density is 0.2-0.5A·dm -2 .

[0021] By adopting the above technical solution, controlling the electroplating temperature between 20-30°C can improve the complexing ability of triazole and slow down the diffusion of silver ions to the surface of molybdenum metal, thereby effectively improving the polarization of the cathode. When the current density is too low, the crystal grains of the coating will be coarse, but when it is too high, it will cause a serious lack of metal ions near the cathode, resulting in loose silver coating, easy shedding and blistering of the coating. At the same time, the appropriate electroplating temperature and current density can accelerate the growth rate of the coating.

[0022] In summary, this application has the following beneficial effects: 1. Since the present application uses triazole compounds as complexing agents, and since they have three triazole ligands inside, they have a good complexing effect on the silver ions in the electroplating solution, helping the silver ions to be quickly deposited on the surface of the molybdenum metal, while improving the flatness of the coating on the molybdenum metal.

[0023] 2. During the application of the electroplating solution in this application, the temperature and current density in the aqueduct are controlled to improve the ability of the complexing agent to complex silver ions in the plating solution, so that a silver coating with fine grains and uniform and smooth coating can be obtained on the surface of the cathode molybdenum metal during the electroplating process. DETAILED DESCRIPTION

[0024] The present application is further described in detail below with reference to the embodiments.

[0025] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0026] 4-Amino-triazole was purchased from Shanghai Yuanye Biotechnology Co., Ltd.; 3-Mercapto-1,2,4-triazole was purchased from Wuhan Xinweiye Chemical Co., Ltd. Example

[0027] Example 1 A high-speed bright silver plating solution is prepared by the following steps: (1) Weigh 40 g of 4-amino-triazole, 35 g of sodium citrate, and 8 g of potassium carbonate and dissolve them in 1 L of deionized water. Stir evenly to obtain a mixed solution A. (2) dissolving 25 g of silver nitrate in the mixed solution A obtained in step (1), stirring evenly to obtain a mixed solution B; (3) 10 g of polypropylene glycol and 25 g of sodium dodecyl sulfate are dissolved in mixed solution B, and the mixture is heated to 35° C. with stirring, and 10 g of a brightener and 15 g of a pH adjuster are added to adjust the pH to 8.5, and the mixture is stirred evenly to obtain the high-speed bright silver plating solution, wherein the brightener is sodium thiosulfate and the pH adjuster is sodium hydroxide.

[0028] The application of a high-speed bright silver plating solution on a molybdenum metal coating specifically comprises the following steps: Clean the surface of the molybdenum sheet and immerse it in the above-mentioned high-speed bright silver plating solution. Use the molybdenum sheet as cathode and the silver plate as anode. Power on and control the current density to 0.2A·dm -2 , control the temperature in the aqueduct to 30℃, silver-plating for 10 minutes. After the silver plating is completed, take out the plated parts from the plating solution, clean the surface with distilled water, and dry them with cold air.

[0029] Example 2 A high-speed bright silver plating solution, which is different from Example 1 in that it is prepared by the following steps: (1) Weigh 50 g of 4-amino-triazole, 30 g of sodium citrate, and 5 g of potassium carbonate and dissolve them in 1 L of deionized water. Stir evenly to obtain a mixed solution A. (2) dissolving 30 g of silver nitrate in the mixed solution A obtained in step (1), stirring evenly to obtain a mixed solution B; (3) 12.5 g of polypropylene glycol and 30 g of sodium dodecyl sulfate were dissolved in mixed solution B, and the mixture was heated to 35° C. with stirring, and 20 g of sodium thiosulfate and 25 g of sodium hydroxide were added, and the pH was adjusted to 8.5, and the mixture was stirred evenly to obtain the high-speed bright silver plating solution.

[0030] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this example is used.

[0031] Example 3 A high-speed bright silver plating solution, which is different from Example 1 in that it is prepared by the following steps: (1) Weigh 60 g of 4-amino-triazole, 25 g of sodium citrate, and 6.5 g of potassium carbonate and dissolve them in 1 L of deionized water. Stir evenly to obtain a mixed solution A. (2) dissolving 20 g of silver nitrate in the mixed solution A obtained in step (1), stirring evenly to obtain a mixed solution B; (3) 15 g of polypropylene glycol and 20 g of sodium dodecyl sulfate were dissolved in mixed solution B, and the mixture was heated to 35° C. with stirring, and 30 g of sodium thiosulfate and 20 g of sodium hydroxide were added, and the pH was adjusted to 8.5, and the mixture was stirred evenly to obtain the high-speed bright silver plating solution.

[0032] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this example is used.

[0033] Example 4 A high-speed bright silver plating solution is different from Example 1 in that the triazole compound used in this example is 3-mercapto-1,2,4-triazole.

[0034] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this example is used.

[0035] Example 5 A high-speed bright silver plating solution is different from Example 4 in that this embodiment further includes 2.5 g of o-benzoylsulfonyl imide and the mass of sodium thiosulfate is adjusted to 7.5 g.

[0036] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this example is used.

[0037] Example 6 A high-speed bright silver plating solution is different from Example 4 in that this embodiment further includes 1g of o-benzoylsulfonyl imide and the mass of sodium thiosulfate is adjusted to 9g.

[0038] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this example is used.

[0039] Example 7 A high-speed bright silver plating solution is different from Example 5 in that the sulfonate used in this example is sodium 3-mercaptopropane sulfonate.

[0040] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this example is used.

[0041] Example 8 A high-speed bright silver plating solution is different from Example 5 in that the sulfonate used in this example is sodium 2-mercaptoethane sulfonate.

[0042] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this example is used.

[0043] Example 9 A high-speed bright silver plating solution, which is different from Example 7 in that the pH adjuster used in this example is sodium bicarbonate, and the pH of the plating solution is adjusted to 9.

[0044] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this example is used.

[0045] Example 10 A high-speed bright silver plating solution, which is different from Example 7 in that the pH adjuster used in this example is ammonia water, and the pH of the plating solution is adjusted to 10.

[0046] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this example is used.

[0047] Embodiment 11 A high-speed bright silver plating solution is prepared in the same manner as in Example 1.

[0048] The application of a high-speed bright silver plating solution on a molybdenum metal coating specifically comprises the following steps: Clean the surface of the molybdenum sheet and immerse it in the above-mentioned high-speed bright silver plating solution. Use the molybdenum sheet as cathode and the silver plate as anode. Power on and control the current density to 0.5A·dm -2 , control the temperature in the aqueduct to 20℃, silver-plating for 10 minutes. After the silver plating is completed, take out the plated parts from the plating solution, clean the surface with distilled water, and dry them with cold air.

[0049] Comparative Example Comparative Example 1 A high-speed bright silver plating solution is different from Example 1 in that no triazole compound is added in this comparative example.

[0050] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this comparative example is used.

[0051] Comparative Example 2 A high-speed bright silver plating solution is different from Example 1 in that no sulfonate substance is added in this comparative example.

[0052] The invention discloses an application of a high-speed bright silver plating solution on a molybdenum metal coating, which is different from Example 1 in that the plating solution prepared in this comparative example is used.

[0053] Comparative Example 3 A high-speed bright silver plating solution is prepared in the same manner as in Example 1.

[0054] The application of a high-speed bright silver plating solution on a molybdenum metal coating specifically comprises the following steps: Clean the surface of the molybdenum sheet and immerse it in the above-mentioned high-speed bright silver plating solution. Use the molybdenum sheet as cathode and the silver plate as anode. Power on and control the current density to 1.0A·dm -2 , control the temperature in the aqueduct to 20℃, silver-plating for 10 minutes. After the silver plating is completed, take out the plated parts from the plating solution, clean the surface with distilled water, and dry them with cold air.

[0055] Performance testing Test Method Test Object: Silver plating solution prepared by Example 1-11 and Comparative Example 1-3 and molybdenum sheet after electroplating; Plating speed test of plating solution: Plating speed test was carried out on the silver plating solution prepared in Examples 1-11 and the molybdenum sheet after electroplating treatment. The temperature was controlled at 35°C, and the test sheet after pre-plating treatment was placed in the aqueduct. The changes on the surface of the test sheet were observed under sufficient stirring. The molybdenum sheet was degreased, washed with water, and dried, and the surface area of ​​the molybdenum sheet was measured and weighed. After being placed in the plating solution for electroplating for 20 minutes, it was weighed again. The weight gain per unit area was calculated, which was the silver plating speed. Detection of coating surface performance: The appearance and covering capacity of the coating on the electroplating solution prepared in Example 1, Examples 5-6, Example 11, Comparative Example 1 and Comparative Example 3 and the molybdenum sheet after electroplating were measured by visual inspection and gloss measurement. The visual inspection method considers the color and roughness of the coating surface. The glossiness is measured by using a gloss meter at a refraction angle of 60°. Plating bonding ability test: Use a grid knife to draw a 10×10 square grid on the surface of the test sample from the horizontal and vertical directions of the electroplated molybdenum sheet, with an interval of 1mm, and each line should be deep enough to reach the substrate; use a soft brush to gently brush the two diagonals of the grid pattern backward 5 times and forward 5 times on the surface of the test sample, use 3M tape or tape of equivalent effectiveness to firmly stick the small grid to be tested, and use an eraser to vigorously wipe the tape to increase the contact area and strength between the tape and the tested area; firmly grasp one end of the tape, and quickly tear off the tape in the vertical (90°) direction, and observe the surface with a magnifying glass. Experimental rating standard parts table 1.

[0056] Table 1 Rating standards for bonding test Table 2 Plating solution electroplating speed test Plating speed μm / 20min Example 1 0.92 Example 9 1.34 Example 10 1.02 Embodiment 11 2.36 Comparative Example 1 0.28 Comparative Example 2 0.64 Comparative Example 3 0.77 Combining Example 7 with Examples 9-10 and Table 2, it can be seen that the electroplating speed of Example 10 slows down, indicating that the pH of the electroplating solution affects the electroplating speed. As the pH value increases, the deposition speed of the coating increases, but when the pH is greater than 9, the electroplating speed of the plating solution decreases significantly.

[0057] Combining Example 1, Example 11 and Comparative Example 3 and Table 2, it can be seen that the electroplating speed of Example 11 is the fastest, indicating that the temperature during electroplating is within an appropriate temperature and the current is within an appropriate range, so that the plating solution has better catalytic activity, accelerates the deposition rate of silver, and improves the electroplating speed of the plating solution.

[0058] Table 3 Coating surface performance test Coating surface properties Glossiness Example 1 Uniform, smooth and bright surface 186.5 Example 4 Uniform, smooth and bright surface 186.9 Example 5 The surface is uniform, smooth and bright 191.6 Example 6 The surface is uniform, smooth and bright 191.2 Embodiment 11 The surface is uniform, smooth and bright 195.4 Comparative Example 1 Rough and matte surface 112.9 Comparative Example 3 Rough surface and uneven coating 125.1 Combining Example 1 with Examples 4-6 and Table 3, it can be seen that the coating electroplated by the electroplating solution prepared in Examples 5-6 has good surface performance and high gloss, indicating that the addition of o-benzoylsulfonyl imide compounded with the brightener can offset the tensile stress formed by the brightener, thereby forming a bright and smooth silver coating, and the composite brightener can bring better gloss to the coating.

[0059] Combining Example 1 with Example 11, Comparative Example 3 and Table 3, it can be seen that the apparent performance of the coating in Example 11 is better than that in Example 1, indicating that the temperature in the aqueduct and the current passing therethrough during electroplating have an impact on the apparent performance of the coating.

[0060] Combining Example 1 with Comparative Example 1 and Table 3, it can be seen that the apparent performance of the coating in Example 1 is far superior to that in Comparative Example 1, indicating that when the electroplating solution lacks triazole compounds as complexing agents, it will affect the deposition of silver ions on the molybdenum metal, resulting in the coating being rough and dull.

[0061] Table 4 Plating bonding strength test results Combining Examples 1-4 with Comparative Example 1 and Table 4, it can be seen that the bonding ability between the coatings of Examples 1-4 and the molybdenum sheet is greatly improved compared with Comparative Example 1, indicating that when the electrolyte lacks mercaptotriazole compounds, it cannot play a stable complexing role on silver, which reduces the adsorption capacity of the coating for metallic molybdenum and the bonding ability of the coating decreases.

[0062] Combining Example 1, Examples 7-8 and Comparative Example 2 and Table 4, it can be seen that the bonding strength between the coating prepared by the electroplating solution of Examples 7-8 and the molybdenum metal is better than that of Example 1 and Comparative Example 2, indicating that when the added sulfonate is mercaptosulfonate, the coating has better bonding strength with the molybdenum metal surface.

[0063] Combining Example 1, Example 11 and Comparative Example 3 and Table 4, it can be seen that the various test performances of Example 11 are better than those of Example 1 and Comparative Example 3, indicating that by controlling the current density and the plating solution temperature during electroplating, the complexing ability of the substances in the plating solution for silver ions can be improved, so that silver can be stably and evenly deposited on the molybdenum metal surface.

[0064] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A high-speed bright silver plating solution, characterized in that: The composition comprises the following raw materials in parts by weight: 20-30 parts of silver nitrate, 25-35 parts of ammonium citrate, 40-60 parts of triazole compounds, 10-30 parts of brighteners, 15-25 parts of pH adjusters, 10-15 parts of polypropylene glycol, 20-30 parts of sulfonates, 5-8 parts of potassium carbonate, and the balance is water.

2. A high-speed bright silver plating solution according to claim 1, characterized in that: The triazole compound is a mercaptotriazole compound.

3. A high-speed bright silver plating solution according to claim 1, characterized in that: The raw materials also include o-benzoylsulfonyl imide, the weight ratio of the o-benzoylsulfonyl imide to the brightener is 1:(3-9), and the total amount of the brightener and the o-benzoylsulfonyl imide is 10-30 parts.

4. A high-speed bright silver plating solution according to claim 1, characterized in that: The sulfonate substance is mercaptosulfonate, which is any one of sodium 3-mercaptopropane sulfonate or sodium 2-mercaptoethane sulfonate.

5. A high-speed bright silver plating solution according to claim 1, characterized in that: The pH regulator is one of sodium bicarbonate, sodium hydroxide and ammonia water.

6. A high-speed bright silver plating solution according to claim 1, characterized in that: The pH of the electroplating solution is between 8.5 and 9.

0.

7. The application of a high-speed bright silver plating solution as described in any one of claims 1 to 6 on a molybdenum metal coating comprises the following steps: Clean the surface of the molybdenum sheet and immerse it in the above-mentioned high-speed bright silver plating solution, using the molybdenum sheet as the cathode and the silver plate as the anode. After the silver plating is completed, take out the plated part from the plating solution, clean the surface with distilled water, and dry it with cold air.