Integrated tantalum-silver composite double-layer functional coating material based on metal continuous porous network structure and preparation method of integrated tantalum-silver composite double-layer functional coating material

By using a tantalum-silver composite double-layer coating material with a metal continuous porous network structure on bone implantation devices, the problems of insufficient bond strength and single function in the prior art are solved, and high biocompatibility is achieved and anti-infection function significantly improves the self-healing cycle and treatment effect of fractures or bone defects.

CN118996571AActive Publication Date: 2024-11-22ZHEJIANG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410941893.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-22
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The coating and substrate bond strength of existing bone implant devices is insufficient, the function is single, and cannot meet the complex clinical needs. The self-healing cycle of fractures or bone defects is long, which can easily lead to infection.

Method used

The integrated tantalum-silver composite double-layer functional coating material based on metal continuous porous network structure is used to form a three-stage inlaid double-layer composite coating structure through ultrasonic cleaning, ultra-high voltage anodization, vacuum heating and physical vapor deposition. , combining the bioactivity and anti-infection properties of tantalum and silver, improves the binding strength and function of the coating.

Benefits of technology

The coating material that achieves high biocompatibility, anti-infection and promotes bone function has been enhanced, and the binding strength and clinical application effect of bone implantation devices have been enhanced, and the effect of bone infection and bone defect treatment has been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996571A_ABST
    Figure CN118996571A_ABST
Patent Text Reader

Abstract

The invention discloses an integrated tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure and a preparation method of the integrated tantalum-silver composite double-layer functional coating material. The preparation method comprises the following steps: 1) controllably constructing a first-stage continuous porous metal network structure on a cleaned titanium / titanium alloy surface by using a specific electrolyte formula and an ultrahigh-voltage anodic oxidation process; 2) performing vacuum heating and cleaning to remove impurities on the surface of the titanium / titanium alloy, performing physical vapor deposition (PVD) on the surface of the titanium / titanium alloy, and fusing a secondary tantalum coating structure into a hole; (3) a silver target material is replaced, secondary vacuum heating and cleaning are carried out, double PVD is carried out, a three-level silver coating structure is fused into meshes, and the porous metal network structure is completely covered with the three-level silver coating structure; 4) performing vacuum high-temperature pressure-maintaining heat treatment on the treated sample; and 5) carrying out multiple cleaning, packaging and irradiation sterilization to obtain the integrated tantalum-silver composite double-layer functional coating material with the continuous porous network structure. The material has long-acting antibacterial and osteogenesis promoting functions, and can be used in the fields of orthopedics and dentistry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a preparation technology of medical devices, and in particular to an integrated tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure and a preparation method thereof. Background Art

[0002] After fractures and bone defects occur, the current clinical treatment method is to use bone implants to fix them and then use the body's own recovery ability to achieve bone regeneration. However, the bone implants currently on the market usually do not have other biological functions besides support and fixation, and the fracture and bone defect process and the surgical process will bring in bacteria or impurities, making the surgical site very susceptible to infection; secondly, fractures and bone defects have a long self-healing period without external intervention. The above two types of problems often bring huge psychological, physiological and economic burdens to patients.

[0003] As a platform technology, coating technology can be introduced on substrates of any shape. However, due to the problem of the bonding strength between the coating and the substrate, and the single function of the coating that cannot meet the complex actual clinical needs, there are no mature multifunctional coating bone implant products on the market. In addition, most current research focuses on the use of organic anti-infective or osteogenic drugs to achieve the treatment of bone infection or bone defects. However, in the face of various enzymes in the body and the long cycle of bone defect repair / bone infection treatment, we are thinking whether inorganic metal materials with corresponding functions are more suitable for orthopedic application scenarios.

[0004] Therefore, in the present invention, we selected two inorganic metal materials, tantalum and silver, as the osteogenic and antibacterial active components, respectively, and introduced a continuous metal network structure on the surface of the titanium matrix as a spatial loading site to prepare an integrated tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure, which can be used for the full-cycle treatment of bone infection and bone defects. Summary of the invention

[0005] The purpose of the present invention is to provide an integrated tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure and a preparation method thereof, in order to address the problems of insufficient bonding strength between the surface coating and the substrate of current medical devices, and the single function of the coating that cannot meet the complex actual clinical needs, by combining the biological activity and anti-infection properties of tantalum and silver metals themselves.

[0006] The present invention is implemented by the following technical solution: a method for preparing an integrated tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure, comprising the following steps:

[0007] 1) Ultrasonic cleaning and chemical film removal pretreatment are first performed on the titanium / titanium alloy, and a primary continuous porous metal network structure is formed on the surface of the titanium / titanium alloy by using a specific electrolyte combined with an ultra-high voltage anodizing process;

[0008] 2) vacuum heating and cleaning the treated sample, and using physical vapor deposition (PVD) to integrate a secondary tantalum coating structure into the mesh of the primary continuous porous metal network structure;

[0009] 3) Replace the silver target, vacuum heat clean it again, and perform double PVD to integrate the three-level silver coating structure into the mesh to form a three-level inlaid double-layer composite coating structure;

[0010] 4) subjecting the treated samples to vacuum high temperature and pressure heat treatment;

[0011] 5) The processed samples are subjected to multiple cleaning, packaging and irradiation sterilization to obtain an integrated tantalum-silver composite functional coating material with a metal continuous porous network structure.

[0012] Furthermore, the ultrasonic cleaning in step 1) specifically includes: first ultrasonic chemical cleaning for 10-20 minutes, and then ultrasonic cleaning with deionized water at least three times, each time for 5 minutes;

[0013] The chemical cleaning liquid used in the ultrasonic chemical cleaning is as follows: 10-15 g / L sodium hydroxide, 6-10 g / L sodium metasilicate pentahydrate, 3-5 g / L sodium tripolyphosphate, 10-18 g / L sodium dodecyl sulfate, 0.4-0.6 g / L nitrilotriacetic acid, 2-5 g / L NP-10 (99%), 0.6-1 g / L MOP-5 (99%), 3-5 g / L LAB (99%), and 2-5 g / L FMES (99%).

[0014] The temperature of the ultrasonic chemical cleaning and the deionized water ultrasonic cleaning are both 45-50°C, the ultrasonic power is both 150-180W, and the ultrasonic frequency is both 80kHz;

[0015] The chemical film removal specifically includes: the chemical film removal formula is: 6-8wt% nitric acid, 2.5-4.5wt% ammonium bifluoride, 0.5-1.5wt% urea, and the rest is deionized water, the chemical film removal time is 2min, the temperature is 28-35°C, and then deionized water ultrasonic cleaning is performed at least three times, each time for 2min, the ultrasonic power is 150-180W, and the ultrasonic frequency is 80kHz.

[0016] Furthermore, the ultra-high voltage anodizing process specifically includes: the specific electrolyte formula is: zirconium fluoride 4.5-8.5g / L, propylene glycol 650-850ml / L, sodium phosphate 5-12g / L, OP-10 surfactant 3-5ml / L, ammonium carbonate 0.25-0.5g / L, aminosulfonic acid 0.5-1.2g / L, and the rest is deionized water, the specific electrolyte pH value is 10-12, the anode is the sample, the cathode is 304 stainless steel, the distance between the anode and the cathode is 40-50cm, the voltage is 80-90V, and the reaction time is 2-5h.

[0017] Further, in step 2), the vacuum heating cleaning specifically includes: vacuum furnace power of 4.5kW, vacuum degree of 50-100Pa, bias voltage ≤200V, vacuum cleaning mode heating of 480-530°C, cleaning time of 25-45min;

[0018] The physical vapor deposition (PVD) specifically includes: evacuating a vacuum furnace for 15-20 minutes, the vacuum degree in the furnace is higher than 0.06 Pa, the target material is a tantalum target material with a purity greater than 99.99%, and the background vacuum is higher than 4.0×10 -2 Pa, target power density is 1-5W / cm 2 , target current is 0.3-1.5A, and temperature is 150-180℃.

[0019] Further, in step 3), the vacuum heating cleaning specifically includes: vacuum furnace power of 4.5kW, vacuum degree of 50-100Pa, bias voltage ≤200V, vacuum cleaning mode heating of 480-530°C, cleaning time of 25-45min;

[0020] The double PVD method is as follows: the vacuum furnace is evacuated for 10-18 minutes, the vacuum degree in the furnace is higher than 0.1 Pa, the target material is a silver target material with a purity greater than 99.99%, and the background vacuum is greater than 4.0×10 -3 Pa, target power density is 1-5W / cm 2 , target current 2-5A, temperature 380-450℃.

[0021] Furthermore, in step 4), the vacuum high temperature pressure heat treatment process is specifically as follows: the vacuum furnace is evacuated to 4.5×10 -1 Pa, vacuum furnace power 100kW, raise the temperature in the furnace to 600-780℃ at a vacuum heating rate of 3-5℃ / min, and keep warm and pressurized for 2-4h; then adjust the slight positive pressure in the furnace to 150-300Pa, and cool the temperature in the furnace to 25-40℃ at a cooling rate of 5-10℃ / min.

[0022] Furthermore, in step 5), the multiple cleaning is ultrasonic cleaning using ultrapure water, the ultrasonic power is 70-90W, and the cleaning time is 10min;

[0023] The packaging is vacuum packaging;

[0024] The irradiation sterilization process uses Co 60 Sterilization, irradiation dose 5-10kGy.

[0025] A fused tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure is prepared by any of the methods described above.

[0026] Compared with the prior art, the present invention has the following advantages:

[0027] 1) The present invention uses titanium / titanium alloy, tantalum, silver, etc. as raw materials, and simultaneously uses a combination of processes such as ultra-high voltage anodizing, vacuum heating cleaning, vacuum PVD, and heat treatment to produce an integrated tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure. The above raw material selection and process combination are original to the present invention.

[0028] 2) The double-layer functional coating material of the present invention has a three-level composite structure: a first-level novel metal continuous porous network structure is obtained by using ultra-high voltage anodizing and an exclusively designed electrolyte formula; a second-level tantalum coating structure is respectively integrated into the mesh of the first-level continuous porous metal network structure by using two PVD processes to form a three-level embedded double-layer composite coating structure, thus obtaining an integrated tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure. The primary structure is made based on the ultra-high voltage anodization and special electrolyte formula of the present invention, the metal porous structures are continuous with each other (the continuous structure can provide complete mechanical bite after the tantalum / silver coating is integrated, so that the coating with the tertiary structure forms a nearly integral structure, thereby ensuring the high bonding strength of the coating), the structure is flat and smooth, and the internal space is large, which provides physical space sites for the deposition of the secondary and tertiary structures, while increasing the contact area and mechanical bite, and providing the possibility for the subsequent improvement of the bonding strength of the secondary and tertiary structures; the tantalum coating and the silver coating are integrated into the metal continuous porous network structure, and the tantalum coating is located in the middle layer and the silver coating is located in the top layer, which matches the time sequence of the silver coating first releasing silver ions for sterilization and the subsequent tantalum ion release to promote osteogenesis in subsequent use.

[0029] 3) The tantalum / silver coating in the present invention is introduced by using a double vacuum physical vapor deposition (PVD) technology. This is based on the problem of high surface tension in the empty holes of the continuous porous metal network structure. The air in the pore structure can be directly stripped by vacuum physical vapor deposition, so that tantalum and silver can be easily deposited in the pores, thereby achieving efficient integration of tantalum and silver in the pores. After forming a three-level composite structure of a double-layer functional coating material, it is further combined with a vacuum heat treatment process. Through heat treatment, the molecules on the interface between the three metal layers of titanium, tantalum and silver enter each other, and the diffusion distance is increased, thereby increasing the bonding strength between the coating and the substrate. In addition, the tantalum and silver coatings are clamped by the physical space sites provided by the primary metal continuous porous network structure, and are integrated into the pore structure, thereby increasing the contact area and mechanical bite, and secondarily empowering the coating bonding strength.

[0030] 4) The coating material in the present invention has high biocompatibility, high bonding strength, anti-infection function and bone-promoting function. The stability of the inorganic metal titanium, tantalum and silver raw materials ensures the high biocompatibility of the coating material; the above-mentioned porous continuous network structure and vacuum heat treatment ensure the high bonding strength of the coating and ensure the long-term stable use of the coating; the outer silver coating has an efficient broad-spectrum and long-term bactericidal effect, and kills bacteria in the surgical site by continuously releasing silver ions; and the tantalum coating in the middle layer is physically wrapped and blocked by the silver coating, so it is released later than silver, which conforms to the clinical scenario of first anti-infection and then bone-promoting, and tantalum ions have a recognized therapeutic effect on bone-promoting. The organic synergy of the above-mentioned materials and structures can ensure the perfect match between the function of the coating material and clinical needs.

[0031] 5) The coating preparation technology of the present invention is also platform-based and can be used to introduce coatings on the surface of bone implant devices of any shape, meeting the needs of various types of bone infections and bone defects, and has obvious universality and scalability. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The SEM image of the metal continuous porous network structure (Comparative Example 1);

[0033] Figure 2 The surface SEM image of the fused tantalum-silver composite double-layer functional coating based on the metal continuous porous network structure (Example 1);

[0034] Figure 3 The photo is of the fused tantalum-silver composite double-layer functional coating material based on the metal continuous porous network structure (A is the TC4 sample without any treatment, and B is the sample in Example 1);

[0035] Figure 4The in vitro release curve of tantalum and silver of the fused tantalum-silver composite double-layer functional coating material based on the metal continuous porous network structure (Example 1);

[0036] Figure 5 It is the anti-infection effect of the fused tantalum-silver composite double-layer functional coating material based on the metal continuous porous network structure (A is comparative example 1, B is example 1). DETAILED DESCRIPTION

[0037] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0038] Comparative Example 1:

[0039] 1) The titanium alloy substrate TC4 was ultrasonically cleaned by chemical waves; ultrasonic chemical cleaning was used for 30 minutes in sequence (ultrasonic cleaning solution formula: sodium hydroxide 10g / L, sodium metasilicate pentahydrate 8g / L, sodium tripolyphosphate 4g / L, sodium dodecyl sulfate 15g / L, nitrilotriacetic acid 0.5g / L, NP-10 (99%) 3.4g / L, MOP-5 (99%) 0.8g / L, LAB (99%) 4.5g / L, FMES (99%) 2.7g / L), and then ultrasonic cleaning was performed with deionized water for 3 times, each time for 5 minutes, the ultrasonic power was 180W, the ultrasonic frequency was 45KHz, and the temperature was 60°C.

[0040] 2) Soak in chemical film removal at room temperature for 90 seconds (the chemical film removal solution formula is: 8% nitric acid, 3% ammonium bifluoride, 0.5% urea, 89.5% water), and then use deionized water ultrasonic cleaning for 3 times, each time for 5 minutes.

[0041] 3) The sample was then subjected to an ultra-high voltage anodizing process to form a primary continuous porous metal network structure on the surface of the titanium substrate (the electrolyte formula was: zirconium fluoride 4.5 g / L, propylene glycol 650 ml / L, sodium phosphate 7 g / L, OP-10 surfactant 4 ml / L, ammonium carbonate 0.3 g / L, aminosulfonic acid 0.8 g / L, and the rest was deionized water), wherein the pH value of the electrolyte was controlled at 10, a rust-free steel plate was used as the cathode, the distance between the two electrodes was 40 cm, the voltage was 90 V, and the reaction time was 4 h.

[0042] 4) The samples were ultrasonically cleaned three times in succession using ultrapure water, with an ultrasonic power of 80W, a frequency of 30KHz, and a cleaning time of 10min; and then vacuum-packed and irradiated for sterilization. 60 Sterilization, irradiation dose 8kGy, finally get the desired sample, SEM picture as shown Figure 1 .

[0043] The binding strength of the above samples was tested, and the result was 56.9MPa. The cell survival rate after 7 days of testing with CCK-8 was 97.3% compared with the control group (i.e., the initial raw material TC4). The antibacterial ability was tested in combination with the inhibition zone experiment, and no inhibition zone appeared. Using the rat intramedullary infection model, the samples were sampled and tested 28 days after implantation, and the results were as follows: Figure 5 As shown in A, the infection has not been cured and there is basically no bone integration effect.

[0044] Embodiment 1:

[0045] 1) The titanium alloy substrate TC4 was ultrasonically cleaned by chemical waves; ultrasonic chemical cleaning was used for 30 minutes in sequence (ultrasonic cleaning solution formula: sodium hydroxide 10g / L, sodium metasilicate pentahydrate 8g / L, sodium tripolyphosphate 4g / L, sodium dodecyl sulfate 15g / L, nitrilotriacetic acid 0.5g / L, NP-10 (99%) 3.4g / L, MOP-5 (99%) 0.8g / L, LAB (99%) 4.5g / L, FMES (99%) 2.7g / L), and then ultrasonic cleaning was performed with deionized water for 3 times, each time for 5 minutes, the ultrasonic power was 180W, the ultrasonic frequency was 45KHz, and the temperature was 60°C.

[0046] 2) Soak in chemical film removal at room temperature for 90 seconds (the chemical film removal solution formula is: 8% nitric acid, 3% ammonium bifluoride, 0.5% urea, 89.5% water), and then use deionized water ultrasonic cleaning for 3 times, each time for 5 minutes.

[0047] 3) The sample was then subjected to an ultra-high voltage anodizing process to form a primary continuous porous metal network structure on the surface of the titanium substrate (the electrolyte formula was: zirconium fluoride 4.5 g / L, propylene glycol 650 ml / L, sodium phosphate 7 g / L, OP-10 surfactant 4 ml / L, ammonium carbonate 0.3 g / L, aminosulfonic acid 0.8 g / L, and the rest was deionized water), wherein the pH value of the electrolyte was controlled at 10, a rust-free steel plate was used as the cathode, the distance between the two electrodes was 40 cm, the voltage was 90 V, and the reaction time was 4 h.

[0048] 4) Vacuum heating cleaning: The power of the vacuum furnace is 4.5 kW, the vacuum degree is 80 Pa, the bias voltage is ≤ 200 V, the vacuum cleaning mode is heated at 530 ° C, the cleaning time is 35 min, and the surface of the sample is deeply cleaned.

[0049] 5) Place the sample in the chamber and evacuate for 18 minutes. The vacuum degree is higher than 0.06Pa, the purity of the tantalum target is 99.99%, and the background vacuum is higher than 4.0×10 -2 Pa, target power density is 4W / cm 2, the target current was 1.2A, the temperature was 168°C, the PVD deposition time was 1500s, and a secondary tantalum coating structure was built in the continuous metal pore structure of the sample;

[0050] 6) Evacuate for 15 minutes, the vacuum degree in the chamber is 0.1Pa; the purity of the silver target is 99.99%, the vacuum degree is higher than 0.1Pa, and the target power density is 3W / cm 2 , target current 3A, temperature 380℃, deposition time 1800s, further integrating and constructing a three-level silver coating structure in the continuous metal pore structure of the sample;

[0051] 7) Vacuum high temperature and pressure heat treatment process: vacuum furnace chamber is evacuated to 4.5×10 -1 Pa, vacuum furnace power 100kW, 5℃ / min vacuum heating rate to 700℃, keep warm and keep pressure for 2h; after the step is completed, adjust the slight positive pressure to 200Pa, and cool to 40℃ at a cooling rate of 10℃ / min.

[0052] 8) The samples were ultrasonically cleaned three times in succession using ultrapure water, with an ultrasonic power of 80W, a frequency of 30KHz, and a cleaning time of 10min; and then vacuum-packed and irradiated for sterilization. 60 After sterilization and irradiation at a dose of 8 kGy, the desired sample was finally obtained.

[0053] Compared with Comparative Example 1, this embodiment adds a secondary tantalum coating structure and a tertiary silver coating structure ( Figure 2 The binding strength of the above samples was tested, and the result was 48.9MPa. The cell survival rate after 7 days of testing with CCK-8 was 88.4% compared with the control group (i.e. the initial raw material TC4). The antibacterial ability was tested by combining the inhibition zone experiment, and the area of ​​the inhibition zone was 3.04cm 2 Using the rat intramedullary infection model, samples were taken 28 days after implantation and the results were as follows: Figure 5 As shown in B, the infection treatment effect is significant, and further combined with Micro-CT detection, it was found that obvious bone integration occurred on the surface of the sample.

[0054] Embodiment 2:

[0055] 1) The titanium alloy substrate TC4 was ultrasonically cleaned by chemical waves; ultrasonic chemical cleaning was used for 30 minutes in sequence (ultrasonic cleaning solution formula: sodium hydroxide 10g / L, sodium metasilicate pentahydrate 8g / L, sodium tripolyphosphate 4g / L, sodium dodecyl sulfate 15g / L, nitrilotriacetic acid 0.5g / L, NP-10 (99%) 3.4g / L, MOP-5 (99%) 0.8g / L, LAB (99%) 4.5g / L, FMES (99%) 2.7g / L), and then ultrasonic cleaning was performed with deionized water for 3 times, each time for 5 minutes, the ultrasonic power was 180W, the ultrasonic frequency was 45KHz, and the temperature was 60°C.

[0056] 2) Soak in chemical film removal at room temperature for 90 seconds (the chemical film removal solution formula is: 8% nitric acid, 3% ammonium bifluoride, 0.5% urea, 89.5% water), and then use deionized water ultrasonic cleaning for 3 times, each time for 5 minutes.

[0057] 3) The sample was then subjected to an ultra-high voltage anodizing process to form a primary continuous porous metal network structure on the surface of the titanium substrate (the electrolyte formula was: zirconium fluoride 4.5 g / L, propylene glycol 650 ml / L, sodium phosphate 7 g / L, OP-10 surfactant 4 ml / L, ammonium carbonate 0.3 g / L, aminosulfonic acid 0.8 g / L, and the rest was deionized water), wherein the pH value of the electrolyte was controlled at 10, a rust-free steel plate was used as the cathode, the distance between the two electrodes was 40 cm, the voltage was 90 V, and the reaction time was 4 h.

[0058] 4) Vacuum heating cleaning: The power of the vacuum furnace is 4.5 kW, the vacuum degree is 80 Pa, the bias voltage is ≤ 200 V, the vacuum cleaning mode is heated at 530 ° C, the cleaning time is 35 min, and the surface of the sample is deeply cleaned.

[0059] 5) Place the sample in the chamber and evacuate for 18 minutes. The vacuum degree is higher than 0.06Pa, the purity of the tantalum target is 99.99%, and the background vacuum is higher than 4.0×10 -2 Pa, target power density is 4W / cm 2 , the target current was 1.2A, the temperature was 168°C, the PVD deposition time was 1500s, and a secondary tantalum coating structure was built in the continuous metal pore structure of the sample;

[0060] 6) Evacuate for 15 minutes, the vacuum degree in the chamber is 0.1Pa; the purity of the silver target is 99.99%, the vacuum degree is higher than 0.1Pa, and the target power density is 3W / cm 2 , target current 3A, temperature 380℃, deposition time 1800s, further integrating and constructing a three-level silver coating structure in the continuous metal pore structure of the sample;

[0061] 7) Evacuate for 15 minutes, the vacuum degree in the chamber is 0.1Pa; the purity of the silver target is 99.99%, the vacuum degree is 4.5-6.54-1 Pa, target power density 3W / cm 2 , target current 3A, temperature 170°C. Deposition time 1800s,, further integrated into the sample continuous metal pore structure to build a three-level silver coating structure;

[0062] 8) The samples were ultrasonically cleaned three times in succession using ultrapure water, with an ultrasonic power of 80W, a frequency of 30KHz, and a cleaning time of 10min; and then vacuum-packed and irradiated for sterilization. 60 After sterilization and irradiation at a dose of 8 kGy, the desired sample was finally obtained.

[0063] Compared with Example 1, this example reduces the vacuum high temperature pressure heat treatment process. The above sample was tested for bonding strength, and the result was 27.4MPa; the cell survival rate after 7 days of testing using CCK-8 was 82.1% compared with the control group (i.e., the initial raw material TC4); the antibacterial ability test was combined with the antibacterial zone experiment, and the antibacterial zone area was 3.97cm 2 ; Using a rat intramedullary infection model, samples were taken 28 days after implantation and the results showed that bacteria washed off the sample surface for plate culture showed significant infection treatment effects. Further Micro-CT detection revealed obvious bone integration on the sample surface.

[0064] Embodiment 3:

[0065] 1) The titanium alloy substrate TC4 was ultrasonically cleaned by chemical waves; ultrasonic chemical cleaning was used for 30 minutes in sequence (ultrasonic cleaning solution formula: sodium hydroxide 10g / L, sodium metasilicate pentahydrate 8g / L, sodium tripolyphosphate 4g / L, sodium dodecyl sulfate 15g / L, nitrilotriacetic acid 0.5g / L, NP-10 (99%) 3.4g / L, MOP-5 (99%) 0.8g / L, LAB (99%) 4.5g / L, FMES (99%) 2.7g / L), and then ultrasonic cleaning was performed with deionized water for 3 times, each time for 5 minutes, the ultrasonic power was 180W, the ultrasonic frequency was 45KHz, and the temperature was 60°C.

[0066] 2) Soak in chemical film removal at room temperature for 90 seconds (the chemical film removal solution formula is: 8% nitric acid, 3% ammonium bifluoride, 0.5% urea, 89.5% water), and then use deionized water ultrasonic cleaning for 3 times, each time for 5 minutes.

[0067] 3) The sample was then subjected to an ultra-high voltage anodizing process to form a primary continuous porous metal network structure on the surface of the titanium substrate (the electrolyte formula was: zirconium fluoride 4.5 g / L, propylene glycol 650 ml / L, sodium phosphate 7 g / L, OP-10 surfactant 4 ml / L, ammonium carbonate 0.3 g / L, aminosulfonic acid 0.8 g / L, and the rest was deionized water), wherein the pH value of the electrolyte was controlled at 10, a rust-free steel plate was used as the cathode, the distance between the two electrodes was 40 cm, the voltage was 90 V, and the reaction time was 4 h.

[0068] 4) Vacuum heating cleaning: The power of the vacuum furnace is 4.5 kW, the vacuum degree is 80 Pa, the bias voltage is ≤ 200 V, the vacuum cleaning mode is heated at 530 ° C, the cleaning time is 35 min, and the surface of the sample is deeply cleaned.

[0069] 5) Vacuum for 15 minutes, vacuum degree in the chamber is 0.1Pa; the purity of silver target is 99.99%, vacuum degree is higher than 0.1Pa, target power density is 3W / cm 2 , target current 3A, temperature 380℃, deposition time 1800s, further integrating and constructing the secondary silver coating structure in the continuous metal pore structure of the sample;

[0070] 6) Vacuum high temperature and pressure heat treatment process: vacuum furnace chamber is evacuated to 4.5×10 -1 Pa, vacuum furnace power 100kW, 5℃ / min vacuum heating rate to 700℃, keep warm and keep pressure for 2h; after the step is completed, adjust the slight positive pressure to 200Pa, and cool to 40℃ at a cooling rate of 10℃ / min.

[0071] 7) The samples were ultrasonically cleaned three times in succession using ultrapure water, with an ultrasonic power of 80W, a frequency of 30KHz, and a cleaning time of 10min; and then vacuum-packed and irradiated for sterilization. 60 After sterilization and irradiation at a dose of 8 kGy, the desired sample was finally obtained.

[0072] Compared with comparative example 1, the present embodiment reduces the construction of the tantalum coating structure. The above sample was tested for binding strength, and the result was 46.5MPa; the cell survival rate after 7 days of testing using CCK-8 was 84.1% compared with the control group (i.e., the initial raw material TC4); the antibacterial ability test was carried out in combination with the antibacterial zone experiment, and the antibacterial zone area was 3.46cm 2 ; Using a rat intramedullary infection model, samples were taken 28 days after implantation and tested. It was found that bacteria washed off the surface of the sample were plated and cultured, and the infection treatment effect was significant. Further combined with Micro-CT testing, it was found that there was basically no bone integration in the sample.

[0073] Embodiment 4:

[0074] 1) The titanium alloy substrate TC4 was ultrasonically cleaned by chemical waves; ultrasonic chemical cleaning was used for 30 minutes in sequence (ultrasonic cleaning solution formula: sodium hydroxide 10g / L, sodium metasilicate pentahydrate 8g / L, sodium tripolyphosphate 4g / L, sodium dodecyl sulfate 15g / L, nitrilotriacetic acid 0.5g / L, NP-10 (99%) 3.4g / L, MOP-5 (99%) 0.8g / L, LAB (99%) 4.5g / L, FMES (99%) 2.7g / L), and then ultrasonic cleaning was performed with deionized water for 3 times, each time for 5 minutes, the ultrasonic power was 180W, the ultrasonic frequency was 45KHz, and the temperature was 60°C.

[0075] 2) Soak in chemical film removal at room temperature for 90 seconds (the chemical film removal solution formula is: 8% nitric acid, 3% ammonium bifluoride, 0.5% urea, 89.5% water), and then use deionized water ultrasonic cleaning for 3 times, each time for 5 minutes.

[0076] 3) The sample was then subjected to an ultra-high voltage anodizing process to form a primary continuous porous metal network structure on the surface of the titanium substrate (the electrolyte formula was: zirconium fluoride 4.5 g / L, propylene glycol 650 ml / L, sodium phosphate 7 g / L, OP-10 surfactant 4 ml / L, ammonium carbonate 0.3 g / L, aminosulfonic acid 0.8 g / L, and the rest was deionized water), wherein the pH value of the electrolyte was controlled at 10, a rust-free steel plate was used as the cathode, the distance between the two electrodes was 40 cm, the voltage was 90 V, and the reaction time was 4 h.

[0077] 4) Vacuum heating cleaning: The power of the vacuum furnace is 4.5 kW, the vacuum degree is 80 Pa, the bias voltage is ≤ 200 V, the vacuum cleaning mode is heated at 530 ° C, the cleaning time is 35 min, and the surface of the sample is deeply cleaned.

[0078] 5) Place the sample in the chamber and evacuate for 18 minutes. The vacuum degree is higher than 0.06Pa, the purity of the tantalum target is 99.99%, and the background vacuum is higher than 4.0×10 -2 Pa, target power density is 4W / cm 2 , the target current was 1.2A, the temperature was 168°C, the PVD deposition time was 1500s, and a secondary tantalum coating structure was built in the continuous metal pore structure of the sample;

[0079] 6) Vacuum high temperature and pressure heat treatment process: vacuum furnace chamber is evacuated to 4.5×10 -1 Pa, vacuum furnace power 100kW, 5℃ / min vacuum heating rate to 700℃, keep warm and keep pressure for 2h; after the step is completed, adjust the slight positive pressure to 200Pa, and cool to 40℃ at a cooling rate of 10℃ / min.

[0080] 7) The samples were ultrasonically cleaned three times in succession using ultrapure water, with an ultrasonic power of 80W, a frequency of 30KHz, and a cleaning time of 10min; and then vacuum-packed and irradiated for sterilization. 60 After sterilization and irradiation at a dose of 8 kGy, the desired sample was finally obtained.

[0081] Compared with comparative example 1, the present embodiment reduces the construction of the silver coating structure. The above sample was tested for binding strength, and the result was 45.8MPa; the cell survival rate after 7 days of testing with CCK-8 was 94.7% compared with the control group (i.e., the initial raw material TC4); the antibacterial ability was tested in combination with the inhibition zone experiment, and basically no inhibition zone appeared; using the rat intramedullary infection model, sampling and testing 28 days after implantation found that the bacteria washed off the surface of the sample were plated and cultured, and the infection was obvious. Further combined with Micro-CT testing, it was found that basically no bone integration occurred on the surface of the sample.

[0082] The coating material of the present invention has both long-term antibacterial and bone-promoting functions, and can be used in the fields of orthopedics, dentistry, etc.

Claims

1. A method for preparing an integrated tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure, Features: The following steps are involved: 1) Ultrasonic cleaning and chemical film removal pretreatment are first performed on the titanium / titanium alloy, and a primary continuous porous metal network structure is formed on the surface of the titanium / titanium alloy by using a specific electrolyte combined with an ultra-high voltage anodizing process; 2) vacuum heating and cleaning the treated sample, and using physical vapor deposition (PVD) to integrate a secondary tantalum coating structure into the mesh of the primary continuous porous metal network structure; 3) Replace the silver target, vacuum heat clean it again, and perform double PVD to integrate the three-level silver coating structure into the mesh to form a three-level inlaid double-layer composite coating structure; 4) subjecting the treated samples to vacuum high temperature and pressure heat treatment; 5) The processed samples are subjected to multiple cleaning, packaging and irradiation sterilization to obtain an integrated tantalum-silver composite functional coating material with a metal continuous porous network structure.

2. The method for preparing the fused tantalum-silver composite double-layer functional coating material based on the metal continuous porous network structure according to claim 1, Features: The ultrasonic cleaning in step 1) specifically includes: first ultrasonic chemical cleaning for 10-20 minutes, and then ultrasonic cleaning with deionized water at least three times, each time for 5 minutes; The chemical cleaning liquid used in the ultrasonic chemical cleaning is as follows: 10-15 g / L sodium hydroxide, 6-10 g / L sodium metasilicate pentahydrate, 3-5 g / L sodium tripolyphosphate, 10-18 g / L sodium dodecyl sulfate, 0.4-0.6 g / L nitrilotriacetic acid, 2-5 g / L NP-10 (99%), 0.6-1 g / L MOP-5 (99%), 3-5 g / L LAB (99%), and 2-5 g / L FMES (99%). The temperature of the ultrasonic chemical cleaning and the deionized water ultrasonic cleaning are both 45-50°C, the ultrasonic power is both 150-180W, and the ultrasonic frequency is both 80kHz; The chemical film removal specifically includes: the chemical film removal formula is: 6-8wt% nitric acid, 2.5-4.5wt% ammonium bifluoride, 0.5-1.5wt% urea, and the rest is deionized water, the chemical film removal time is 2min, the temperature is 28-35°C, and then deionized water ultrasonic cleaning is performed at least three times, each time for 2min, the ultrasonic power is 150-180W, and the ultrasonic frequency is 80kHz.

3. The method for preparing the fused tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure according to claim 1, Features: The ultra-high voltage anodizing process specifically includes: the specific electrolyte formula is: zirconium fluoride 4.5-8.5g / L, propylene glycol 650-850ml / L, sodium phosphate 5-12g / L, OP-10 surfactant 3-5ml / L, ammonium carbonate 0.25-0.5g / L, aminosulfonic acid 0.5-1.2g / L, and the rest is deionized water. The pH value of the specific electrolyte is 10-12, the anode is the sample, the cathode is 304 stainless steel, the distance between the anode and the cathode is 40-50cm, the voltage is 80-90V, and the reaction time is 2-5h.

4. The method for preparing the fused tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure according to claim 1, Features: In step 2), the vacuum heating cleaning specifically includes: vacuum furnace power of 4.5kW, vacuum degree of 50-100Pa, bias voltage ≤200V, vacuum cleaning mode heating of 480-530°C, cleaning time of 25-45min; The physical vapor deposition (PVD) specifically includes: evacuating a vacuum furnace for 15-20 minutes, the vacuum degree in the furnace is higher than 0.06 Pa, the target material is a tantalum target material with a purity greater than 99.99%, and the background vacuum is higher than 4.0×10 -2 Pa, target power density is 1-5W / cm 2 , target current is 0.3-1.5A, and temperature is 150-180℃.

5. The method for preparing the fused tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure according to claim 1, Features: In step 3), the vacuum heating cleaning specifically includes: vacuum furnace power of 4.5kW, vacuum degree of 50-100Pa, bias voltage ≤200V, vacuum cleaning mode heating of 480-530°C, cleaning time of 25-45min; The double PVD method is as follows: the vacuum furnace is evacuated for 10-18 minutes, the vacuum degree in the furnace is higher than 0.1 Pa, the target material is a silver target material with a purity greater than 99.99%, and the background vacuum is greater than 4.0×10 -3 Pa, target power density is 1-5W / cm 2 , target current 2-5A, temperature 380-450℃.

6. The method for preparing the fused tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure according to claim 1, Features: In step 4), the vacuum high temperature pressure heat treatment process is specifically as follows: the vacuum furnace is evacuated to 4.5×10 -1 Pa, vacuum furnace power 100kW, raise the temperature in the furnace to 600-780℃ at a vacuum heating rate of 3-5℃ / min, and keep warm and pressurized for 2-4h; then adjust the slight positive pressure in the furnace to 150-300Pa, and cool the temperature in the furnace to 25-40℃ at a cooling rate of 5-10℃ / min.

7. The method for preparing the fused tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure according to claim 1, Features: In step 5), the multiple cleaning is ultrasonic cleaning using ultrapure water, the ultrasonic power is 70-90W, and the cleaning time is 10min; The packaging is vacuum packaging; The irradiation sterilization process uses Co 60 Sterilization, irradiation dose 5-10kGy.

8. An integrated tantalum-silver composite double-layer functional coating material based on a metal continuous porous network structure, It is characterized in that The method is prepared by the method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Products of manufacture having tantalum coated nanostructures, and methods of making and using them

    CN104203293A

  • Multilayer-structure tantalum-silver film implanted into surface of medical device and preparation method of multilayer-structure tantalum-silver film

    CN116688229A

  • A bone implant material with a tantalum-copper coating deposited on its surface and its preparation method.