Electrochemical corrosive liquid and application thereof in high-speed steel EBSD sample preparation

By combining chemical mechanical polishing and electrolytic polishing, the problem of difficult removal of the hardened layer of the surface of high-speed steel is solved, the calibration rate and resolution rate of EBSD sample preparation are improved, and the high-quality preparation of high-speed steel EBSD samples is achieved.

CN118996594APending Publication Date: 2024-11-22泛锐云智科技(郑州)有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093806.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the EBSD sample preparation process, high-speed steel has problems such as high sample preparation and low calibration rate. This is mainly because its surface hardened layer is difficult to effectively remove, which affects the authenticity of signal acquisition and structural information.

Method used

Using electrochemical corrosion solution based on chemical mechanical polishing and electrolytic polishing processes, including hydrochloric acid, phosphoric acid, ferric chloride, lauryl polyoxyethylene ether and glycerol, the high-speed removal is achieved through chemical corrosion and mechanical polishing. Hardened layers and scratches on the steel surface reduce surface stress and improve polishing quality.

Benefits of technology

The calibration rate and resolution rate of high-speed steel EBSD sample preparation have been significantly improved, reaching no less than 99%, ensuring the flatness and analytical effect of the sample.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996594A_ABST
    Figure CN118996594A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of structure and performance analysis and detection of high-speed steel, particularly relates to electrochemical corrosion liquid and application thereof in high-speed steel EBSD sample preparation, and discloses the electrochemical corrosion liquid aiming at the problem that a hardened layer is easily formed on the surface of the high-speed steel and a qualified EBSD sample cannot be prepared through a conventional method. Chemical mechanical polishing and electrolytic polishing treatment processes are combined, surface stress is reduced while a hardened layer on the surface of the high-speed steel is eliminated through mechanical polishing assisted by chemical etching, and the purpose of rapidly eliminating scratches, mechanical damage layers and residual stress on the surface of the high-speed steel is achieved; the surface roughness is further reduced, the Kikuchi pattern on the surface of the high-speed steel is clearer, the grain orientation and the grain boundary are more obvious, the high-speed steel EBSD sample preparation calibration rate is improved, meanwhile, the analysis rate of the high-speed steel EBSD sample is increased, and the calibration rate and the analysis rate of the high-speed steel EBSD sample prepared through the treatment method are both not lower than 99%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of structure and performance analysis and detection of high-speed steel, and particularly relates to an electrochemical etching solution and application thereof in EBSD sample preparation of high-speed steel. Background Art

[0002] High-speed steel is a tool steel with high hardness, high wear resistance and high heat resistance. It is widely used in cutting processing, molds and other fields. Due to its excellent wear resistance and high temperature resistance, high-speed steel has become an ideal choice for manufacturing turbine blades and other high-speed components of aircraft engines. It also has important application value in the aerospace field.

[0003] High-speed steel usually contains carbon, tungsten, molybdenum, chromium, vanadium, cobalt and other elements. For example, chromium can increase the hardness and wear resistance of high-speed steel and significantly improve its corrosion resistance. Molybdenum can enhance the hardness and strength of high-speed steel and enhance its corrosion resistance. The microstructure of high-speed steel is mainly composed of martensite, retained austenite and carbide phases. For example, the formation and distribution of martensite phase determines the hardness and strength of high-speed steel. The appropriate amount of retained austenite phase can improve the toughness of the material and prevent brittle fracture. Uniformly distributed carbides can improve the hardness and wear resistance of high-speed steel. It can be seen that the element composition, phase distribution, grain size, shape, and orientation of crystal structure in high-speed steel are closely related to its macroscopic properties. By reasonably controlling the composition, morphology and distribution of the microstructure and the heat treatment process, high-speed steel materials with excellent macroscopic properties can be obtained. Therefore, the characterization of the microstructure of high-speed steel is of great significance for optimizing the preparation process of high-speed steel, improving material properties and expanding its application field.

[0004] Since high-speed steel has strong wear resistance and hardness, a surface hardened layer is easily generated during its cutting process. The surface hardened layer of high-speed steel will not only affect the collection of EBSD signals, but also cover up the real structural information inside the sample, greatly increasing the difficulty of EBSD sample preparation. In addition, stress is easily generated during mechanical polishing, so higher energy and more delicate operations are required in the grinding and mechanical polishing steps, such as the need to use harder polishing pastes and finer polishing cloths. Even so, mechanical polishing is difficult to effectively remove the deformation layer and scratches on the sample surface, which is not conducive to subsequent chemical polishing or electrolytic polishing treatments, resulting in a low calibration rate of sample preparation, which in turn affects the accuracy of EBSD analysis. Summary of the invention

[0005] Aiming at the problems of high difficulty in sample preparation and low calibration rate in the existing EBSD sample preparation process of high-speed steel, the present invention aims to provide an electrochemical etching solution and its application in high-speed steel EBSD sample preparation. The present invention is based on the combination of chemical mechanical polishing and electrolytic polishing process, and selects electrochemical etching solution with suitable components and contents for use in the chemical mechanical polishing and electrolytic polishing processes of high-speed steel, respectively. While effectively eliminating the hardened layer on the surface of the high-speed steel, high-quality polishing of its surface is achieved, which significantly improves the calibration rate and resolution rate of high-speed steel EBSD sample preparation. The calibration rate and resolution rate of the high-speed steel EBSD sample prepared by the electrochemical etching solution of the present invention combined with the corresponding polishing process are not less than 99%.

[0006] Based on the above purpose, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides an electrochemical etching solution for high-speed steel EBSD sample preparation, comprising the following components: hydrochloric acid, phosphoric acid, ferric chloride, lauryl alcohol polyoxyethylene ether, glycerol and water.

[0007] Based on the high hardness and high wear-resistant characteristics of high-speed steel, its surface is very easy to form a hardened layer during processing, which is not conducive to the problem of EBSD sample preparation. In the electrochemical etching solution of the present invention, hydrochloric acid and phosphoric acid are used as the main corrosion components on the surface of high-speed steel, for etching the surface of high-speed steel to eliminate its surface hardened layer, while ferric chloride can promote the metal atoms on the surface of high-speed steel to undergo oxidation reaction, and then dissolve in the etching solution, which helps to further remove the microscopic unevenness and defects on the surface of high-speed steel; lauryl alcohol polyoxyethylene ether can significantly reduce the surface tension of the etching solution, making the etching solution more easily wet and penetrate into the surface fine pores of high-speed steel, helping to level the tiny concave-convex of the high-speed steel surface, and synergistically with other components to promote the redox reaction and product dissolution process on the surface of high-speed steel, further reducing surface roughness; glycerol can prevent acid mist from being generated, and forms a complex with phosphate ions, which plays a corrosion inhibition role. Through the compounding of the above-mentioned components, the electrochemical etching solution provided by the present invention has a good application effect in high-speed steel EBSD sample preparation.

[0008] Preferably, when the above-mentioned electrochemical etching solution is used in the chemical mechanical polishing process of high-speed steel, the electrochemical etching solution also includes a nano-diamond aqueous suspension. Calculated by weight percentage, the electrochemical etching solution includes the following components: 70wt% to 80wt% of the nano-diamond aqueous suspension, 2wt% to 10wt% of hydrochloric acid, 1wt% to 5wt% of phosphoric acid, 1wt% to 2wt% of ferric chloride, 0.1wt% to 0.5wt% of lauryl alcohol polyoxyethylene ether and 0.1wt% to 0.5wt% of glycerol, and the balance is water.

[0009] The present invention adopts a combination of chemical etching and mechanical polishing to perform surface treatment on high-speed steel. While chemical etching assists mechanical polishing to eliminate the hardened layer on the surface of the high-speed steel, the surface stress is reduced, thereby achieving the purpose of quickly eliminating scratches, mechanical damage layers and residual stress on the surface of the high-speed steel, and providing a clean, flat and stress-free surface for subsequent processing.

[0010] The present invention adds 70wt% to 80wt% of a nano-diamond aqueous suspension into a chemical etching solution, utilizes the extremely small particle size and extremely high hardness of the nano-diamond particles to provide a highly efficient grinding effect during the polishing process, cooperates with the etching effect of the chemical etching solution, and can avoid lattice distortion and phase change caused by mechanical stress, thereby maintaining the original microstructure of the sample.

[0011] Experiments have shown that, during the chemical mechanical polishing process, when the weight percentage of the nanodiamond aqueous suspension in the chemical etching solution is lower than 70wt%, the effective contact between the nanodiamond and the high-speed steel surface is reduced, and the surface hardened layer, rough layer and defects cannot be effectively removed in a short time. If the mechanical polishing time is extended, the surface stress will increase and the lattice distortion will be caused, which is not conducive to obtaining qualified EBSD samples. When the weight percentage is higher than 80wt%, if the same polishing time is maintained, the nanodiamonds will be unevenly distributed during the polishing process, and uneven scratches or rough areas will be easily left on the surface of the high-speed steel, causing over-polishing. If the chemical mechanical polishing time is shortened, the etching effect of other components of the chemical etching solution will be reduced, and the surface treatment effect of the high-speed steel will be poor.

[0012] Preferably, the concentration of nano-diamonds in the nano-diamond aqueous suspension is 2wt% to 5wt%; and the particle size of the nano-diamonds is 10 to 60 nm.

[0013] The concentration of nanodiamonds in the nanodiamond aqueous suspension is in the range of 2wt% to 5wt%, which enables the nanodiamond aqueous suspension to have good dispersion stability when used in combination with other components in a chemical etching solution, and effectively avoids the problem of uneven polishing of the high-speed steel surface caused by agglomeration of nanodiamonds.

[0014] The particle size of nano-diamond is in the range of 10 to 60 nm, and it cooperates with other components in the chemical etching solution to have a better polishing effect on the surface of high-speed steel.

[0015] Preferably, when the electrochemical etching solution is used in the electrolytic polishing process of high-speed steel, the electrochemical etching solution includes the following components in weight percentage: 25wt% to 35wt% of hydrochloric acid, 20wt% to 40wt% of phosphoric acid, 5wt% to 10wt% of ferric chloride, 1wt% to 5wt% of lauryl alcohol polyoxyethylene ether and 3wt% to 8wt% of glycerol, and the balance is water.

[0016] Compared with the chemical mechanical polishing process, the content of each component in the electrochemical etching solution is increased in the electrolytic polishing process. The compounding of hydrochloric acid, phosphoric acid and ferric chloride achieves the purpose of rapid electrolytic polishing of the high-speed steel surface after chemical mechanical polishing. At the same time, lauryl alcohol polyoxyethylene ether can significantly reduce the surface tension of the etching solution, making it easier for the etching solution to wet and penetrate into the fine pores on the surface of the high-speed steel, which is helpful to level the tiny concave and convex surfaces of the high-speed steel and further reduce the surface roughness. In addition, glycerol and phosphate ions form a complex to play a corrosion inhibition role. The compounding of the components in the above etching solution makes the kikuchi pattern on the surface of the high-speed steel clearer, the grain orientation and the grain boundary more obvious, and improves the resolution rate while improving the EBSD sample preparation calibration rate of the high-speed steel.

[0017] Preferably, the volume ratio of phosphoric acid to glycerol is (4-12):1.

[0018] Glycerol is one of the essential components in the chemical etching solution for EBSD sample preparation of high-speed steel. On the one hand, glycerol can increase the viscosity of the etching solution and effectively avoid the volatilization of acid mist produced by hydrochloric acid and the like during the electrolytic polishing process, which affects the etching effect; on the other hand, glycerol and phosphoric acid form a composite mucous film layer during the electrolytic polishing process, which adheres to the polished surface of the high-speed steel and helps to increase the resistance between different concave and convex parts of the surface, so that the metal grains in the protruding parts are preferentially dissolved during the electrolytic polishing process, further improving the surface polishing quality of high-speed steel and improving the calibration rate and resolution rate of EBSD sample preparation of high-speed steel.

[0019] In a second aspect, the present invention provides a method for preparing a high-speed steel EBSD sample, comprising the following steps: S1 Pre-grinding: Use diamond sandpaper to perform coarse grinding, fine grinding and fine grinding on the surface of the high-speed steel to be observed after wire cutting until the scratches on the surface are consistent; S2 chemical mechanical polishing: the high-speed steel treated in step S1 is subjected to chemical mechanical polishing rough polishing for 15 to 20 minutes using the electrochemical etching solution of claim 2, and then subjected to chemical mechanical polishing fine polishing for 30 to 40 minutes; S3 electrolytic polishing: placing the high-speed steel treated in step S2 in the electrochemical etching solution of claim 4, with the high-speed steel as the anode and the lead plate as the cathode, for electrolytic polishing for 10 to 20 seconds; S4 cleaning: The electropolished sample was ultrasonically cleaned in ethanol, then cleaned and dried with deionized water to obtain a high-speed steel EBSD sample.

[0020] The present invention adopts chemical mechanical polishing to subject the pre-ground high-speed steel to chemical etching and assist mechanical polishing to eliminate the hardened layer on the surface of the high-speed steel, while reducing the surface stress, so as to achieve the purpose of quickly eliminating scratches, mechanical damage layer and residual stress on the surface of the high-speed steel, and provide a clean, flat and stress-free surface for subsequent electrolytic polishing treatment; and then electrolytic polishing treatment is performed to eliminate tiny concave and convex on the surface of the high-speed steel, further reduce the surface roughness, make the kikuchi pattern on the surface of the high-speed steel clearer, and make the grain orientation and grain boundary more obvious, improve the calibration rate of the EBSD sample preparation of the high-speed steel, and improve its resolution rate, and the calibration rate and resolution rate of the high-speed steel EBSD sample prepared by the processing method of the present invention are not less than 99%.

[0021] Preferably, the pre-grinding in step S1 is to use 1000 mesh, 2000 mesh, 3000 mesh, 4000 mesh and 5000 mesh diamond sandpaper to perform coarse grinding, fine grinding and fine grinding on the high-speed steel in sequence.

[0022] Preferably, the particle size of the nano-diamond in the electrochemical etching solution used in the rough chemical mechanical polishing process in step S2 is 40-60 nm; the particle size of the nano-diamond in the electrochemical etching solution used in the fine chemical mechanical polishing process is 10-20 nm.

[0023] Preferably, the rotation speed of the rough chemical mechanical polishing in step S2 is 200-300 rpm; the rotation speed of the fine chemical mechanical polishing is 100-150 rpm.

[0024] When chemical mechanical polishing is performed on high-speed steel, an electrochemical etching solution containing a 40-60nm nano-diamond water suspension is used in advance for relatively high-speed rough polishing to further eliminate scratches, hardened layers and stress on the surface of the fine-ground high-speed steel. Then, an electrochemical etching solution containing a 10-20nm nano-diamond water suspension with a smaller particle size is used for relatively low-speed fine polishing to further reduce the surface roughness and residual stress of the high-speed steel, providing a clean, flat and stress-free surface for subsequent electrolytic polishing.

[0025] Preferably, the voltage of electrolytic polishing in step S3 is 5 to 10 V, and the current density is 3 to 8 A / dm 2 , the electrolytic polishing temperature is 25℃~35℃.

[0026] Based on the composition of the electrochemical etching solution of the present invention, within the above electrolytic polishing parameter range, electrolytic polishing is performed on high-speed steel after chemical mechanical polishing, and a relatively good EBSD sample preparation effect can be obtained.

[0027] Compared with the prior art, the present invention has the following beneficial effects: (1) Aiming at the problem that a hardened layer is easily formed on the surface of high-speed steel with high hardness and high wear resistance, it is impossible to obtain a qualified EBSD sample by using traditional mechanical polishing, chemical polishing or electrolytic polishing. The present invention discloses an electrochemical etching solution, which can effectively etch the surface of high-speed steel, help to eliminate the hardened layer on its surface, and avoid excessive stress, thereby helping to obtain a qualified high-speed steel EBSD sample.

[0028] (2) The present invention adopts chemical mechanical polishing treatment on the pre-ground high-speed steel. While chemical etching assists mechanical polishing to eliminate the hardened layer on the surface of the high-speed steel, the surface stress is reduced, so as to achieve the purpose of quickly eliminating scratches, mechanical damage layer and residual stress on the surface of the high-speed steel, and provide a clean, flat and stress-free surface for subsequent electrolytic polishing treatment; and then electrolytic polishing treatment is performed to eliminate the tiny asperities on the surface of the high-speed steel, further reduce the surface roughness, make the Kikuchi pattern on the surface of the high-speed steel clearer, and make the grain orientation and grain boundary more obvious. While improving the calibration rate of the EBSD sample preparation of the high-speed steel, its resolution rate is also improved. The calibration rate and resolution rate of the high-speed steel EBSD sample prepared by the treatment method of the present invention are not less than 99%. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the Kikuchi diffraction pattern of the M50 high-speed steel EBSD sample prepared in Example 1; Figure 2 The Euler diagram of the EBSD sample of M50 high speed steel in Example 1; Figure 3 This is the Kikuchi diffraction pattern of the M50 high-speed steel EBSD sample prepared in Example 2; Figure 4 This is the Kikuchi diffraction pattern of the M50 high-speed steel EBSD sample prepared in Example 3. DETAILED DESCRIPTION

[0030] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The test methods used in the examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified. Example 1

[0031] This embodiment takes M50 high-speed steel as an example to provide a method for preparing a high-speed steel EBSD sample, comprising the following steps: S1 Pre-grinding: Take the M50 high-speed steel sample, avoid the defective or damaged area, and use the wire cutting method to cut the M50 high-speed steel into 8mm×8mm×3mm samples, ensuring that the cut is smooth to avoid introducing new damage or stress. Use 1000 mesh diamond sandpaper to coarsely grind the surface to be treated to remove the rough layer and oxide layer on the surface of the sample; then use 2000 mesh, 3000 mesh and 4000 mesh diamond sandpaper for fine grinding in turn. Each time the sandpaper is changed, the sample is rotated 90 degrees to eliminate the scratches left by the previous grinding; finally, use 5000 mesh diamond sandpaper to finely grind the surface to be observed of the high-speed steel sample until the scratches on its surface are consistent.

[0032] S2 Chemical Mechanical Polishing: The M50 high speed steel finely ground in step S1 is subjected to chemical mechanical polishing using an electrochemical etching solution. The specific steps are as follows: The electrochemical etching liquid is evenly applied on the polishing disk, and the high-speed steel is placed on the polishing disk for polishing. During the polishing process, the polishing disk and the polishing head rotate and reciprocate at the same time to achieve uniform polishing of the sample surface. The high-speed steel is first subjected to chemical mechanical rough polishing at a speed of 300 rpm using the electrochemical etching liquid for 20 minutes, and then subjected to chemical mechanical fine polishing at a speed of 150 rpm using the chemical etching liquid for 30 minutes.

[0033] The composition of the electrochemical etching solution used in the chemical mechanical rough polishing process is as follows: 80wt% of nano-diamond water suspension, 10wt% of hydrochloric acid, 5wt% of phosphoric acid, 2wt% of ferric chloride, 0.5wt% of lauryl alcohol polyoxyethylene ether and 0.5wt% of glycerol, and the balance is 2wt% of deionized water, wherein the concentration of nano-diamonds in the nano-diamond water suspension is 5wt%, and the particle size range of the nano-diamonds is 40 to 60nm.

[0034] The composition of the electrochemical etching solution used in the chemical mechanical polishing process is as follows: 70wt% nano-diamond water suspension, 2wt% hydrochloric acid, 1wt% phosphoric acid, 1wt% ferric chloride, 0.1wt% lauryl alcohol polyoxyethylene ether and 0.1wt% glycerol, and the remainder is 25.8wt% deionized water, wherein the concentration of nano-diamonds in the nano-diamond water suspension is 2wt%, and the particle size range of the nano-diamonds is 10 to 20nm.

[0035] S3 electrolytic polishing: immerse the high-speed steel treated in step S2 in an electrochemical etching solution at 30°C, use the high-speed steel as the anode and the lead plate as the cathode, set the electrolytic polishing voltage to 10V and the current density to 8 A / dm 2 , electrolytic polishing was performed for 10 s.

[0036] The electrochemical etching solution includes the following components in weight percentage: 35wt% hydrochloric acid, 35wt% phosphoric acid, 8wt% ferric chloride, 5wt% lauryl alcohol polyoxyethylene ether and 5wt% glycerol, and the balance is water; wherein the volume ratio of phosphoric acid to glycerol is 7:1.

[0037] S4 cleaning: The electropolished sample is placed in anhydrous ethanol for ultrasonic cleaning to remove the residual corrosive liquid and impurities on the surface, and then the surface is rinsed with deionized water and blown dry to obtain a high-speed steel EBSD sample.

[0038] The Kikuchi diffraction pattern of the high-speed steel EBSD sample prepared in this example is as follows: Figure 1 As shown in the figure, it can be seen that the high-speed steel EBSD sample preparation method in this embodiment can obtain a clear Kikuchi diffraction pattern of high-speed steel. Figure 2 As shown, the grain orientation distribution and lattice information inside the sample can be clearly seen, and the calibration rate and resolution rate are both up to 99.5%. Example 2

[0039] This embodiment provides a method for preparing an M50 high speed steel EBSD sample, comprising the following steps: S1 Pre-grinding: Take the M50 high-speed steel sample, avoid the defective or damaged area, and use the wire cutting method to cut the M50 high-speed steel into 8mm×8mm×3mm samples, ensuring that the cut is smooth to avoid introducing new damage or stress. Use 1000 mesh diamond sandpaper to coarsely grind the surface to be treated to remove the rough layer and oxide layer on the surface of the sample; then use 2000 mesh, 3000 mesh and 4000 mesh diamond sandpaper for fine grinding in turn. Each time the sandpaper is changed, the sample is rotated 90 degrees to eliminate the scratches left by the previous grinding; finally, use 5000 mesh diamond sandpaper to finely grind the surface to be observed of the high-speed steel sample until the scratches on its surface are consistent.

[0040] S2 Chemical Mechanical Polishing: The M50 high speed steel finely ground in step S1 is subjected to chemical mechanical polishing using an electrochemical etching solution. The specific steps are as follows: The electrochemical etching liquid is evenly applied on the polishing disk, and the high-speed steel is placed on the polishing disk for polishing. During the polishing process, the polishing disk and the polishing head rotate and reciprocate at the same time to achieve uniform polishing of the sample surface. The high-speed steel is first subjected to chemical mechanical rough polishing at a speed of 200 rpm using the electrochemical etching liquid for 15 minutes, and then subjected to chemical mechanical fine polishing at a speed of 100 rpm using the chemical etching liquid for 40 minutes.

[0041] The composition of the electrochemical etching solution used in the chemical mechanical rough polishing process is as follows: 75wt% of nano-diamond water suspension, 8wt% of hydrochloric acid, 3wt% of phosphoric acid, 1wt% of ferric chloride, 0.3wt% of lauryl alcohol polyoxyethylene ether and 0.2wt% of glycerol, and the balance is 12.5wt% of deionized water, wherein the concentration of nano-diamonds in the nano-diamond water suspension is 4wt%, and the particle size range of the nano-diamonds is 40 to 60nm.

[0042] The composition of the electrochemical etching solution used in the chemical mechanical polishing process is as follows: 70wt% nano-diamond water suspension, 5wt% hydrochloric acid, 2wt% phosphoric acid, 1wt% ferric chloride, 0.2wt% lauryl alcohol polyoxyethylene ether and 0.3wt% glycerol, and the balance is 21.5wt% deionized water, wherein the concentration of nano-diamonds in the nano-diamond water suspension is 3wt%, and the particle size range of the nano-diamonds is 10 to 20nm.

[0043] S3 electrolytic polishing: immerse the high-speed steel treated in step S2 in an electrochemical etching solution at 35°C, use the high-speed steel as the anode and the lead plate as the cathode, set the electrolytic polishing voltage to 5V and the current density to 3 A / dm 2 , and electrolytic polishing was performed for 20 s.

[0044] The electrochemical etching solution includes the following components in weight percentage: 35wt% hydrochloric acid, 20wt% phosphoric acid, 10wt% ferric chloride, 1wt% lauryl alcohol polyoxyethylene ether and 4wt% glycerol, and the balance is water; wherein the volume ratio of phosphoric acid to glycerol is 5:1.

[0045] S4 cleaning: The electropolished sample is placed in anhydrous ethanol for ultrasonic cleaning to remove the residual corrosive liquid and impurities on the surface, and then the surface is rinsed with deionized water and blown dry to obtain a high-speed steel EBSD sample.

[0046] The Kikuchi diffraction pattern of the high-speed steel EBSD sample prepared in this example is as follows: Figure 3 As shown, it can be seen that the high-speed steel EBSD sample preparation method of this embodiment can obtain a clear Kikuchi diffraction pattern of high-speed steel. The calibration rate and resolution rate of the high-speed steel EBSD sample prepared by this embodiment are both 99.1%. Example 3

[0047] This embodiment provides a method for preparing an M50 high speed steel EBSD sample, comprising the following steps: S1 Pre-grinding: Take the M50 high-speed steel sample, avoid the defective or damaged area, and use the wire cutting method to cut the M50 high-speed steel into 8mm×8mm×3mm samples, ensuring that the cut is smooth to avoid introducing new damage or stress. Use 1000 mesh diamond sandpaper to coarsely grind the surface to be treated to remove the rough layer and oxide layer on the surface of the sample; then use 2000 mesh, 3000 mesh and 4000 mesh diamond sandpaper for fine grinding in turn. Each time the sandpaper is changed, the sample is rotated 90 degrees to eliminate the scratches left by the previous grinding; finally, use 5000 mesh diamond sandpaper to finely grind the surface to be observed of the high-speed steel sample until the scratches on its surface are consistent.

[0048] S2 Chemical Mechanical Polishing: The M50 high speed steel finely ground in step S1 is subjected to chemical mechanical polishing using an electrochemical etching solution. The specific steps are as follows: The electrochemical etching liquid is evenly applied on the polishing disk, and the high-speed steel is placed on the polishing disk for polishing. During the polishing process, the polishing disk and the polishing head rotate and reciprocate at the same time to achieve uniform polishing of the sample surface. The high-speed steel is first subjected to chemical mechanical rough polishing at a speed of 250rpm using the electrochemical etching liquid for 20min, and then subjected to chemical mechanical fine polishing at a speed of 120rpm using the chemical etching liquid for 35min.

[0049] The composition of the electrochemical etching solution used in the chemical mechanical rough polishing process is as follows: 80wt% of nano-diamond water suspension, 6wt% of hydrochloric acid, 3wt% of phosphoric acid, 5wt% of ferric chloride, 0.1wt% of lauryl alcohol polyoxyethylene ether and 0.1wt% of glycerol, and the balance is 5.8wt% of deionized water, wherein the concentration of nano-diamonds in the nano-diamond water suspension is 5wt%, and the particle size range of the nano-diamonds is 40 to 60nm.

[0050] The composition of the electrochemical etching solution used in the chemical mechanical polishing process is as follows: 70wt% nano-diamond water suspension, 3wt% hydrochloric acid, 2wt% phosphoric acid, 1.5wt% ferric chloride, 0.2wt% lauryl alcohol polyoxyethylene ether and 0.3wt% glycerol, and the balance is 23wt% deionized water, wherein the concentration of nano-diamonds in the nano-diamond water suspension is 3wt%, and the particle size range of the nano-diamonds is 10 to 20nm.

[0051] S3 electrolytic polishing: immerse the high-speed steel treated in step S2 in an electrochemical etching solution at 25°C, use the high-speed steel as the anode and the lead plate as the cathode, set the electrolytic polishing voltage to 8V and the current density to 6 A / dm 2 , electrolytic polishing was performed for 15s.

[0052] The electrochemical etching solution includes the following components in weight percentage: 25wt% hydrochloric acid, 40wt% phosphoric acid, 5wt% ferric chloride, 3wt% lauryl alcohol polyoxyethylene ether and 8wt% glycerol, and the balance is water; wherein the volume ratio of phosphoric acid to glycerol is 5:1.

[0053] S4 cleaning: The electropolished sample is placed in anhydrous ethanol for ultrasonic cleaning to remove the residual corrosive liquid and impurities on the surface, and then the surface is rinsed with deionized water and blown dry to obtain a high-speed steel EBSD sample.

[0054] The Kikuchi diffraction pattern of the high-speed steel EBSD sample prepared in this example is as follows: Figure 4 As shown, it can be seen that the high-speed steel EBSD sample preparation method of this embodiment can obtain a clear Kikuchi diffraction pattern of high-speed steel. The calibration rate and resolution rate of the high-speed steel EBSD sample prepared by this embodiment are both 99.3%. Comparative Example 1

[0055] The difference between this comparative example and Example 1 is that the "chemical mechanical polishing" in step S2 is replaced by "mechanical polishing". The mechanical polishing steps of this comparative example are as follows: The high-speed steel after the fine grinding treatment in step S1 is mechanically polished and roughly polished at a rotation speed of 300 rpm for 20 minutes using a 5 wt % nano-diamond aqueous suspension; wherein the particle size of the nano-diamonds in the nano-diamond aqueous suspension is 40-60 nm.

[0056] The high-speed steel after mechanical rough polishing is mechanically polished and finely polished using 2wt% nano-diamond water suspension at a rotation speed of 150rpm for 30 minutes; wherein the particle size of the nano-diamond in the nano-diamond water suspension is 10-20nm.

[0057] The rest of the parts not mentioned are the same as those in Example 1. The calibration rate of the high-speed steel EBSD sample prepared by the comparative example method is 88%, while the resolution rate is only 85%, which is lower than 99.5% in Example 1. It can be seen that for high-speed steel, the use of a chemical etching solution containing hydrochloric acid, phosphoric acid, ferric chloride, lauryl alcohol polyoxyethylene ether and glycerol combined with a mechanical polishing treatment method is helpful to further improve the calibration rate and resolution rate of high-speed steel EBSD sample preparation. Comparative Example 2

[0058] The only difference between this comparative example and Example 1 is that this comparative example does not undergo the electrolytic polishing treatment in step S3, and the rest of the parts not described are the same as Example 1. The calibration rate of the high-speed steel EBSD sample prepared in this comparative example reaches 90%, and the resolution rate is only 80%. It can be seen that although a high-speed steel EBSD sample with a relatively clear Kikuchi diffraction pattern can be prepared without electrolytic polishing treatment, the resolution rate of the sample is relatively low, which is not conducive to observing the grain boundary characteristics of the sample. Comparative Example 3

[0059] The difference between this comparative example and Example 1 is that the chemical mechanical polishing step S2 is a chemical mechanical fine polishing process, the processing time is 50 minutes, and no chemical mechanical rough polishing process is performed. The specific steps are as follows: The electrochemical etching liquid is evenly applied on the polishing disk, and the high-speed steel is placed on the polishing disk for polishing. During the polishing process, the polishing disk and the polishing head rotate and reciprocate at the same time to achieve uniform polishing of the sample surface. The high-speed steel is subjected to chemical mechanical fine polishing treatment at a speed of 150rpm for 50 minutes using chemical etching liquid.

[0060] The composition of the electrochemical etching solution used in the chemical mechanical polishing process is as follows: 70wt% nano-diamond water suspension, 2wt% hydrochloric acid, 1wt% phosphoric acid, 1wt% ferric chloride, 0.1wt% lauryl alcohol polyoxyethylene ether and 0.1wt% glycerol, and the balance is 25.8wt% deionized water, wherein the concentration of nano-diamonds in the nano-diamond water suspension is 2wt%, and the particle size range of the nano-diamonds is 10 to 20nm.

[0061] The rest of the parts not described are the same as those in Example 1. The calibration rate of the high-speed steel EBSD sample prepared in this comparative example reaches 93%, and the resolution rate is 90%. It can be seen that although a high-speed steel EBSD sample with a relatively clear Kikuchi diffraction pattern and a relatively high resolution rate can be obtained without chemical mechanical rough polishing, compared with the sample after step-by-step chemical mechanical rough polishing and chemical mechanical fine polishing (Example 1), the step-by-step chemical mechanical polishing treatment is more conducive to obtaining a higher high-speed steel EBSD sample preparation calibration rate and resolution rate. Comparative Example 4

[0062] The difference between this comparative example and Example 1 is that in the electrochemical etching solution components used in the chemical mechanical rough polishing and chemical mechanical fine polishing processes in step S2, the mass percentage of the nano-diamond aqueous suspension exceeds 80wt%, as follows: The composition of the electrochemical etching solution used in the chemical mechanical rough polishing process is as follows: 85wt% of nano-diamond water suspension, 6wt% of hydrochloric acid, 3wt% of phosphoric acid, 5wt% of ferric chloride, 0.1wt% of lauryl alcohol polyoxyethylene ether and 0.1wt% of glycerol, and the balance is 0.8wt% of deionized water, wherein the concentration of nano-diamonds in the nano-diamond water suspension is 5wt%, and the particle size range of the nano-diamonds is 40 to 60nm.

[0063] The composition of the electrochemical etching solution used in the chemical mechanical polishing process is as follows: 83wt% of nano-diamond water suspension, 3wt% of hydrochloric acid, 2wt% of phosphoric acid, 1.5wt% of ferric chloride, 0.2wt% of lauryl alcohol polyoxyethylene ether and 0.3wt% of glycerol, and the balance is 10wt% of deionized water, wherein the concentration of nano-diamonds in the nano-diamond water suspension is 3wt%, and the particle size range of the nano-diamonds is 10 to 20nm.

[0064] The rest of the parts not described are the same as those in Example 1. The calibration rate of the high-speed steel EBSD sample prepared in this comparative example is 83%. It can be seen that during the chemical mechanical polishing process, an excessively high content of the nanodiamond aqueous suspension in the chemical etching solution will lead to uneven distribution of the abrasive during the polishing process, leaving uneven scratches or rough areas on the surface of the high-speed steel, thereby reducing the calibration rate of the final high-speed steel EBSD sample preparation. Comparative Example 5

[0065] The difference between this comparative example and Example 1 is that in the electrochemical etching solution components used in the chemical mechanical rough polishing and chemical mechanical fine polishing processes in step S2, the mass percentage of the nano-diamond aqueous suspension is less than 70wt%, as follows: The composition of the electrochemical etching solution used in the chemical mechanical rough polishing process is as follows: 65wt% of nano-diamond water suspension, 6wt% of hydrochloric acid, 3wt% of phosphoric acid, 5wt% of ferric chloride, 0.1wt% of lauryl alcohol polyoxyethylene ether and 0.1wt% of glycerol, and the balance is 20.8wt% of deionized water, wherein the concentration of nano-diamonds in the nano-diamond water suspension is 5wt%, and the particle size range of the nano-diamonds is 40 to 60nm.

[0066] The composition of the electrochemical etching solution used in the chemical mechanical polishing process is as follows: 63wt% of nano-diamond aqueous suspension, 3wt% of hydrochloric acid, 2wt% of phosphoric acid, 1.5wt% of ferric chloride, 0.2wt% of lauryl alcohol polyoxyethylene ether and 0.3wt% of glycerol, and the balance is 30wt% of deionized water, wherein the concentration of nano-diamonds in the nano-diamond aqueous suspension is 3wt%, and the particle size range of the nano-diamonds is 10 to 20nm.

[0067] The rest of the parts not described are the same as Example 1. The calibration rate of the high-speed steel EBSD sample prepared in this comparative example reaches 78%. It can be seen that during the chemical mechanical polishing process, too low a content of nanodiamond aqueous suspension in the chemical etching solution will reduce the effective contact area between the abrasive and the high-speed steel, and the hardened layer, rough layer and defects on the surface of the high-speed steel cannot be effectively removed, resulting in poor polishing effect. Example 4

[0068] During the experiment, it was found that in the electrochemical etching solution system used in step S3 electrolytic polishing, the amount of phosphoric acid and glycerol and their compounding ratio had a significant effect on the high-speed steel EBSD sample preparation effect. This example explored the appropriate amount range and compounding ratio of phosphoric acid and glycerol in the electrochemical etching solution to obtain a better high-speed steel sample preparation effect through the following single factor analysis.

[0069] In this example, the contents of phosphoric acid and glycerol in the electrochemical etching solution used for electrolytic polishing in step S3 are used as single factor variables, the balance is supplemented with water, the contents of other components remain unchanged, and the remaining parts not described are the same as those in Example 1. The effects of the dosage and compounding ratio of phosphoric acid and glycerol on the calibration rate and resolution rate of high-speed steel EBSD sample preparation are analyzed, as shown in Table 1.

[0070] Table 1 Phosphoric acid / wt% Glycerol / wt% Compounding ratio Calibration rate / % Resolution rate / % 45 5 9:1 85 80 40 5 8:1 98 97 30 5 6:1 99 98 20 5 4:1 99 99 15 5 3:1 80 78 35 2 17.5:1 78 70 35 3 11.7:1 97 96 35 5 7:1 98 98 35 8 4.4:1 99 99 35 10 3.5:1 82 80 From the results in Table 1, it can be seen that when the phosphoric acid content in the electrochemical etching solution is higher than 40wt% or lower than 20wt%, the calibration rate and resolution rate of EBSD sample preparation are reduced when the dosage of other components remains unchanged. It is speculated that this may be because when the phosphoric acid content in the electrochemical etching solution is too high, the sample surface reacts too violently during the electrolytic polishing process, resulting in uneven corrosion, making the sample surface rough and interfering with the collection and analysis of EBSD signals; when the phosphoric acid content is too low, the polishing ability of the electrochemical etching solution is weakened, and it is impossible to effectively remove the tiny pits, oxide film, residual stress and other subtle defects on the sample surface. At the same time, the stability of the electrolyte will also decrease, all of which lead to a decrease in the calibration rate and resolution rate of EBSD sample preparation.

[0071] When the glycerol content in the electrochemical etching solution is higher than 8wt% or lower than 3wt%, the calibration rate and resolution rate of high-speed steel EBSD sample preparation are also reduced when the contents of other components remain unchanged. It is speculated that this may be because when the glycerol content in the electrochemical etching solution is too high, the complex formed by its combination with phosphoric acid increases the corrosion inhibition effect during the electrolytic polishing process, slows down the corrosion rate, and causes under-polishing; when the glycerol content in the electrochemical etching solution is too low, the complex formed by its combination with phosphoric acid is less, the corrosion inhibition effect is weakened, and over-corrosion occurs, such as pitting pits, which leads to a decrease in the calibration rate and resolution rate of EBSD sample preparation. Comparative Example 6

[0072] The difference between this comparative example and Example 3 is only the difference in electrolytic polishing parameters. The electrolytic polishing parameters of this comparative example are shown in Table 2, and the remaining parts not described are the same as those of Example 3.

[0073] Table 2 Electrolysis voltage / V <![CDATA[Current density / A / dm 2 > Electrolysis temperature / ℃ Calibration rate / % 15 10 30 75 3 2 30 80 8 6 10 85 8 6 40 77 From the results in Table 2, it can be seen that when the voltage of electropolishing exceeds 10V and the current density exceeds 8A / dm2 When the electrolytic voltage is lower than 5V and the current density is lower than 3A / dm 2 When the surface dissolution rate of high-speed steel decreases, the dissolution is uneven, and some parts are not completely polished, which makes it impossible to effectively remove the surface residual stress, resulting in a decrease in the calibration rate of EBSD sample preparation.

[0074] For high-speed steel, the suitable electrolytic polishing temperature range is around room temperature. When the electrolytic polishing temperature is higher than 35°C, the chemical reaction rate between the electrochemical etching solution and the high-speed steel surface is accelerated, the surface dissolution is accelerated, the dissolution is uneven, and point or strip corrosion occurs, resulting in a decrease in the calibration rate of EBSD sample preparation; when the electrolytic polishing temperature is lower than 25°C, the electrolytic polishing efficiency is low, the reaction activity of the electrochemical etching solution decreases, and the residual stress on the high-speed steel surface cannot be effectively removed, resulting in a decrease in the calibration rate of EBSD sample preparation.

Claims

1. An electrochemical etching solution for high-speed steel EBSD sample preparation, characterized in that: The electrochemical etching solution comprises the following components: hydrochloric acid, phosphoric acid, ferric chloride, lauryl alcohol polyoxyethylene ether, glycerol and water.

2. The electrochemical etching solution according to claim 1, characterized in that: When the electrochemical etching solution is used in the chemical mechanical polishing process of high-speed steel, the electrochemical etching solution also includes a nano-diamond aqueous suspension. In terms of weight percentage, the electrochemical etching solution includes the following components: 70wt% to 80wt% of the nano-diamond aqueous suspension, 2wt% to 10wt% of hydrochloric acid, 1wt% to 5wt% of phosphoric acid, 1wt% to 2wt% of ferric chloride, 0.1wt% to 0.5wt% of lauryl alcohol polyoxyethylene ether and 0.1wt% to 0.5wt% of glycerol, and the balance is water.

3. The electrochemical etching solution according to claim 2, characterized in that: The concentration of nano-diamonds in the nano-diamond water suspension is 2wt% to 5wt%; the particle size of the nano-diamonds is 10 to 60nm.

4. The electrochemical etching solution according to claim 1, characterized in that: When the electrochemical etching solution is used in the electrolytic polishing process of high-speed steel, the electrochemical etching solution includes the following components in weight percentage: 25wt% to 35wt% of hydrochloric acid, 20wt% to 40wt% of phosphoric acid, 5wt% to 10wt% of ferric chloride, 1wt% to 5wt% of lauryl alcohol polyoxyethylene ether and 3wt% to 8wt% of glycerol, and the balance is water.

5. The electrochemical etching solution according to claim 2, characterized in that: The volume ratio of the phosphoric acid to glycerol is (4-12):

1.

6. A method for preparing high-speed steel EBSD samples, characterized in that: The steps include: S1 Pre-grinding: Use diamond sandpaper to perform coarse grinding, fine grinding and fine grinding on the surface of the high-speed steel to be observed after wire cutting until the scratches on the surface are consistent; S2 chemical mechanical polishing: the high-speed steel treated in step S1 is subjected to chemical mechanical polishing rough polishing for 15 to 20 minutes using the electrochemical etching solution of claim 2, and then subjected to chemical mechanical polishing fine polishing for 30 to 40 minutes; S3 electrolytic polishing: placing the high-speed steel treated in step S2 in the electrochemical etching solution of claim 4, with the high-speed steel as the anode and the lead plate as the cathode, for electrolytic polishing for 10 to 20 seconds; S4 cleaning: The electropolished sample was ultrasonically cleaned in ethanol, then cleaned and dried with deionized water to obtain a high-speed steel EBSD sample.

7. The method for preparing high speed steel EBSD samples according to claim 6, characterized in that: The pre-grinding in step S1 is to use 1000 mesh, 2000 mesh, 3000 mesh, 4000 mesh and 5000 mesh diamond sandpaper to perform coarse grinding, fine grinding and fine grinding on the high-speed steel in sequence.

8. The method for preparing high speed steel EBSD samples according to claim 6, characterized in that: The particle size of the nano-diamond in the electrochemical etching solution used in the rough chemical mechanical polishing process in step S2 is 40-60 nm; the particle size of the nano-diamond in the electrochemical etching solution used in the fine chemical mechanical polishing process is 10-20 nm.

9. The method for preparing high speed steel EBSD samples according to claim 6, characterized in that: The rotation speed of the rough chemical mechanical polishing in step S2 is 200-300 rpm; the rotation speed of the fine chemical mechanical polishing is 100-150 rpm.

10. The method for preparing high speed steel EBSD samples according to claim 6, characterized in that: The voltage of electrolytic polishing in step S3 is 5-10V, and the current density is 3-8 A / dm 2 , the electrolytic polishing temperature is 25℃~35℃.