High-strength polyetherketoneketone fiber and preparation method based on molecular chain softening induction high densification
By using small-molecule chlorinated hydrocarbons and polar solvents to dissolve polyether ketone ketone during wet spinning, combined with multi-stage heat treatment, the molecular chain structure is softened, achieving high densification of polyether ketone ketone fibers and improving the fiber's mechanical and high-temperature resistance properties.
Patent Information
- Application Number
- CN202411255732.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
AI Technical Summary
Existing technologies make it difficult to achieve high densification of polyether ketone ketone fibers during wet spinning, resulting in numerous pores inside the fibers, which affects mechanical properties and high-temperature resistance.
Small molecule chlorinated hydrocarbons and polyether ketones are co-dissolved in fluorinated and/or chlorinated polar solvents. Through wet spinning and multi-stage heat treatment, the molecular chain structure is softened, and densification during the phase separation process is promoted, including static setting, multi-stage thermal stretching and heat setting treatment.
High-strength polyetherketone ketone fiber was prepared, with a density increased to 1.2-1.26 g/cm3, tensile breaking strength higher than 900 MPa, and thermal weight loss temperature higher than 450℃, significantly improving the mechanical properties and high-temperature resistance of the fiber.
Smart Images

Figure CN118996639A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-strength polyetherketoneketone fiber and a preparation method based on molecular chain softening-induced high densification, belonging to the technical field of high-performance fibers. Background Art
[0002] Thermoplastic fibers have been widely used in the fields of electronic information, transportation, aerospace, etc. due to their good plasticity, specific strength, fatigue resistance and impact resistance. However, traditional thermoplastic fibers made from polyester, polyamide, polyacrylonitrile, polyethylene, etc. have weak high temperature resistance and are greatly limited in high-end applications. For this reason, high-performance polymers such as polyphenylene sulfide, polytetrafluoroethylene and polyaryletherketone (PAEK) are used to develop high temperature resistant fibers. Among them, PAEK has attracted much attention due to its excellent mechanical properties, high temperature stability and chemical corrosion resistance due to its aromaticity and strong polarity.
[0003] At present, the preparation of PAEK fibers is mainly based on melt extrusion and its derivative processes (such as melt-blown spinning, melt electrospinning, etc.). However, due to the high melt viscosity and weak molecular chain mobility of PAEK, melt spinning is difficult to effectively control the microstructure of the fiber, and the preparation of high-performance fibers still faces many difficulties. In order to reduce the melt viscosity of PAEK, people have taken a variety of measures, such as optimizing the spinning temperature, adding lubricants, and polymer co-melt spinning, but the overall effect of these methods is limited. In contrast, wet spinning can effectively disentangle the molecular chains by dissolving, and then use the phase separation of polymer-solvent to induce polymer chain coagulation. It is a fiber preparation method that is easy to control the microstructure. For PAEK, solvents such as 4-phenylphenol, diphenyl sulfone, and 9-fluorenone can be used to achieve dissolution at high temperatures (≥200°C), but it is difficult to achieve efficient and stable continuous spinning. To this end, chemical modification of the PAEK molecular chain (such as grafting sulfonic acid groups, carboxylic acid groups or chloromethyl groups) can be used to achieve dissolution at room temperature, but this changes the molecular structure of PAEK and reduces its mechanical properties and high temperature resistance. How to achieve lossless dissolution spinning of PAEK has become a difficult problem at present. In recent years, it has been found that polyetherketoneketone (PEKK) in the PAEK family exhibits high molecular polarity due to its rich ketone groups, and can be dissolved losslessly in polar solvents containing fluorine and / or chlorine groups at room temperature. Based on this, Chinese invention patents ZL202111055042.1, CN 114232109A and ZL202210401927.0 disclose the technology of preparing PEKK fibers, PEKK / carbon fiber composite materials and composite powders by solution method (also known as wet method), and Chinese invention patent application 202310442837.0 further develops a method for preparing PEKK nanofiber membranes by electrospinning. At present, the wet spinning method can achieve the continuous preparation of PEKK fibers with a fiber diameter of 20 to 50 μm and a tensile breaking strength of 600 to 700 MPa. It also has excellent high temperature resistance and flame retardant properties.
[0004] However, there are still many pore structures inside the PEKK fibers prepared by ordinary wet spinning, which seriously affects the mechanical properties and high temperature resistance of the fibers. Therefore, how to make the fibers denser during the coagulation process is the key to improving their performance. At present, the main method used in wet spinning is to reduce the diffusion rate of the solvent to inhibit the formation of pores, such as lowering the coagulation bath temperature or adding solvent to the coagulation bath. However, due to the strong rigidity of the PEKK molecular chain and the easy formation of strong entanglements between the chains, traditional phase separation is difficult to fully realize the high-density coagulation of the molecular chains, and the pores in the fiber cannot be eliminated. For example, even if the phase separation rate is significantly reduced, the fiber density is only 0.9-1.0g / cm 3 .
[0005] Therefore, there is an urgent need in the art for a high-strength polyetherketoneketone fiber and a preparation method based on molecular chain softening-induced high densification. Summary of the invention
[0006] The purpose of the present invention is to solve the problem in the prior art of how to soften the PEKK rigid chain, thereby changing its phase separation process, achieving high densification of PEKK fibers, and then improving the mechanical properties of the fibers.
[0007] In order to achieve the purpose of solving the above-mentioned problems, the technical solution adopted by the present invention is to provide a high-strength polyetherketoneketone fiber and a preparation method based on molecular chain softening-induced high densification.
[0008] In a first aspect of the present invention, there is provided a method for preparing high-strength polyetherketoneketone fiber based on molecular chain softening-induced high densification, comprising the following steps:
[0009] Step 1, dissolving polyetherketoneketone and small molecular weight chlorinated hydrocarbon in a fluorine-based and / or chlorine-based polar solvent to obtain a uniform polyetherketoneketone solution, and using the solution as a spinning solution;
[0010] Step 2: Extruding the spinning solution obtained in step 1 through a spinneret for wet spinning, coagulating and forming in a first coagulation bath, removing the fluorine-based and / or chlorine-based polar solvents and retaining the small molecular weight chlorinated hydrocarbon reagents, and then collecting and winding to obtain the initially spun polyetherketoneketone fibrils;
[0011] Step 3: placing the initially spun polyetherketoneketone fibrils retaining small molecular weight chlorinated hydrocarbons obtained in step 2 in a closed space;
[0012] Step 4: subjecting the polyetherketoneketone fibrils after standing in step 3 to a second coagulation bath to remove residual small molecular weight chlorinated hydrocarbons, and then subjecting the polyetherketoneketone fibrils to high temperature drying to completely remove the small molecular weight chlorinated hydrocarbons, and then subjecting the polyetherketoneketone fibrils to winding to obtain initially spun polyetherketoneketone fibers;
[0013] Step 5: The initially spun polyetherketoneketone fiber obtained in step 4 is subjected to multi-stage heat drawing and heat setting, and then wound and collected to obtain polyetherketoneketone high-performance fiber.
[0014] Preferably, the molar ratio of the para-phenylene structure to the ortho-phenylene structure of the polyether ketone ketone in step 1 is 50:50 to 100:0; the particle size of the polyether ketone ketone powder is ≤300 μm; in the polyether ketone ketone solution, the mass ratio of small molecule chlorinated hydrocarbons to fluorine-based or chlorine-based polar solvents is 10:90, 20:80, 30:70, 40:60, preferably 10:90, 20:80, 30:70; the concentration of the obtained polyether ketone ketone solution is 5 to 25%, preferably 16 to 22%, and the dissolution temperature is 20 to 120°C, preferably 25 to 80°C.
[0015] Preferably, in step 1, the fluorine-based or chlorine-based polar solvent is specifically at least one of trifluoroacetic acid, dichloroacetic acid, trichloroacetic acid or p-chlorophenol; the small molecule chlorinated hydrocarbon is specifically at least one of dichloromethane or dichloroethane.
[0016] Preferably, in step 2, the wet spinning uses a spinneret aperture of 0.05 to 0.5 mm; the spinning parameters are: extrusion rate of 1 to 30 m / min, preferably 2 to 20 m / min; extrusion temperature of 20 to 100° C., preferably 25 to 80° C.
[0017] Preferably, the first coagulation bath in step 2 is water or a caustic solution, which is miscible with trifluoroacetic acid, dichloroacetic acid, trichloroacetic acid or p-chlorophenol, but not miscible with dichloromethane, dichloroethane, etc.; the coagulation bath temperature is 1 to 30°C, preferably 5 to 10°C; the ratio of the winding collection rate to the extrusion rate is 1.0 to 1.3, preferably 1.05 to 1.2; the time required for the molding is 20 to 120s.
[0018] Preferably, in step 3, the standing time is 1 to 24 hours, preferably 2 to 12 hours; the standing temperature is 10 to 30°C, preferably 15 to 25°C.
[0019] Preferably, in step 4, the second coagulation bath is ethanol, ether or acetone, preferably ethanol; the coagulation bath temperature is 10-30°C; the drying temperature is 100-180°C, preferably 110-150°C; the drying time is 0.5-3h, preferably 1-2h.
[0020] Preferably, the length of the hot zone for hot stretching in step 5 is 50 to 120 cm, preferably 60 to 100 cm, and the hot stretching adopts 4-stage hot stretching, and the specific process parameters are: the first-stage stretching temperature is 220 to 260° C., the stretching multiple is 1.5 to 3 times, the second-stage stretching temperature is 250 to 270° C., the stretching multiple is 1.5 to 2 times, the third-stage stretching temperature is 250 to 270° C., the stretching multiple is 1.5 to 2 times, and the fourth-stage stretching temperature is 260 to 290° C., and the stretching multiple is 1.2 to 2 times.
[0021] Preferably, the heat setting temperature in step 5 is 200-300° C., preferably 220-260° C.; the heat setting time is 0.5-3 h, preferably 0.5-2 h.
[0022] The second aspect of the present invention provides a high-strength polyetherketoneketone fiber prepared by the above method.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention is based on a breakthrough in the wet spinning technology of polyetherketoneketone, in which small molecule chlorinated hydrocarbons (such as dichloromethane or dichloroethane) and PEKK are dissolved together in a fluorine-based and / or chlorine-based polar solvent to obtain a spinning solution. The small molecule chlorinated hydrocarbons have a strong interaction with the PEKK molecules, which weakens the strength of the covalent bonds in the ketone group, thereby softening the rigid molecular chain of PEKK. At the same time, during the phase separation process, the strong capillary action brought by the small molecule promotes the high-densification coagulation of PEKK. This is different from the previous wet spinning process, in which the rigidity of the polyetherketoneketone molecular chain and the entanglement between the chains keep the fiber volume unchanged during the phase separation process, resulting in numerous pores in the fiber.
[0025] 2. Small molecular weight chlorinated hydrocarbons also reduce the phase separation rate, so that the spinning solution flow can achieve dense coagulation of the fiber in a pure water coagulation bath, simplifying the preparation process.
[0026] 3. The mass density of the polyetherketoneketone fiber prepared by the present invention is 1.2 to 1.26 g / cm 3 , tensile strength at break is higher than 900MPa, and thermal weight loss temperature is higher than 450℃. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of phase separation;
[0028] Figure 2 The spinning solution obtained in step 1 of Example 1;
[0029] Figure 3 The as-spun polyetherketoneketone fiber obtained in step 3 of Example 1;
[0030] Figure 4 This is a scanning electron microscope image of the cross section of the as-spun polyetherketoneketone fiber prepared in Example 1;
[0031] Figure 5 The heat-set polyetherketoneketone fiber obtained in step 5 of Example 1;
[0032] Figure 6 The mechanical test results of the polyetherketoneketone fiber prepared in Example 1;
[0033] Figure 7 The thermal gravimetric test results of the polyetherketoneketone fiber prepared in Example 1 in an air environment. DETAILED DESCRIPTION
[0034] In order to make the present invention more clearly understood, a preferred embodiment is described in detail with reference to the accompanying drawings as follows:
[0035] like Figure 1-4 As shown, the present invention provides a kind of.
[0036] Example 1
[0037] This embodiment provides a high-strength polyetherketoneketone fiber and a preparation method based on molecular chain softening-induced high densification, specifically comprising:
[0038] 1) First, prepare a polyetherketoneketone spinning solution. Dissolve dichloroethane in trifluoroacetic acid at a mass ratio of 20:80. Then dissolve polyetherketoneketone (T / I ratio of 60:40) in a mixed solution of trifluoroacetic acid and dichloroethane at room temperature (25°C) at a concentration of 20wt%, stirring at a speed of 1500rpm for 24h to obtain a uniform and stable spinning solution. Figure 2 shown.
[0039] 2) The polyetherketoneketone solution was injected into a pure water coagulation bath at room temperature using a spinneret with an aperture of 400 mm and a length of 60 cm. The coagulation bath temperature was 200 °C and the extrusion rate was 2 m / min. The coagulated fibers were led out of the coagulation bath through two guide rails and then wound and collected through two guide rails at a collection rate of 2.1 m / min. The time the fibers spent in the coagulation bath was 60 s.
[0040] 3) The collected polyetherketone fibrils retaining ethylene dichloride are placed in a closed environment at 25°C for 6 hours, and then the polyetherketoneketone fibrils after standing are taken from the reel through a guide roller into an ethanol bath to remove ethylene dichloride. The bath fiber spends 50 seconds in the coagulation bath, and the lead-out speed is 6 m / min; then the as-spun polyetherketoneketone fiber is obtained by drying and winding, the drying time is 1 hour, the drying temperature is 150°C, and the winding collection speed is 6 m / min. Figure 3 and 4 shown.
[0041] 4) The initially spun polyetherketone ketone fiber is led out from the reel, passed through the hot zone for heat drawing, and then collected on another reel. The length of the drawing hot zone is 80 cm, and four-stage (secondary) heat drawing is adopted. The specific process parameters are: the first-stage drawing temperature is 230°C, the drawing multiple is 2 times, the second-stage drawing temperature is 250°C, the drawing multiple is 2 times, the third-stage drawing temperature is 270°C, the drawing multiple is 1.5 times, and the fourth-stage drawing temperature is 280°C, and the drawing multiple is 1.5 times.
[0042] 5) putting the heat-stretched polyetherketoneketone fiber together with the roll into a hot oven for high-temperature heat setting treatment, the heat setting temperature is 260° C., the heat setting time is 1 h, and the heat-set polyetherketoneketone fiber is obtained, such as Figure 5 shown.
[0043] The polyetherketoneketone fiber obtained through the above steps has a uniform diameter of 39 μm and a mass density of about 1.29 g / cm 3, tensile strength at break 1020MPa, decomposition temperature above 450℃, such as Figure 6 and 7 shown.
[0044] Example 2
[0045] This embodiment provides a high-strength polyetherketoneketone fiber and a preparation method based on molecular chain softening-induced high densification, which specifically includes:
[0046] 1) First, a polyetherketoneketone spinning solution was prepared. Ethylene dichloride was first dissolved in trifluoroacetic acid at a mass ratio of 30:70; then, polyetherketoneketone (T / I ratio of 60:40) was dissolved in a mixed solution of trifluoroacetic acid and ethylene dichloride at room temperature (25°C) at a concentration of 20wt%, with a stirring speed of 1500rpm and a stirring time of 24h to obtain a uniform and stable spinning solution.
[0047] 2) A spinneret with an aperture of 0.5 mm and a length of 60 cm was used, and the rest of the operations were the same as step 2) in Example 1.
[0048] 3): Same as step 3) in Example 1.
[0049] 4) The initially spun polyetherketone ketone fiber is led out from the reel, passed through the hot zone for heat drawing, and then collected on another reel. The length of the drawing hot zone is 80 cm, and four-stage (secondary) heat drawing is adopted. The specific process parameters are: the first-stage drawing temperature is 240°C, the drawing multiple is 2 times, the second-stage drawing temperature is 260°C, the drawing multiple is 1.5 times, the third-stage drawing temperature is 270°C, the drawing multiple is 1.5 times, and the fourth-stage drawing temperature is 280°C, and the drawing multiple is 1.2 times.
[0050] 5) Same as step 5 in Example 1.
[0051] The polyetherketoneketone fiber obtained through the above steps has a uniform diameter of 69 μm and a mass density of about 1.27 g / cm 3 , tensile breaking strength 960MPa.
[0052] Example 3
[0053] This embodiment provides a high-strength polyetherketoneketone fiber and a preparation method based on molecular chain softening-induced high densification, specifically comprising:
[0054] 1) First, a polyetherketoneketone spinning solution was prepared. Ethylene dichloride was first dissolved in trifluoroacetic acid at a mass ratio of 2:8; then, polyetherketoneketone (T / I ratio of 50:50) was dissolved in a mixed solution of trifluoroacetic acid and ethylene dichloride at room temperature (25°C) at a concentration of 20wt%, with a stirring speed of 1500rpm and a stirring time of 24h to obtain a uniform and stable spinning solution.
[0055] 2): 2)-5) are the same as steps 2)-5) in Example 1.
[0056] The polyetherketoneketone fiber obtained through the above steps has a uniform diameter of 36 μm and a mass density of 1.26 g / cm 3 , tensile breaking strength 940MPa.
[0057] Example 4
[0058] This embodiment provides a high-strength polyetherketoneketone fiber and a preparation method based on molecular chain softening-induced high densification, specifically comprising:
[0059] 1) First, a polyetherketoneketone spinning solution was prepared. Dichloroethane was first dissolved in dichloroacetic acid at a mass ratio of 2:8; then polyetherketoneketone (T / I ratio of 50:50) was dissolved in a mixed solution of dichloroacetic acid and dichloroethane at 80° C. with a concentration of 20wt%, a stirring speed of 1500rpm, and a stirring time of 24h to obtain a uniform and stable spinning base.
[0060] 2): 2)-5) are the same as steps 2)-5) in Example 1.
[0061] The polyetherketoneketone fiber obtained through the above steps has a uniform diameter of 40 μm and a mass density of 1.2 g / cm 3 , tensile breaking strength 905MPa.
[0062] Comparative Example 1
[0063] Densification of PEKK fibers is achieved in the traditional way by lowering the coagulation bath temperature and adding solvent to the coagulation bath.
[0064] 1) preparing a polyetherketoneketone solution, dissolving polyetherketoneketone (T / I ratio of 50:50) in dichloroacetic acid at room temperature with a concentration of 13 wt %, stirring at a speed of 800 rpm, and stirring for 48 h to obtain a uniform and stable spinning solution.
[0065] 2) Using a spinneret with an aperture of 0.4 mm and a length of 60 cm, the polyetherketoneketone solution was injected into a coagulation bath composed of dichloroacetic acid and water at a temperature of 10°C (the mass ratio of dichloroacetic acid to water was 7:3) at room temperature, and the extrusion rate was 2 m / min. The fiber spent 50 s in the coagulation bath.
[0066] 3) The coagulated fiber is passed through two guide rails and then introduced into a coagulation bath composed only of water. The coagulation bath temperature is 25°C. The fiber is immersed in water for 100 seconds. The fiber is then dried and wound and collected through two guide rails to obtain the initially spun polyetherketoneketone fiber. The drying time is 60 seconds and the drying temperature is 100°C.
[0067] 4) The initially spun polyetherketone ketone fiber is led out from the reel, passed through the hot zone for heat drawing, and then collected on another reel. The length of the drawing hot zone is 80 cm, and three-stage (secondary) heat drawing is adopted. The specific process parameters are: the first-stage drawing temperature is 240°C, the drawing multiple is 2 times, the second-stage drawing temperature is 260°C, the drawing multiple is 1.5 times, and the third-stage drawing temperature is 270°C, and the drawing multiple is 1.5 times.
[0068] 5) The heat-stretched polyetherketoneketone fiber and the roll are placed in a hot oven for high-temperature heat setting treatment. The heat setting temperature is 260° C. and the heat setting time is 1 hour to obtain heat-set polyetherketoneketone fiber.
[0069] The polyetherketoneketone fiber obtained through the above steps has a uniform diameter of 45 μm and a mass density of 0.90 g / cm 3 , tensile breaking strength 560MPa.
[0070] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and equivalent changes made by using the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing high-strength polyetherketoneketone fiber based on molecular chain softening-induced high densification, characterized in that: The following steps are involved: Step 1, dissolving polyetherketoneketone and small molecular weight chlorinated hydrocarbon in a fluorine-based and / or chlorine-based polar solvent to obtain a uniform polyetherketoneketone solution, and using the solution as a spinning solution; Step 2: Extruding the spinning solution obtained in step 1 through a spinneret for wet spinning, coagulating and forming in a first coagulation bath, removing the fluorine-based and / or chlorine-based polar solvents and retaining the small molecular weight chlorinated hydrocarbon reagents, and then collecting and winding to obtain the initially spun polyetherketoneketone fibrils; Step 3: placing the initially spun polyetherketoneketone fibrils retaining small molecular weight chlorinated hydrocarbons obtained in step 2 in a closed space; Step 4: subjecting the polyetherketoneketone fibrils after standing in step 3 to a second coagulation bath to remove residual small molecular weight chlorinated hydrocarbons, and then subjecting the polyetherketoneketone fibrils to high temperature drying to completely remove the small molecular weight chlorinated hydrocarbons, and then subjecting the polyetherketoneketone fibrils to winding to obtain initially spun polyetherketoneketone fibers; Step 5: The initially spun polyetherketoneketone fiber obtained in step 4 is subjected to multi-stage heat drawing and heat setting, and then wound and collected to obtain polyetherketoneketone high-performance fiber.
2. The method for preparing high-strength polyetherketoneketone fiber based on molecular chain softening-induced high densification as claimed in claim 1, characterized in that: The polyetherketoneketone in step 1 has a molar ratio of para-phenylene structure to ortho-phenylene structure of 50:50 to 100:0; the particle size of the polyetherketoneketone powder is ≤300 μm; in the polyetherketoneketone solution, the mass ratio of small molecule chlorinated hydrocarbon to fluorine-based or chlorine-based polar solvent is 10:90, 20:80, 30:70, 40:60; the concentration of the obtained polyetherketoneketone solution is 5 to 25%, and the dissolution temperature is 20 to 120°C.
3. The method for preparing high-strength polyetherketoneketone fiber based on molecular chain softening-induced high densification as claimed in claim 1, characterized in that: In the step 1, the fluorine-based or chlorine-based polar solvent is specifically at least one of trifluoroacetic acid, dichloroacetic acid, trichloroacetic acid or p-chlorophenol; the small molecule chlorinated hydrocarbon is specifically at least one of dichloromethane or dichloroethane.
4. The method for preparing high-strength polyetherketoneketone fiber based on molecular chain softening-induced high densification as claimed in claim 1, characterized in that: In the step 2, the wet spinning adopts a spinneret aperture of 0.05 to 0.5 mm; the spinning parameters are: extrusion rate of 1 to 30 m / min, and extrusion temperature of 20 to 100°C.
5. The method for preparing high-strength polyetherketoneketone fiber based on molecular chain softening-induced high densification as claimed in claim 1, characterized in that: The first coagulation bath in step 2 is water or caustic solution, the coagulation bath temperature is 1-30° C., the ratio of the winding collection rate to the extrusion rate is 1.0-1.3; and the time required for the molding is 20-120 seconds.
6. The method for preparing high-strength polyetherketoneketone fiber based on molecular chain softening-induced high densification as claimed in claim 1, characterized in that: In step 3, the standing time is 1 to 24 hours, and the standing temperature is 10 to 30°C.
7. The method for preparing high-strength polyetherketoneketone fiber based on molecular chain softening-induced high densification as claimed in claim 1, characterized in that: In step 4, the second coagulation bath is ethanol, ether or acetone; the coagulation bath temperature is 10-30° C.; the drying temperature is 100-180° C.; and the drying time is 0.5-3 hours.
8. The method for preparing high-strength polyetherketoneketone fiber based on molecular chain softening-induced high densification as claimed in claim 1, characterized in that: The length of the hot zone for hot stretching in step 5 is 50-120 cm, and the hot stretching adopts 4-stage hot stretching. The specific process parameters are: the first-stage stretching temperature is 220-260°C, the stretching multiple is 1.5-3 times, the second-stage stretching temperature is 250-270°C, the stretching multiple is 1.5-2 times, the third-stage stretching temperature is 250-270°C, the stretching multiple is 1.5-2 times, and the fourth-stage stretching temperature is 260-290°C, and the stretching multiple is 1.2-2 times.
9. The method for preparing high-strength polyetherketoneketone fiber based on molecular chain softening-induced high densification as claimed in claim 1, characterized in that: The heat setting temperature in step 5 is 200-300° C., and the heat setting time is 0.5-3 hours.
10. A high-strength polyetherketoneketone fiber prepared by the method of any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of polymer hollow fiber membrane
CN105289319A
Continuous fiber reinforced polyaryletherketone composite material and preparation method thereof
CN110499012A
Method for preparing polyetherketoneketone fibers based on lossless dissolution wet method
CN114232109A
Ultrathin high-performance hollow fiber membranes
US6015516A
Films and membranes of poly(ARYL ketones) and methods of casting the same from solution
WO2012166340A1
Cited By
A method for preparing polyetherketoneketone composite powder based on rapid phase separation of high boiling point coagulant and efficient recovery of solvent
CN119751971A
Polyether ketone ketone fiber anti-adhesion porous spinning method
CN121610908A