Uniform high-rigidity graphene fiber and preparation method thereof
Through the swelling of graphene fibers and microwave-assisted thermal reduction treatment, the problem of low bending stiffness when the fiber increases the diameter is solved, high density and uniformity are achieved, and the mechanical properties of the fiber are improved. It is suitable for complex application environments .
Patent Information
- Application Number
- CN202411298301.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-18
AI Technical Summary
When the existing graphene fibers increase the diameter, they have low bending stiffness and uneven cross-sections, making them difficult to apply to complex stress-bearing environments, and the fibers are not dense enough, which affects performance.
By swelling the incompletely dried primary wire, the stepwise weakening swelling bath and microwave-assisted thermal reduction method can achieve full rearrangement and density improvement of the fiber sheet layer, combined with chemical reduction and multi-stage roller stretching, optimized Axial and radial structural uniformity of fibers.
Prepare uniform high-stiffness graphene fibers with diameters greater than 20 μm, with bending stiffness up to 1.02 N mm², tensile strength up to 2.5 GPa, density up to 1.8 g cm-3, high orientation, suitable for spacecraft skeletons and bioelectrodes, etc. field.
Smart Images

Figure CN118996679A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of graphene preparation, and in particular to a uniform high-rigidity graphene fiber and a preparation method thereof. Background Art
[0002] Graphene is a new material with a single-layer two-dimensional honeycomb lattice structure of carbon atoms connected by sp² hybridization. It has excellent mechanical, electrical, thermal and optical properties. By arranging graphene sheets tightly and orderly along one dimension, macroscopic high-performance graphene fibers can be prepared, which have important application prospects in aerospace, biosensing, smart fabrics and other fields. Although the mechanical strength of small-diameter (diameter ≤ 10 μm) graphene fibers can reach 3.2 GPa, the small diameter results in a fiber bending stiffness of ≤ 2×10 -5 N mm², not resistant to bending and compression, and difficult to apply in complex actual stress environments. One of the effective ways to improve the bending stiffness of graphene fibers is to increase the fiber diameter while ensuring the density and high orientation of the internal sheets. At present, the fiber diameter is mainly increased by increasing the diameter of the spinning head. However, this method faces many problems. For example, the double diffusion process of the gel fiber in the coagulation bath and the subsequent carbonization treatment will form a serious skin-core structure, and the internal sheets are looser and less dense than the skin; because the core graphene oxide sheets are subjected to weak shear force from the tube wall, the core sheets are poorly oriented and the bending stiffness is less than 6×10 -4 N mm²; In addition, the fiber radial and axial structures are not uniform, and there is a serious size effect, that is, as the axial and radial dimensions of the fiber increase, the fiber performance decreases sharply. Although there are currently coarse fibers integrated by tow stretching, there are still problems such as uneven cross-sections and insufficient density inside the fibers, which seriously affect the performance of large-diameter fibers. Summary of the invention
[0003] Aiming at the problems that the coarse fibers integrated by tow stretching in the prior art have uneven cross sections and the interior of the fibers is not dense enough, the present invention provides a method for preparing graphene fibers.
[0004] The present invention proposes for the first time to swell the spun silk that has not been completely dried, which solves the problem that the spun silk cannot be fully swelled and separated due to the tight stacking of the fully dehydrated and dried lamellae in the swelling bath of the finished silk, the lamellae rearrangement plasticity is poor, and there are still many wrinkles on the fiber surface, resulting in the inability to achieve complete adaptive bonding between the fibers. After the spun silk that has not been completely dried is immersed in the swelling bath, since the lamellae are in an incompletely stacked state, the graphene oxide sheets can achieve better solvent immersion between the sheets, which can induce the sheets to rearrange to the greatest extent. And the full immersion of the solvent causes the fiber to fully swell into a wrinkle-free state on the surface, and the surfaces between the fibers can fully bond, and the π-π stacking under the action of the van der Waals force is regenerated during the drying process, to obtain a large-diameter graphene oxide fiber with overall dense and high orientation.
[0005] Secondly, by adjusting the polarity of the swelling bath solution and setting up a multi-stage gradual weakening of the swelling bath, the uniformity and density of the axial and radial structures of the tow are optimized in the process of repeated wet-melt splitting, avoiding the decrease in the skin-core structure and stiffness caused by direct wet spinning. By stretching the chemical reduction bath and the special microwave-assisted thermal reduction method, a high reduction of the carbon-oxygen ratio ≥ 25 is achieved. The graphene fiber prepared by the method of the present invention has a diameter greater than 20 μm, a regular circular cross-section, uniform density, high orientation, high stiffness, a standard deviation of tensile strength of different diameters and test lengths ≤ 0.095, and a bending stiffness of 1.02 N mm². In addition, the preparation process is continuous and the wire collection efficiency is high. The prepared graphene fiber has the characteristics of large diameter, axial and radial uniformity, density, high bending stiffness, etc., and has extremely important application value in spacecraft skeletons, bioelectrodes, building materials, etc.
[0006] One of the technical solutions of the present invention is to provide a method for preparing uniform high-rigidity graphene fibers, comprising the following steps: (1) extruding a graphene oxide dispersion into a coagulation bath through a porous spinning head to obtain a primary graphene oxide filament bundle; (2) sending the primary graphene oxide filament bundle into a first swelling bath for swelling, pulling out and drying, and obtaining primary wet-melt graphene oxide fibers; (3) continuing to perform swelling baths for two or more times, performing swelling rearrangement, pulling out and drying, and obtaining uniform and dense graphene oxide fibers with sufficient lamellae orientation; the polarity of the swelling bath solvent is gradually weakened, thereby adjusting the degree of fiber swelling; (4) The graphene oxide fibers with sufficient flaky orientation are continuously fed into a chemical reduction bath and a microwave-assisted thermal reduction drum through rollers to obtain uniform high-rigidity graphene fibers.
[0007] Furthermore, the porous spinning head in step 1 has ≥10 holes, and the hole diameter is 60 μm-240 μm.
[0008] Furthermore, the coagulation bath described in step 1 is a poor solvent for graphene oxide and is miscible with the graphene oxide dispersion.
[0009] Further, the swelling bath includes one or more of ethanol, acetone, isopropanol, ethyl acetate, methanol, water, glycerol, propylene glycol, ethylene glycol, triethylene glycol, tetraethylene glycol, pentaethylene glycol, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, succinic acid, and acrylic acid.
[0010] Furthermore, the chemical reduction bath in step 4 includes one or more of acetic acid, trifluoroacetic acid, vitamin C, hydroiodic acid, and hydrazine hydrate.
[0011] Furthermore, the chemical reduction bath in step 4 is carried out in a chemical reduction tank, which is equipped with side-by-side multi-stage rollers to fully improve the stretching ratio and reduction time of the fiber. The stretching ratio is as high as 10%, and the carbon-oxygen ratio of the reduced fiber is ≥12, ensuring the high bending stiffness of the reduced fiber.
[0012] Furthermore, in step 4, the microwave-assisted thermal reduction cylinder has a temperature of 100°C-350°C and a microwave power of 100W-800W. The dual reducing effects of high temperature and microwaves further improve the reduction degree of the fiber. After reduction, the carbon-oxygen ratio of the fiber is ≥25, which further improves the bending stiffness.
[0013] Furthermore, the repeated wet-melt splitting process described in step 3 can gradually increase the drawing speed of the rollers, so that the fiber bundles can be stretched to a certain extent during the densification process, thereby improving the degree of orientation.
[0014] The second technical solution of the present invention is to provide a uniform high-rigidity graphene fiber prepared by the above preparation method.
[0015] The graphene fiber prepared by the present invention has a diameter of ≥20 μm, a standard deviation of tensile strength of different diameters and test lengths of ≤0.095, a bending stiffness of up to 1.02 N mm², a tensile strength of greater than 2.5 GPa, an elongation at break of 1%-2.5%, and a density of graphene fibers of different diameters greater than 1.8 g cm -3 , the orientation degree is greater than 8.5.
[0016] Compared with the prior art, the present invention has the following advantages: 1) Utilize the gradually weakened swelling process to repeatedly split by wet melting. Through the splitting and rearrangement process, the internal layer orientation is optimized to improve uniformity and density.
[0017] 2) The nascent fibers that have not been fully dried are immediately swollen on the continuous spinning line. After the nascent fibers are immersed in the swelling bath, the graphene oxide sheets can achieve better solvent penetration because the sheets are not completely stacked, which can induce sheet rearrangement to the greatest extent. The full penetration of the solvent causes the fibers to fully swell to a wrinkle-free state, and the surfaces between the fibers can fully fit together. During the drying process, π-π stacking under the action of van der Waals forces is regenerated, and large-diameter graphene oxide fibers with overall denseness and high orientation are obtained.
[0018] 3) Using a chemical reduction bath equipped with parallel multi-stage rollers and a special microwave-assisted thermal reduction cylinder, the fiber is continuously reduced to a high degree with a carbon-oxygen ratio of ≥ 25. The preparation and reduction process is continuously integrated, which is convenient for large-scale production.
[0019] 4) The prepared fiber can ensure high orientation and density of the internal layers when the diameter is arbitrarily increased. The fiber cross-section is regular and circular, and is uniform in the axial and radial directions. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the continuous preparation process.
[0021] Figure 2 This is the SEM image of the fiber cross section prepared in Example 1.
[0022] Figure 3 The strength of the fibers prepared in Example 1 varies with the length tested.
[0023] Figure 4 The fiber strength prepared in Example 1 varies with fiber diameter. DETAILED DESCRIPTION
[0024] The following examples are used to further illustrate the present invention, and their purpose is to illustrate the present invention and should not be construed as limiting the scope of the present invention. Unless otherwise specified, all parts by weight and weight percentages are used below.
[0025] The raw materials used in the present invention, unless otherwise specified, are conventional commercially available products; the methods used in the present invention, unless otherwise specified, are conventional methods in the art.
[0026] The embodiments of the present invention are further described below with reference to a plurality of embodiments.
[0027] It should be clear that the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0028] The wet fusion mentioned in the present invention refers to wet spinning fusion.
[0029] The swelling degree of the present invention refers to the ratio of the equivalent diameter of the graphene fiber after the fiber is swelled in a solvent to the equivalent diameter of the fiber before the fiber is swelled.
[0030] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0031] Embodiment 1: 1. 8 mg g -1 The DMF-phase graphene oxide spinning solution was loaded into a 100 ml syringe and stirred at a rate of 1 ml min -1 The graphene oxide filaments were pushed forward at a speed of 100 μm and squeezed into an ethyl acetate coagulation bath through a 100-hole multi-porous spinning head with a pore size of 100 μm. The coagulation time was 30 s. After being pulled out, they were fully dried in situ to obtain graphene oxide filament bundles. 2. The graphene oxide tow is fed into the first strong swelling bath through rollers, which is a mixed solution of ethanol and water in a ratio of 2:1 and a swelling degree of 250%. The tow is pulled out from the swelling bath and dried to obtain the initially wet-melted graphene oxide fiber; 3. The initially wet-melted graphene oxide fiber is sent into the second micro-swelling bath through a roller, which is a mixed solution of ethanol and water in a ratio of 3:1, with a swelling degree of 190% and a drafting rate increased to 1.05 times. The fiber undergoes a certain degree of splitting in the swelling bath, and the orientation and uniformity are optimized. The fiber is pulled out and dried to achieve secondary wet melting; 4. The fiber obtained in step 3 is continuously fed into the third micro-swelling bath through a roller, the ratio of ethanol to water is increased to 4:1, the swelling degree is 130%, and the drawing speed is increased to 1.1 times to continue to improve the fiber orientation and density.
[0032] 5. The fiber obtained in step 4 is continuously fed into the fourth micro-swelling bath through a roller, the ratio of ethanol to water is increased to 5:1, the swelling degree is 90%, and the drawing speed is increased to 1.2 times to obtain a highly oriented and dense wet-melt graphene oxide fiber.
[0033] 6. The wet melted graphene oxide fiber obtained in step 5 is sent into a mixed chemical reduction bath of acetic acid and trifluoroacetic acid in a ratio of 3:1 by rollers for continuous room temperature chemical reduction to obtain reduced graphene oxide fiber with a stretching ratio of up to 10% and a carbon-oxygen ratio of 12 after reduction.
[0034] 7. The reduced graphene oxide fiber is further fed into the microwave-assisted thermal reduction cylinder through a roller and thermally reduced under tension. The temperature of the thermal reduction cylinder is 100 °C and the microwave power is 100 W. Finally, uniform and dense graphene fibers with a diameter of 124 μm are collected on a roller with a diameter of 15 cm. The carbon-oxygen ratio of the fiber is 25 and the density is 1.87 g cm -3 .like Figure 3 As shown in the figure, as the test length of the obtained fiber increases from 0.5 cm to 10 cm, the mechanical strength can always be maintained above 2.5 GPa, and there is no obvious downward trend. The elongation at break is 2.5%, and the conductivity is 6.28×10 4 S m -1 , the bending stiffness is 1.02 N mm².
[0035] 8. By changing the number of holes in the porous spinning head in step 1 to 20, 40, 60, and 80, and keeping the other steps unchanged, uniform high-rigidity graphene fibers with different diameters can be obtained, with diameters of 26 μm, 52 μm, 73 μm, and 101 μm, respectively. The strength did not show a significant downward trend with the increase of diameter, and was maintained above 2.5 GPa. Figure 4 As shown, the density is basically the same; the conductivity is maintained at 6×10 4 S m -1 The bending stiffness increases with the increase of diameter. And with the increase of diameter, the orientation degree is maintained above 8.5.
[0036] Comparative Example 1 This comparative example is the same as Example 1, except that a large-aperture single-hole spinning head with apertures of 610 μm, 840 μm, 1000 μm, 1100 μm, and 1250 μm is directly used for spinning.
[0037] 1. 8 mg g -1 The DMF phase graphene oxide dispersion is squeezed into an ethyl acetate coagulation bath from a large-diameter single-hole spinning head, and then pulled out and fully dried to obtain primary graphene oxide coarse fibers.
[0038] 2. The graphene oxide coarse fibers obtained in step 1 are sent into a swelling bath of ethanol and water in a ratio of 3:1 by rollers, and the stretching ratio is 1.05, which is consistent with step 3 of example 1.
[0039] 3. The fiber obtained in step 2 is continuously fed into a swelling bath of ethanol and water in a ratio of 4:1 through a roller, and the stretching ratio is 1.1, which is consistent with step 2 of example 1.
[0040] 4. The chemical reduction treatment process is the same as step 5 of Example 1.
[0041] 5. Similarly, the chemically reduced fibers were placed in a microwave-assisted thermal reduction cylinder at a temperature of 300 °C and a microwave power of 500 W. The resulting fibers had irregular cross-sectional morphology, with equivalent diameters of 23 μm, 49 μm, 82 μm, and 106 μm. The density was only 1.56 g cm -3 The maximum orientation degree is only 7.2, the maximum strength is only 560 MPa, the elongation at break is 3%-6%, and the conductivity is only 2.2×10 3 S m -1 , bending stiffness ≤3.9×10 -3 N mm², the various performance indicators show a sharp decrease trend with the increase of diameter, and the various performance indicators are significantly lower than those in Example 1.
[0042] Comparative Example 2 This comparative example is the same as Example 1, except that there is no repeated wet-melt splitting process.
[0043] 1. Same as step 1 in example 1.
[0044] 2. The obtained graphene oxide filament bundle is sent into a swelling bath of ethanol and water in a ratio of 2:1 through a roller, with a drawing ratio of 1.1 times, and the graphene oxide crude fiber is obtained after drying and wet melting.
[0045] 3. The chemical reduction and thermal reduction processes were the same as step 6 of Example 1. The final fiber cross section was irregular, with many voids and poor compactness, and a density of 1.71 g cm -3 , the orientation degree is 7.9, the strength is only 832 MPa, the elongation at break is 3%, and the electrical conductivity is 0.97×10 4 S m -1 , the bending stiffness is 0.11 N mm².
[0046] Embodiment 2: 1. Add 5 mg g -1 The DMSO phase graphene oxide spinning solution was loaded into a 50 ml syringe and stirred at a rate of 0.8 ml min -1 The filaments were pushed forward at a speed of 1000 μm and squeezed into an acetone coagulation bath through a 50-hole porous spinning head with an aperture size of 120 μm. The time in the coagulation bath was 25 s. The filaments were pulled out from the coagulation bath and fully dried in situ to obtain primary graphene oxide filament bundles.
[0047] 2. The obtained graphene oxide filament bundle is sent into a swelling bath consisting of a mixed solution of acetic acid and ethylene glycol through a roller, with a ratio of 3:1 and a swelling degree of 210%, and then pulled out from the swelling bath and dried.
[0048] 3. Continue to send it into the second swelling bath through rollers. The ratio of acetic acid to water is 4:1, the swelling degree is 175%, and the stretching ratio in this process is 1.15 times. Pull it out from the second swelling bath and dry it to achieve the second wet melting.
[0049] 4. Continue to pass through the third swelling bath, the ratio of acetic acid and water increases to 5:1, the swelling degree is 110%, and the stretching ratio is further increased to 1.25 times. Pull out from the third swelling bath and dry to achieve the third wet melting. The orientation and density of the fiber are further increased.
[0050] 5. Finally, the obtained wet melt fiber is sent into a pure acetic acid solvent through a roller for pure plastic stretching, and the stretching ratio is increased to 1.3 times. After drying, highly oriented and highly densified graphene oxide coarse fibers are obtained.
[0051] 6. The fiber obtained in step 5 is further fed into hydrazine hydrate through a roller, and after being pulled out and dried, chemically reduced graphene fiber is obtained. The graphene fiber stretching ratio is as high as 10%, and the carbon-oxygen ratio of the reduced fiber is 12.
[0052] 7. The chemically reduced graphene fiber was sent into a microwave-assisted thermal reduction cylinder with a reduction temperature of 280 °C and a microwave power of 800 W for thermal reduction under tension. Finally, uniform graphene coarse fibers were obtained with a carbon-oxygen ratio of 31, a diameter of 82 μm, and a density of 1.89 g cm -3 , orientation degree is 8.8, within the test length range of 0.5 cm-10 cm, the strength standard deviation is ≤0.082, and all are above 2.5 GPa, the elongation at break is 2.1%, and the conductivity is 9.73×10 4 S m -1 , bending stiffness is 0.2 N mm².
[0053] Embodiment 3: 1. Add 15 mg g -1 The NMP phase graphene oxide spinning solution was loaded into a 100 ml syringe and stirred at 0.5 ml min. -1 The graphene oxide filaments were pushed forward at a speed of 200 μm through a porous spinning head with 20 holes and an aperture size of 200 μm and squeezed into a n-hexane coagulation bath. The time in the coagulation bath was 20 s. The filaments were pulled out from the coagulation bath and fully dried in situ to obtain primary graphene oxide filament bundles.
[0054] 2. The obtained graphene oxide filament bundle is sent into a swelling bath consisting of a mixed solution of ethanol and ethylene glycol through a roller, with a ratio of 4:1 and a swelling degree of 180%, and then pulled out from the swelling bath and dried.
[0055] 3. Continue to send it into the second swelling bath through rollers. The ratio of ethanol to ethylene glycol is 5:1, the swelling degree is 160%, and the stretching ratio in this process is 1.15 times. Pull it out from the second swelling bath and dry it to achieve the second wet melting.
[0056] 4. Continue to pass through the third swelling bath, the ratio of ethanol and ethylene glycol increases to 6:1, the swelling degree is 130%, and the stretching ratio is further increased to 1.25 times. Pull out from the third swelling bath and dry to achieve the third wet melting. The orientation and density of the fiber are further increased.
[0057] 5. Finally, the obtained wet melt fiber is sent into a pure acetic acid solvent through a roller for pure plastic stretching, and the stretching ratio is increased to 1.3 times. After drying, highly oriented and highly densified graphene oxide coarse fibers are obtained.
[0058] 6. The fiber obtained in step 5 is further fed into the sodium ascorbate solution through a roller, and after being pulled out and dried, chemically reduced graphene fibers are obtained. The graphene fiber stretching ratio is as high as 10%, and the carbon-oxygen ratio of the reduced fiber is 12.
[0059] 7. The chemically reduced graphene fiber was sent into a microwave-assisted thermal reduction cylinder with a reduction temperature of 350 °C and a microwave power of 400 W for thermal reduction under tension. The final result was uniform graphene coarse fiber with a carbon-oxygen ratio of 27, a diameter of 56 μm, and a density of 1.9 g cm -3 , the orientation degree is 9.1, the strength standard deviation is ≤0.072 within the test length range of 0.5 cm-10 cm, and it is maintained above 2.6 GPa, the elongation at break is 1%, and the conductivity is 3.96×10 4 S m -1 , bending stiffness is 0.06 N mm².
[0060] The above embodiments describe in detail the structure, features and effects of the present invention. The above are only preferred embodiments of the present invention. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which do not exceed the scope covered by the specification, should be within the protection scope of the present invention.
[0061] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.
Claims
1. A method for preparing uniform high-rigidity graphene fibers, characterized in that: The following steps are involved: (1) extruding a graphene oxide dispersion into a coagulation bath through a porous spinning head to obtain a primary graphene oxide filament bundle; (2) sending the primary graphene oxide filament bundle into a first swelling bath for swelling, pulling out and drying, and obtaining primary wet-melt graphene oxide fibers; (3) continuing to perform swelling baths for two or more times, performing swelling rearrangement, pulling out and drying, and obtaining uniform and dense graphene oxide fibers with sufficient lamellae orientation; the polarity of the swelling bath solvent is gradually weakened; (4) The graphene oxide fibers with sufficient flaky orientation are continuously fed into a chemical reduction bath and a microwave-assisted thermal reduction drum through rollers to obtain uniform high-rigidity graphene fibers.
2. The preparation method according to claim 1, characterized in that: The porous spinning head in step 1 has ≥10 holes, and the hole diameter is 60 μm-240 μm.
3. The preparation method according to claim 1, characterized in that: The swelling bath includes one or more of ethanol, acetone, isopropanol, ethyl acetate, methanol, water, glycerol, propylene glycol, ethylene glycol, triethylene glycol, tetraethylene glycol, pentaethylene glycol, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, succinic acid, and acrylic acid.
4. The preparation method according to claim 1, characterized in that: The chemical reduction bath in step 4 includes one or more of acetic acid, trifluoroacetic acid, vitamin C, hydroiodic acid, and hydrazine hydrate.
5. The preparation method according to claim 1, characterized in that: In step 4, the microwave-assisted thermal reduction cylinder has a temperature of 100°C-350°C and a microwave power of 100W-800W.
6. A uniform high-rigidity graphene fiber prepared by the method according to any one of claims 1 to 5.
7. The uniform high-rigidity graphene fiber according to claim 6, characterized in that: Fiber diameter ≥20 μm.
8. The uniform high-rigidity graphene fiber according to claim 6, characterized in that: The graphene fiber density is greater than 1.8 g cm -3 .
Citation Information
Patent Citations
Method for preparing high-elongation graphene fiber
CN113322546A
Method for preparing graphene oxide fibers, graphene fibers or their composite fibers by using wet spinning induced by electric field
KR1020180019130A
Self-fused graphene fiber and method of preparing the same
US20200040519A1