Preparation method of novel mixed raw material wood pulp
By combining semi-chemical pulping in raw material structure matching and process adjustment, the problem of lack of mixed raw material wood pulp in the market is solved, the cost of paper mills is reduced, product quality and market recognition are improved, and the profit of paper companies is achieved promote.
Patent Information
- Application Number
- CN202410361266.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There are fewer new mixed raw material wood pulp products on the market, resulting in high prices of conventional broad-leaf wood pulp and conifer wood pulp, resulting in low purchasing intentions of downstream customers, and papermaking companies face difficulties in purchasing raw materials and profit difficulties.
By developing processes such as combining different raw material structures, controlling the slurry concentration of pressure screens, adjusting the gas phase temperature, liquid ratio and alkali quantity of the cooking tower, a new low-cost mixed raw material wood pulp is produced, combining semi-chemical pulping and appropriate Karber value control ensures the cleanliness and strength indicators of the slurry.
It has achieved the reduction of paper mill production costs, increased profits, and provided mixed wood pulp with high quality and low price, gained market recognition, reduced manufacturing costs and improved company efficiency.
Smart Images

Figure CN118996889A_ABST
Abstract
Description
Technical Field
[0001] The patent of this invention relates to the field of pulping and papermaking technology, especially the research and development of new mixed raw material wood pulp on the market. Background Art
[0002] The wood pulp products circulating in the market are mainly conventional hardwood pulp and coniferous pulp, and there are fewer wood pulp products with mixed raw materials. Conventional hardwood pulp products and coniferous pulp products are sold at high prices, and the production costs are too high for downstream customers, resulting in low purchasing willingness and product sales that are not as good as expected. In the context of the waste ban, papermaking companies that mainly rely on waste paper for production often face problems such as difficulties in purchasing raw materials, too low intensity indicators of purchased waste paper due to multiple recycling, and difficulties in corporate profitability. Therefore, it is necessary to develop a medium- and low-grade mixed raw material wood pulp. Summary of the invention
[0003] The purpose of the present invention is to solve the above problems and develop a new type of mixed raw material wood pulp with low cost and meeting market demand, which is beneficial to reduce the production cost of paper mills, increase the profits of paper mills, and achieve a win-win situation.
[0004] To achieve the above-mentioned purpose, the technical scheme of the present invention is to develop different raw material structure matching ratios, control the appropriate pressure screen pulp concentration, adjust the key processes such as the gas phase temperature, liquid ratio, and alkali dosage of the cooking tower, so as to realize the production of new mixed raw material wood pulp.
[0005] The raw material matching ratio, the broadleaf wood chips and the bamboo chips are matched with a suitable feeding ratio, the pulping is carried out by using a semi-chemical method, and the appropriate Kappa number and spraying concentration are controlled.
[0006] The above-mentioned control of the appropriate pressure screen feed concentration allows the coarse pulp to enter the pressure screen section after passing through the high-concentration desander. The appropriate feed concentration can most efficiently separate the good pulp from the slag pulp, and can further improve the cleanliness of the pulp. This ensures that downstream customers will not have paper defects due to pulp problems during use, which will affect production operations and the quality of finished products.
[0007] The adjustment of the gas phase temperature, liquid ratio, alkali amount, etc. of the cooking tower is based on the structural design of the cooking tower, the type of pulp produced, and the cooking temperature. On the basis of the original type of pulp produced, the production operation is stabilized, the cooking temperature is appropriately adjusted, the cooking liquid ratio and alkali amount parameters are adjusted according to different ratios of raw materials, and further fine-tuning is performed according to the strength indicators of the finished pulp until high-quality wood pulp with qualified strength indicators is produced. DETAILED DESCRIPTION
[0008] The raw material matching ratio is as follows: the broadleaf wood chips are fed through a wood chip yard belt, and the bamboo chips are fed through a bamboo chip spiral according to a fixed ratio. The mixed raw materials pass through a wood chip metering spiral and a prepreg tower for steaming, and finally enter a cooking tower for pulping using a semi-chemical method, and the Kappa number is controlled at 80-100.
[0009] The control of the appropriate pressure screen feed concentration is one of the main factors affecting the screening efficiency, but in actual production, the feed concentration often fluctuates. When the feed concentration increases, the feed volume also increases accordingly, and the good pulp and coarse slag cannot be effectively separated, which will increase the amount of good pulp in the tailings, increase the amount of slag discharge, and easily cause the board to stick, so the amount of water spraying must be increased. Therefore, the screening efficiency is highest and the screening effect is relatively best when the feed concentration is controlled between 2.8% and 3.2%.
[0010] The adjustment of the gas phase temperature, liquid ratio, alkali amount, etc. of the cooking tower is based on the structural design of the cooking tower, the type of pulp produced, and the cooking temperature. On the basis of the original type of pulp produced, the production operation is stabilized, the cooking temperature is appropriately lowered, the liquid ratio of the upper, middle and lower parts is adjusted, and fine-tuning is performed according to the strength index of the finished pulp until high-quality wood pulp with qualified strength indicators is produced.
[0011] The characteristic of this technical solution is that it is based on hardwood pulp and makes slight adjustments. It can reduce the company's production costs while keeping the strength indicators unchanged, optimize the company's product structure, provide downstream customers with high-quality and low-cost mixed wood pulp, reduce the manufacturing costs of papermaking enterprises, and indirectly improve the profitability of paper mills. While gaining recognition from market customers, it also improves the company's benefits.
[0012] The new mixed raw material wood pulp produced by the present invention has been widely recognized in the market, with a production cost reduced by about 32 yuan / ton, a monthly output of about 22,500 tons, and a cost of about 720,000 yuan / month.
[0013] The above technical solutions only reflect the preferred technical solutions of the present invention. Any changes that may be made to certain parts thereof by technicians in this technical field reflect the debugging and optimization of the present invention and fall within the protection scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is the process flow chart of the new mixed raw material wood pulp preparation method described in the patent of this invention: The mixed raw materials enter the wood chip metering screw through the wood chip conveyor belt, and are steamed in the pre-preg tower and cooked in the cooking tower. The obtained coarse pulp is further refined by the high-concentration mill, sent to the spray tower, desandered and de-slag treated, and then enter the vacuum pulp washer and double-roll pulp washer for pulp washing and squeezing. Then, according to the needs of customers, it is decided whether to load the loose pulp on the ground or squeeze it through the wet pulp machine, and it is cut, packaged, weighed and offline according to different needs.
Claims
1. A method for preparing a new type of mixed raw material wood pulp, which mainly includes the research and development of the process aspects such as the change of raw material structure, the optimization of the cooking process, the adjustment of the pressure screen pulp concentration, the washing factor of the pulp washer and other related parameters, and is characterized in that Adjust the proportion of raw materials, control the appropriate pressure screen pulp concentration, adjust the gas phase temperature, liquid ratio, alkali amount and other key processes in the cooking tower to produce a new type of mixed raw material wood pulp.
2. The method for preparing a novel mixed raw material wood pulp according to claim 1, characterized in that The mixed wood pulp with qualified strength index is produced using raw materials such as bamboo chips and hardwood chips.
3. The method for preparing a novel mixed raw material wood pulp according to claim 1, characterized in that The gas phase temperature, liquid ratio, alkali dosage, etc. of the cooking tower should be properly adjusted to produce a new type of mixed raw material wood pulp.
4. According to the method for preparing a novel mixed raw material wood pulp according to claim 1, the mixed raw material wood pulp mainly uses hardwood chips and bamboo chips, which can be sold as finished pulp and used for paper machines after a series of treatments. The main process flow is as follows: Hardwood chips → chip metering screw → prepreg tower → cooking tower → high-consistency refiner → blow tower → high-consistency desander → pressure screen → vacuum pulp washer → double-roll press pulp washer → wet pulp loading and transportation / medium-consistency pulp tower → low-consistency disc grinding → post-grinding pulp tower → paper machine workshop disc grinding → paper machine pulping.
5. According to the method for preparing a novel mixed raw material wood pulp of claim 1, bamboo chips are fed into the pulp mill as one of the raw materials according to a certain proportion, and the main process flow is as follows: Bamboo chips are fed into the screw feeder according to the specified proportion → wood chip metering screw → prepreg tower → cooking tower → high-consistency refiner → blow tower → high-consistency desander → pressure screen → vacuum pulp washer → double-roll press pulp washer → wet pulp loading and transportation / medium-consistency pulp tower → low-consistency disc grinding → post-grinding pulp tower → paper machine workshop disc grinding → paper machine pulping.
Citation Information
Patent Citations
Preparation method for bamboo wood dissolving pulp
CN102352572A
Hybrid pulping and papermaking technology
CN106223094A
Method for producing semi-chemical pulp on large scale by utilizing forest waste
CN112431050A
Antibacterial soft toilet paper and preparation method thereof
CN113338075A
Method for making high-grade packaging paper by mixing and pulping high-calorie pulp and waste paper
CN116536968A