Super-strong water-resistant paper and preparation method thereof

Through the dense structure of twisted and entangled microfibers and in-situ regenerated nanofibers, combined with two-step treatment solution treatment technology, the existing water-resistant paper process is solved, and the high cost of high humidity strength and water resistance are achieved. , has wide application prospects.

CN118996906AActive Publication Date: 2024-11-22NANJING UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411262752.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-22
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The existing water-resistant paper has complex processes, high production costs and is not environmentally friendly, which limits its application and promotion, and is difficult to maintain strength in water for a long time.

Method used

The dense structure consisting of twisted and tangled microfibers and in-situ regenerated nanofibers is adopted. The cellulose paper is treated through two-step treatment solution to form a hydrated ion pair dipole compound, destroying the hydrogen bond structure of the fibers, and causing the fibers to expand, shrink and twist. Increase the bonding point to form a dense membrane structure to block moisture penetration.

Benefits of technology

It significantly improves the wet tensile strength and water resistance of the paper, maintains high humidity strength, reduces production costs, and realizes environmentally friendly water-resistant paper preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996906A_ABST
    Figure CN118996906A_ABST
Patent Text Reader

Abstract

The invention discloses super-strong water-resistant paper and a preparation method thereof.The super-strong water-resistant paper comprises micron fibers and in-situ regenerated nanofibers which are twisted and entangled, and the twisted and entangled structure of the micron fibers cannot lose strength due to the fact that hydrogen bonds are opened; the in-situ regenerated nanofibers form a compact membrane structure to tightly wrap the joints of the micron fibers; the preparation method of the waterproof paper comprises the following steps: treating cellulose paper by using concentrated alkali, so that fibers of the cellulose paper are twisted and entangled from a tiled and lapped structure, and the mutual locking and interaction are obviously improved; furthermore, fine fibers on the surfaces of the fibers are dissolved and regenerated in situ, so that the overall binding sites of the fibers are obviously increased, and the interaction is further enhanced. According to the invention, the problem of how to keep excellent water resistance of paper under the condition of not adding any other materials is solved. Based on the bonding effect of twisted and entangled fibers and regenerated fibers, the wet strength of the paper is greatly improved, and the paper has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to water-resistant paper and a preparation method thereof, and in particular to super-strong water-resistant paper and a preparation method thereof. Background Art

[0002] In the current social environment, plastic pollution and plastic crisis have become hot topics of global concern. The extensive use of plastic products has led to environmental pollution, ecological damage and health risks, and an environmentally friendly material that can replace plastic is urgently needed. Paper, as a degradable and environmentally friendly material, has great potential to replace plastic, but its poor water resistance limits its application and development. Improving the water resistance of paper so that it can work in water for a long time and maintain good strength, so that it can be applied to more fields, is an urgent problem to be solved.

[0003] A lot of research has been done on this issue. It mainly includes introducing hydrophobic additives during paper preparation or coating the surface of paper with waterproofing agents after paper preparation to enhance the water resistance of paper. In addition, by modifying, regenerating, and cross-linking the fibers, the stability of the fibers in water environments can be improved, further enhancing the performance of super water-resistant paper.

[0004] However, there are some challenges in the existing water-resistant paper preparation methods, such as complex processes, high production costs, and environmental issues, which limit the application and promotion of super water-resistant paper. Therefore, it is of great research significance to propose innovative solutions to these challenges and to develop paper materials with excellent water-resistant properties. Summary of the invention

[0005] Purpose of the invention: The present invention aims to provide a super water-resistant paper with excellent water-resistant performance, and the present invention also aims to provide a method for preparing the super water-resistant paper.

[0006] Technical solution: The super water-resistant paper of the present invention is a dense structure composed of twisted and entangled micron fibers and in-situ regenerated fibers. The twisted and entangled structure of the micron fibers will not lose strength due to the opening of hydrogen bonds. The in-situ regenerated nanofibers fill the micron fibers and connect them closely. The regenerated nanofibers form a dense membrane structure to tightly wrap the connection between the micron-level fibers, effectively blocking the penetration of water and further improving the water resistance of the paper.

[0007] Preferably, the thickness of the super water-resistant paper is 50 to 200 μm, and the density is 1.0 to 1.4 g·cm -3 .

[0008] Preferably, the wet tensile strength of the super water-resistant paper can reach 2.85 to 9.5 KN / m, the dry tensile strength can reach 7.6 to 11.4 KN / m, and the wet strength retention rate can reach 25% to 83%.

[0009] The method for preparing the super water-resistant paper comprises the following steps:

[0010] The cellulose paper is immersed in a treatment solution A, treated with alkali and washed to obtain a first intermediate; the treatment solution A is one or more of a sodium hydroxide solution, a calcium hydroxide solution and a potassium hydroxide solution;

[0011] The first intermediate is immersed in a treatment solution B to dissolve part of the fiber to obtain a second intermediate; the treatment solution B is one of an alkali / urea mixed solution, a lithium chloride / NN dimethylacetamide solution, an N-methylmorpholine-N-oxide solution, an ion solution, and a cuprammonia solution;

[0012] The second intermediate is washed and dried to obtain super water-resistant paper.

[0013] During the concentrated alkali treatment, the hydrated ion-dipole compounds formed penetrate into the amorphous and crystalline regions inside the cellulose fibers, forming hydrogen bonds with the cellulose molecules, changing the crystal structure, destroying the cell walls of the plant cells, and causing the fibers to swell, shrink, and twist. Furthermore, the fine fibers on the fiber surface are partially dissolved and regenerated in situ, greatly increasing their binding sites. Even if they are not twisted or entangled, the fibers can be tightly bound, further enhancing the interaction between the fibers and improving the water resistance of the paper.

[0014] Preferably, the source of cellulose in the cellulose paper includes but is not limited to woody plants, vines or herbaceous plants.

[0015] Preferably, the concentration of the treatment solution A is 1% to 20%, and the treatment temperature is 0 to 60°C.

[0016] Preferably, the mass ratio of the absolute dry cellulose paper to the treatment solution A is 1 to 5:30, and the treatment method of the treatment solution A comprises: soaking in the treatment solution A at 0 to 60° C. for 10 min to 5 h, and washing with water after the treatment. In this step, the cellulose paper is treated with concentrated alkali to change its fibers from a flat overlapping structure to a twisted, tangled, and interlocked structure.

[0017] Preferably, the treatment temperature of the B treatment solution is -20 to 170° C., and the treatment time is 5 min to 5 h.

[0018] Preferably, the second intermediate obtained after treatment with the treatment solution B needs to be left to stand for 1 to 30 minutes.

[0019] Preferably, the drying method includes but is not limited to air drying at room temperature, oven drying, hot press drying and the like, and the drying temperature is 20-120°C.

[0020] Preferably, during the washing process of the sample in step (3), the addition of the washing reagent destroys the dissolution system of the fiber and regenerates the fiber.

[0021] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the water-resistant paper has a higher wet strength of the paper, and the two-step treatment of cellulose by solution A and solution B has a synergistic effect on the improvement of the wet strength and water resistance of the paper. The regenerated nanofibers in the obtained water-resistant paper form a dense membrane structure that tightly wraps the micron-level fiber joints, effectively blocking the penetration of water and improving the water resistance of the paper. The present invention solves the problem of how to keep the excellent water resistance of the paper without adding any other materials. Based on the bonding effect of the twisted and entangled fibers and the regenerated fibers, the wet strength of the paper is greatly improved, and it has a wide range of application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a scanning electron microscope cross-sectional morphology of the twisted and tangled fibers of the super water-resistant paper prepared in Example 1 fully filled with regenerated cellulose;

[0023] Figure 2 This is the SEM image of the base paper;

[0024] Figure 3 This is the SEM image of the water-resistant paper prepared in Comparative Example 1;

[0025] Figure 4 This is the SEM image of the water-resistant paper prepared in Comparative Example 2;

[0026] Figure 5 This is a diagram of the wet tensile strength of the water-resistant paper prepared in base paper, Example 1, Comparative Example 1, and Comparative Example 2. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0028] Example 1

[0029] like Figure 1 As shown, a super water-resistant paper and a preparation method thereof, the super water-resistant paper comprises twisted and entangled micron fibers and in-situ regenerated nanofibers. The twisted and entangled structure of the micron fibers does not lose strength due to the opening of hydrogen bonds, and the in-situ regenerated nanofibers fill the micron fibers and connect them closely.

[0030] The preparation method of the above-mentioned super water-resistant paper is as follows:

[0031] (1) removing lignin, hemicellulose, etc. from the wood, extracting cellulose and preparing cellulose paper. The cellulose paper is immersed in an 18% sodium hydroxide solution, the mass ratio of the cellulose paper to the sodium hydroxide solution is 1:30, heated at 50° C. for 30 minutes, and washed with water to obtain a first intermediate;

[0032] (2) immersing the above-mentioned partially lignin-removed bamboo material in a NN dimethylacetamide solution, placing it in a 160°C environment to fully react for 20 minutes, then cooling it to 105°C, adding lithium chloride and heat-treating it for 30 minutes, the mass ratio of lithium chloride to NN dimethylacetamide solution is 1:10, and standing it for 10 minutes to obtain a second intermediate;

[0033] (3) The second intermediate was washed with anhydrous ethanol and placed in a hot press at 60°C and 20 MPa until completely dried.

[0034] The obtained super strong water-resistant paper has a thickness of 50 μm, a dry tensile strength of up to 11.4 KN / m, a wet tensile strength of up to 6.5 KN / m, and a wet strength retention rate of 58.3%.

[0035] Example 2

[0036] (1) removing lignin, hemicellulose, etc. from the wood, extracting cellulose and preparing cellulose paper. The cellulose paper is immersed in a 10% calcium hydroxide solution, the mass ratio of the cellulose paper to the calcium hydroxide solution is 2:30, heated at 30°C for 5 hours, and washed with water to obtain a first intermediate;

[0037] (2) immersing the first intermediate in a copper ammonia solution and placing it in an environment of 80° C. to fully react for 2 hours to obtain a second intermediate;

[0038] (3) The second intermediate is washed with anhydrous ethanol and dried to obtain super water-resistant paper.

[0039] The thickness of the obtained super strong water-resistant paper is 120 μm, the dry tensile strength can reach 8.55 KN / m, the wet tensile strength can reach 3.325 KN / m, and the wet strength retention rate is 38.8%.

[0040] Example 3

[0041] (1) removing lignin, hemicellulose and the like from lianas, extracting cellulose and preparing cellulose paper. The cellulose paper is immersed in a 10% sodium hydroxide solution, the mass ratio of the absolute dry mass of the cellulose paper to the sodium hydroxide solution being 1:30, heated at 40° C. for 1 h, and washed with clean water to obtain a first intermediate;

[0042] (2) immersing the first intermediate in an alkali / urea mixed solution and placing it in a -20°C environment to fully react for 4 hours to obtain a second intermediate;

[0043] (3) The second intermediate was washed with clean water and placed in a hot press at 90°C and 10 MPa until completely dried.

[0044] The obtained super strong water-resistant paper has a thickness of 70 μm, a dry tensile strength of up to 10.45 KN / m, a wet tensile strength of up to 5.23 KN / m, and a wet strength retention rate of 50%.

[0045] Example 4

[0046] (1) removing lignin, hemicellulose, etc. from lianas, extracting cellulose and preparing cellulose paper. Immersing the cellulose paper in a 10% potassium hydroxide solution, wherein the mass ratio of the cellulose paper to the potassium hydroxide solution is 4:30, heating at 30° C. for 30 min, and washing with clean water to obtain a first intermediate;

[0047] (2) immersing the first intermediate in a NN dimethylacetamide solution, placing it in a 160°C environment to fully react for 5 minutes, then cooling it to 105°C, adding lithium chloride and keeping it warm for 2 hours, the mass ratio of lithium chloride to NN dimethylacetamide solution is 1:10, and standing it for 30 minutes to obtain a second intermediate;

[0048] (3) The second intermediate was washed with clean water and placed in a hot press at 30°C and 20 MPa until completely dried.

[0049] The thickness of the obtained super strong water-resistant paper is 55 μm, the dry tensile strength can reach 10.93 KN / m, the wet tensile strength can reach 5.7 KN / m, and the wet strength retention rate is 52.2%.

[0050] Example 5

[0051] (1) removing lignin, hemicellulose, etc. from the herb, extracting cellulose and preparing cellulose paper. Immersing the cellulose paper in a 5% sodium hydroxide solution, with the mass ratio of the cellulose paper to the sodium hydroxide solution being 5:30, heating at 20° C. for 5 h, and washing with clean water to obtain a first intermediate;

[0052] (2) immersing the first intermediate in a NN dimethylacetamide solution, placing it in a 160°C environment to fully react for 1 hour, then cooling it to 105°C, adding lithium chloride and keeping it warm for 10 minutes, the mass ratio of lithium chloride to NN dimethylacetamide solution is 1:10, and standing it for 5 minutes to obtain a second intermediate;

[0053] (3) The second intermediate was washed with clean water and placed in an oven at 90°C until completely dried.

[0054] The obtained super strong water-resistant paper has a thickness of 200 μm, a dry tensile strength of up to 7.6 KN / m, a wet tensile strength of up to 2.85 KN / m, and a wet strength retention rate of 47.5%.

[0055] Example 6

[0056] (1) removing lignin, hemicellulose, etc. from the herb, extracting cellulose and preparing cellulose paper. Immersing the cellulose paper in a 20% calcium hydroxide solution, with the mass ratio of the cellulose paper to the calcium hydroxide solution being 1:30, heating at 60° C. for 30 min, and washing with clean water to obtain a first intermediate;

[0057] (2) immersing the first intermediate in a copper ammonia solution and placing it in a 60° C. environment to fully react for 4 hours to obtain a second intermediate;

[0058] (3) The second intermediate was washed with anhydrous ethanol and placed in an oven at 40°C until completely dried.

[0059] The thickness of the obtained super strong water-resistant paper is 200 μm, the dry tensile strength can reach 7.6 KN / m, the wet tensile strength can reach 7.63.8 KN / m, and the wet strength retention rate is 50%.

[0060] Example 7

[0061] (1) removing lignin, hemicellulose, etc. from the herb, extracting cellulose and preparing cellulose paper. The cellulose paper is immersed in a 20% potassium hydroxide solution, the mass ratio of the cellulose paper to the potassium hydroxide solution is 5:30, heated at 60° C. for 15 minutes, and washed with water to obtain a first intermediate;

[0062] (2) immersing the first intermediate in an alkali / urea mixed solution and placing it in a -5°C environment to fully react for 5 hours to obtain a second intermediate;

[0063] (3) The second intermediate was washed with clean water and placed in an oven at 30°C until completely dried.

[0064] The thickness of the obtained super strong water-resistant paper is 200 μm, the dry tensile strength can reach 5.7 KN / m, the wet tensile strength can reach 2.85 KN / m, and the wet strength retention rate is 50%.

[0065] Comparative Example 1

[0066] Lignin, hemicellulose and the like in the wood are removed, cellulose is extracted and prepared into cellulose paper. The cellulose paper is immersed in 18% sodium hydroxide solution, the mass ratio of the absolute dry mass of the cellulose paper to the sodium hydroxide solution is 1:30, heated at 50°C for 30 minutes, washed with water to obtain comparative example 1 paper, washed with anhydrous ethanol, and placed in a hot press at 60°C and 20MPa until completely dried.

[0067] The SEM image of the water-resistant paper obtained in Comparative Example 1 is shown in Figure 3, its thickness is 50μm, the dry tensile strength can reach 3.37KN / m, the wet tensile strength can reach 0.71KN / m, and the wet strength retention rate is 21.07%.

[0068] Comparative Example 2

[0069] (2) Remove lignin, hemicellulose, etc. from the wood, extract cellulose and prepare cellulose paper. Immerse the cellulose paper in N-N-dimethylacetamide solution, place it in a 160°C environment for full reaction for 20 minutes, then cool it to 105°C and add lithium chloride for 30 minutes, the mass ratio of lithium chloride to N-N-dimethylacetamide solution is 1:10, let it stand for 10 minutes, wash it with clean water to obtain comparative example 2 paper, wash it with anhydrous ethanol, and place it in a hot press at 60°C and 20MPa until it is completely dried.

[0070] The SEM image of the water-resistant paper of Comparative Example 2 is shown in Figure 4 , its thickness is 40μm, the dry tensile strength can reach 3.95KN / m, the wet tensile strength can reach 0.54KN / m, and the wet strength retention rate is 13.67%.

[0071] like Figure 5 The base paper is shown (see the SEM image of the base paper Figure 2 ), wet tensile strength diagram of the water-resistant paper prepared in Example 1, Comparative Example 1 and Comparative Example 2. It can be clearly seen from the figure that the wet tensile strength of the water-resistant paper prepared in Example 1 is significantly better than that of the base paper and the water-resistant papers of Comparative Examples 1 and 2, which shows that the water resistance of the water-resistant paper of the present invention is significantly improved.

Claims

1. A super water-resistant paper, characterized in that: The super water-resistant paper is a dense structure composed of twisted and entangled micron fibers and in-situ regenerated fibers. The in-situ regenerated nanofibers form a dense membrane structure to tightly wrap the connection between the micron fibers.

2. The super water-resistant paper according to claim 1, characterized in that: The wet tensile strength of the super strong water-resistant paper is 2.85-9.5 KN / m, the dry tensile strength is 7.6-11.4 KN / m, and the wet strength retention rate is 25%-83%.

3. The super water-resistant paper according to claim 1, characterized in that: The thickness of the super water-resistant paper is 50-200 μm, and the density is 1.0-1.4 g·cm -3 .

4. A method for preparing the super water-resistant paper according to any one of claims 1 to 3, characterized in that: The following steps are involved: Immersing cellulose paper in a treatment solution A to obtain a first intermediate; the treatment solution A is one or more of a sodium hydroxide solution, a calcium hydroxide solution, and a potassium hydroxide solution; The first intermediate is immersed in a treatment solution B to dissolve part of the fiber to obtain a second intermediate; the treatment solution B is one or more of an alkali / urea mixed solution, a lithium chloride / NN dimethylacetamide solution, an N-methylmorpholine-N-oxide solution, an ion solution, and a cuprammonia solution; The second intermediate is washed and dried to obtain super water-resistant paper.

5. The method for preparing super water-resistant paper according to claim 4, characterized in that: The cellulose in the cellulose paper comes from woody plants, vines or herbaceous plants.

6. The method for preparing super water-resistant paper according to claim 4, characterized in that: The concentration of the treatment solution A is 1% to 20%, and the treatment temperature is 0 to 60°C.

7. The method for preparing super water-resistant paper according to claim 4, characterized in that: The mass ratio of the absolute dry mass of the cellulose paper to the A treatment solution is 1 to 5:

30. The treatment method of the A treatment solution comprises: soaking in the A treatment solution at 0 to 60° C. for 10 minutes to 5 hours, and washing with water after the treatment is completed.

8. The method for preparing super water-resistant paper according to claim 4, characterized in that: The treatment temperature of the B treatment solution is -20 to 170° C., and the treatment time is 5 min to 5 h.

9. The method for preparing super water-resistant paper according to claim 4, characterized in that: The second intermediate obtained after treatment with the B treatment solution needs to be left to stand for 1 to 30 minutes.

10. The method for preparing super water-resistant paper according to claim 4, characterized in that: The drying method includes air drying at room temperature, oven drying or hot press drying, and the drying temperature is 20-120°C.

Citation Information

Patent Citations

  • Cellulose waterproof paper and preparation method thereof

    CN113026420A

  • Water-resistant transparent paper as well as preparation method and application thereof

    CN113123158A

  • High-strength pure cellulose hydrogel and preparation method thereof

    CN115819799A

  • High-strength paper and preparation method thereof

    CN117626694A

  • Pure cellulose water-resistant and oil-resistant paper and preparation method thereof

    CN117646351A