Reflection crack resistant white-to-black pavement structure and implementation method

By using a combined structure of old cement pavement, modified asphalt waterproof bonding layer, large-particle gravel layer, high-viscosity asphalt gravel layer and high-modulus asphalt concrete layer in white-to-black pavement, the problem of reflective cracks is solved. It achieves high strength, low cost and high durability road surface repair effects.

CN118996945APending Publication Date: 2024-11-22BEIJING ZHONGTIAN ROAD IND TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310548755.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The problem of reflective cracks in the existing white-to-black pavement technology is difficult to effectively solve. Traditional methods such as increasing the thickness of asphalt surface layer and laying geosynthetic interlayers, etc. are not ideal, and the cost and construction complexity are high.

Method used

Using a structural combination including old cement pavement, modified asphalt waterproof bonding layer, large-particle gravel layer, high-viscosity asphalt gravel layer, high-modulus asphalt concrete layer and wear layer, it is used to crush modified asphalt and large-particle gravel layer. The combination of the gradient connection of stone and the combination of high-modulus asphalt concrete forms a pavement structure with high strength and strong deformation ability, reducing the asphalt mixing process and reducing costs.

Benefits of technology

Effectively resist reflective cracks, retain the high strength of the original cement pavement, reduce the thickness of asphalt mixture, improve driving comfort and road durability, reduce construction complexity and cost, and has good market promotion value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996945A_ABST
    Figure CN118996945A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of road engineering, and particularly relates to a reflection-crack-resistant white-to-black pavement structure and an implementation method, and the reflection-crack-resistant white-to-black pavement structure comprises an old cement pavement, a modified asphalt waterproof bonding layer, a large-particle-size macadam layer, a high-viscosity asphalt macadam layer, a high-modulus asphalt concrete layer and a wearing layer. The modified asphalt waterproof bonding layer is arranged at the upper end of the old cement pavement, the large-particle-size gravel layer is arranged at the upper end of the modified asphalt waterproof bonding layer, the original strength of the old cement pavement is fully utilized, an old cement slab does not need to be crushed or removed, and the strength of large gravel is high enough under the boundary constraint condition. Through combination of materials and structures, the problem of reflection cracks of the white-to-black pavement is solved, the asphalt mixing process is reduced, energy conservation and emission reduction are achieved, the manufacturing cost is low, and the good market popularization value is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road engineering, and in particular to a white-to-black road surface structure capable of resisting reflective cracks and an implementation method thereof. Background Art

[0002] Cement pavement has high structural strength and long service life, but it is difficult to restore the original pavement performance after repairing the defects, and the driving comfort is poor. Overlaying asphalt concrete on old cement pavement - changing from white to black can significantly improve the travel experience of residents and is accepted by many cities in my country. The white-to-black pavement has high strength and strong deformation resistance, and rarely has deformation-related diseases, but reflective cracks have always been the biggest challenge facing this solution. There are various forms of measures to prevent reflective cracks. The road engineering community at home and abroad is still in the process of testing and exploring measures to prevent and mitigate reflective cracks. The main methods used so far are as follows: ① Increase the thickness of the asphalt surface layer; ② Lay a geosynthetic interlayer; ③ Add a stress absorption layer; ④ Set up a large-size asphalt mixture intermediate layer; ⑤ Set up a graded crushed stone relief layer; ⑥ Pre-cut joints in the semi-rigid reinforcement layer + geosynthetics; ⑦ Crushing and stabilizing the old cement concrete slab.

[0003] Although installing geotextiles, glass fiber grids, modified asphalt stress absorption layers, etc. between the old cement concrete pavement and the asphalt overlay has a certain effect on delaying reflective cracks, reflective cracks will still appear after a period of time, and the effect is not ideal; excessively increasing the thickness of the asphalt overlay or adding an intermediate layer of large-particle asphalt mixture is not economical; crushing plate impact compaction reduces the bearing capacity of the original pavement and increases the complexity of design and construction. It is only economically reasonable to use it when the road panel is severely broken and the breakage rate is high. For many cement pavements with good strength, using the crushing plate method to eliminate reflective cracks is a waste of resources.

[0004] Some countries have conducted research on the use of graded crushed stone layers to prevent reflective cracks. A high-quality graded crushed stone crack mitigation layer is laid between the old cement concrete road slab and the asphalt overlay layer. This inverted structure with soft top and hard bottom not only fully utilizes the residual strength of the old cement concrete pavement, but also reduces the reflective cracks of the asphalt overlay layer. It is a relatively reasonable measure in terms of both technical and economic efficiency. my country has also made some attempts in this regard and achieved some research results. However, graded crushed stone requires curing, has a long construction period, is easy to segregate, has high construction requirements, and local segregation will bring huge hidden dangers to the quality of the project. In addition, graded crushed stone is a loose layer with poor deformation resistance. A thicker asphalt overlay is required to effectively withstand traffic loads, and the cost is relatively high.

[0005] Reflective cracks are a common problem of conventional white-to-black pavement solutions. There are currently two main methods with good solutions: one is to increase the thickness of the asphalt mixture layer, and the other is to gravel the cement pavement. Increasing the thickness of the asphalt mixture layer can delay the time for cracks to reflect to the surface, but it cannot completely avoid the occurrence of reflective cracks; the gravel technology of cement pavement disperses the concentrated cracks among the gravels, eliminating stress concentration, and has a better solution effect on reflective cracks, but the original structural strength of the cement pavement is almost completely lost, and the upper layer needs to be re-paved with a water-stabilizing layer or a thicker asphalt concrete layer. After the water-stabilizing layer is added, the problem of reflective cracks in the water-stabilizing layer also arises, and the cost of thickening the asphalt concrete layer is high. Summary of the invention

[0006] The purpose of the present invention is to provide a white-to-black pavement structure and implementation method that can resist reflective cracks, so as to solve the problems raised in the above-mentioned background technology.

[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a white-to-black pavement structure that resists reflective cracks, comprising an old cement pavement, a modified asphalt waterproof bonding layer, a large-size crushed stone layer, a high-viscosity asphalt crushed stone layer, a high-modulus asphalt concrete layer and a wear layer, wherein the modified asphalt waterproof bonding layer is arranged on the upper end of the old cement pavement, the large-size crushed stone layer is arranged on the upper end of the modified asphalt waterproof bonding layer, the high-viscosity asphalt crushed stone layer is arranged on the upper end of the large-size crushed stone layer, the high-modulus asphalt concrete layer is arranged on the upper end of the high-viscosity asphalt crushed stone layer, and the wear layer is arranged on the upper end of the high-modulus asphalt concrete layer.

[0008] Preferably, the old cement pavement is an old cement concrete pavement that has been treated for bottom hollowing, and surface damage, cracking, and broken slabs are allowed to exist.

[0009] Preferably, the modified asphalt waterproof bonding layer is sprinkled with 2.0-2.4 kg / m 2 .

[0010] Preferably, the large-size crushed stone layer is crushed stone with a particle size of 20-30 mm and a thickness of 5-15 cm, and the crushed stone index meets the technical requirements for coarse aggregate in the highway asphalt pavement construction specifications.

[0011] Preferably, the high-viscosity asphalt gravel layer uses 3-5 mm gravel and high-viscosity modified asphalt, the high-viscosity modified asphalt has a dynamic viscosity of >20000 Pa·s at 60°C, and the asphalt dosage is 2-4 kg / m 2 The crushed stone index meets the technical requirements for coarse aggregate in the highway asphalt pavement construction specifications.

[0012] Preferably, the high-viscosity modified asphalt is poured into the upper 2-5 cm of the lower large-diameter crushed stone layer to form a gradual connection structure.

[0013] Preferably, the high modulus asphalt concrete layer has a thickness of 4-9 cm and a dynamic stability of the mixture higher than 8000 times / mm.

[0014] Preferably, the wear layer is made of wear-resistant aggregate and high-performance binder, with a thickness of 1.5-2.5 cm.

[0015] An implementation method of a white-to-black pavement structure that resists reflective cracks as claimed in any one of claims 1 to 8, wherein the specific steps of the implementation method are as follows:

[0016] Step 1: Roughen the original road surface to ensure the surface roughness and treat the old cement road surface for defects, mainly including grouting the original cement road surface for mud pumping and the bottom of the board to ensure the balanced bearing capacity of the road surface;

[0017] Step 2: Spread modified asphalt, 2.0-2.4kg / m 2 ;

[0018] Step 3: Pave large-size gravel with a particle size of 20-30mm and a thickness of 5-15cm, and vibrate and compact it with a heavy-duty roller;

[0019] Step 4: Spread high-viscosity modified asphalt on the surface of the large-size gravel layer, and simultaneously spread gravel with a size of 3-5mm. The gravel coverage rate is 60-80%, the less the better. It only needs to be rolled by a heavy-duty rubber-wheeled roller after the gravel is spread. After the rubber-wheeled roller is rolled, the excess gravel should be cleaned and recycled;

[0020] Step 5: Spread emulsified asphalt on the surface of the high-viscosity asphalt gravel layer after construction, and pave a high-modulus asphalt concrete layer with a thickness of 4-9cm;

[0021] Step 6: Sprinkle modified emulsified asphalt on the surface of high modulus asphalt concrete and lay the wearing course.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention utilizes the loose structure of large-size crushed stone to reduce the concentrated stress at the cracks of cement pavement, avoids the segregation risk of graded crushed stone scheme, pours modified asphalt into the large-size crushed stone layer for connection, forms a gradually connected structure, gradually eliminates stress, fills the upper layer with small-size crushed stone to fill the gap, and the modified asphalt, large-size crushed stone and small-size crushed stone form a stress absorption layer with strong deformation ability. The upper high modulus asphalt concrete structure has strong anti-deformation ability and high bearing capacity, and the surface wear layer is comfortable to drive and has good wear resistance. The high strength of the original cement pavement is retained to provide strong support for the upper asphalt mixture. The upper layer only needs a thinner asphalt mixture. While driving is comfortable, the pavement has high durability. The present invention fully utilizes the original strength of the old cement pavement, does not need to crush or remove the cement board of the old road, utilizes the characteristics of large crushed stone with sufficiently high strength under boundary constraints, and solves the problem of reflective cracks in the white-to-black pavement through the combination of materials and structures, reduces the asphalt mixing process, saves energy and reduces emissions, has low cost, and has good market promotion value. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the white-to-black pavement structure to resist reflective cracks.

[0025] In the figure: 1 old cement pavement, 2 modified asphalt waterproof bonding layer, 3 large-size gravel layer, 4 high-viscosity asphalt gravel layer, 5 high modulus asphalt concrete layer, 6 wear layer. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "front", "back", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0028] See also Figure 1The present invention provides a technical solution: a white-to-black pavement structure for resisting reflective cracks, comprising an old cement pavement 1, a modified asphalt waterproof bonding layer 2, a large-size crushed stone layer 3, a high-viscosity asphalt crushed stone layer 4, a high-modulus asphalt concrete layer 5 and a wear layer 6, characterized in that the modified asphalt waterproof bonding layer 2 is arranged on the upper end of the old cement pavement 1, the large-size crushed stone layer 3 is arranged on the upper end of the modified asphalt waterproof bonding layer 2, the high-viscosity asphalt crushed stone layer 4 is arranged on the upper end of the large-size crushed stone layer 3, the high-modulus asphalt concrete layer 5 is arranged on the upper end of the high-viscosity asphalt crushed stone layer 4, and the wear layer 6 is arranged on the upper end of the high-modulus asphalt concrete layer 5. The modified asphalt waterproof bonding layer 2 is an SBS modified asphalt waterproof bonding layer, which plays a role in sealing cracks in the cement pavement and preventing water from infiltrating and affecting the roadbed. The asphalt penetrates into the seams between the damaged cement plates to stabilize the old cement plates, and the upper large crushed stones are bonded to the old cement pavement to form constraints on the upper large-size crushed stone layer.

[0029] The modified asphalt waterproof bonding layer 2 can prevent moisture from the upper layer from entering the lower layer to avoid affecting the roadbed. The large-size gravel layer 3 can effectively reduce the concentrated stress of the old cement pavement and disperse and release it. The high-viscosity asphalt gravel layer 4 fixes the upper part of the large-size gravel layer 3 to facilitate the construction of the upper road surface, and forms an asphalt-rich gravel layer with strong deformation resistance, further reducing the stress transmitted from the gravel layer and providing strong support for the upper road surface; the high-modulus asphalt concrete layer 5 has a strong bearing capacity and a strong ability to resist road loads, reducing the deformation amplitude of the road surface and reducing the risk of stress cracking; the wear layer 6 provides comfortable and durable driving performance for the road surface.

[0030] The old cement pavement 1 is an old cement concrete pavement that has been treated for hollowing out of the bottom of the slab. Surface damage, cracking, and broken slabs are allowed to exist. The stability of the old cement pavement 1 is crucial to the long-term use of the road and is the basis for the durability of the road.

[0031] Modified asphalt waterproof bonding layer 2 Sprinkle modified asphalt 2.0-2.4kg / m 2 .

[0032] The large-size crushed stone layer 3 is a crushed stone with a particle size of 20-30 mm and a thickness of 5-15 cm. The crushed stone index meets the technical requirements for coarse aggregate in the highway asphalt pavement construction specification. The large-size crushed stone layer 3 can effectively reduce the concentrated stress of the old cement pavement and disperse it. The large-size crushed stone avoids the maintenance and segregation of graded crushed stone, has higher stability and low cost.

[0033] High-viscosity asphalt gravel layer 4, using 3-5mm gravel and high-viscosity modified asphalt, the dynamic viscosity of high-viscosity modified asphalt at 60℃>20000Pa·s, the asphalt dosage is 2-4kg / m 2The crushed stone index meets the technical requirements of coarse aggregate in the highway asphalt pavement construction specifications. A large amount of high-viscosity modified asphalt is poured into the large crushed stone, forming an asphalt crushed stone structure with gradually decreasing asphalt from top to bottom. The stress at the bottom cracks is transmitted step by step, and the upward deformation capacity of the crushed stone layer decreases step by step, releasing the concentrated stress of the bottom layer in stages. The high-viscosity asphalt crushed stone layer fixes the upper part of the large-size crushed stone layer, which is convenient for the construction of the upper asphalt pavement and provides strong support for the upper pavement.

[0034] High-viscosity modified asphalt is poured into the upper 2-5 cm of the lower large-size gravel layer to form a gradual connection structure.

[0035] The thickness of the high modulus asphalt concrete layer 5 is 4-9 cm, and the dynamic stability of the mixture is higher than 8000 times / mm. The high modulus asphalt concrete layer 5 has a strong bearing capacity and a strong ability to resist road surface loads, thereby reducing road surface deformation and the risk of fatigue cracking.

[0036] The wear layer 6 is made of wear-resistant aggregate and high-performance binder with a thickness of 1.5-2.5cm. The ultra-thin overlay surface is beautiful and provides comfortable and durable driving performance for the road surface.

[0037] An implementation method of a white-to-black pavement structure that resists reflective cracks as claimed in any one of claims 1 to 8, wherein the specific steps of the implementation method are as follows:

[0038] Step 1: Roughen the original road surface to ensure the surface roughness and treat the old cement road surface for defects, mainly including grouting the original cement road surface for mud pumping and the bottom of the board to ensure the balanced bearing capacity of the road surface;

[0039] Step 2: Spread modified asphalt. The modified asphalt uses SBS modified asphalt, 2.0-2.4kg / m 2 ;

[0040] Step 3: Pave large-size gravel with a particle size of 20-30mm and a thickness of 5-15cm. The width needs to be widened by one meter twice on the basis of the upper bearing layer or the curbstones form a constraint on the large-size gravel layer, and vibrate and roll it with a heavy roller;

[0041] Step 4: Sprinkle high-viscosity modified asphalt on the surface of the large-size gravel layer, and simultaneously spread gravel with a particle size of 3-5mm. The gravel coverage rate is 60-80%, the less the better. It is only necessary to roll the gravel with a heavy-duty rubber-wheel roller after the gravel is spread. After the rubber-wheel roller rolls, clean and recycle the excess gravel. After the gravel is spread, use a heavy-duty roller for vibration rolling to ensure the stability of the gravel.

[0042] Step 5: Spread emulsified asphalt on the surface of the high-viscosity asphalt gravel layer after construction, and pave a high-modulus asphalt concrete layer with a thickness of 4-9 cm. The high-modulus asphalt mixture has no restrictions on materials, grading and additives, and the dynamic stability (60°C, 0.7MPa) is higher than 8000 times / mm;

[0043] Step 6: Add 1.5-2.5cm ultra-thin overlay, spread modified emulsified asphalt on the surface of high modulus asphalt concrete, and lay the wear layer. The ultra-thin overlay asphalt mixture has no restrictions on materials, grading and additives. The wear layer directly bears the vehicle load, and has high requirements for the adhesion of the binder. The mixture scattering loss should be less than 5%.

[0044] Example:

[0045] The thickness of each layer of the structure for converting the old cement pavement from white to black is set as shown in the following table, and the total thickness of the overlay is 17cm.

[0046] Pavement level name Thickness, cm 2 Waterproof adhesive layer - 3 Large-size gravel layer 9 4 High viscosity asphalt gravel layer - 5 High modulus asphalt concrete 6 6 Wear layer 2

[0047] Step 1: Clean the original cement pavement where mud is pumped, use a heavy truck to load the cement slab, reinforce or replace the unstable slab surface under pressure to ensure balanced bearing capacity of the pavement;

[0048] Step 2, spreading a modified asphalt waterproof bonding layer;

[0049] The modified asphalt uses SBS modified asphalt, and the spreading amount is 2.4kg / m 2 , the spreading temperature is 180℃.

[0050] SBS modified asphalt meets the following technical requirements

[0051]

[0052]

[0053] Step 3: Add a lime-fly ash soil layer with a width of 1m and a height of 18cm on the shoulders of both sides of the old cement pavement to widen the road and restrain the large-size gravel layer. Pave large-size gravel with a particle size of 20-30mm and a thickness of 9cm, and use a heavy roller for vibration compaction.

[0054] Step 4: Spread high-viscosity asphalt on the surface of the large-size crushed stone layer at a temperature of 160°C and a spreading amount of 3-4 kg / m 2 . And simultaneously spread gravel with a particle size of 3-5mm, and the gravel coverage rate is suitable for non-stick wheels. After the gravel is spread, use a heavy roller to vibrate and roll it to ensure the stability of the gravel. High-viscosity modified asphalt requires a dynamic viscosity of more than 20,000 Pa·s at 60°C. The spreading temperature is 20°C lower than step 2. The asphalt viscosity is relatively large and it is not easy to form accumulation at the bottom of the gravel layer.

[0055] The large-size crushed stone layer has been rolled once after paving, but it still has a large void ratio, which is conducive to the next step of asphalt pouring. After the asphalt is poured, it is rolled uniformly to ensure the depth of asphalt pouring and the good bonding strength and deformation capacity of the upper part of the large-size crushed stone layer;

[0056] Step 5: paving a high modulus asphalt concrete layer with a thickness of 6 cm;

[0057] The selected coarse and fine aggregates and fillers all meet the requirements of the specifications. The asphalt used is A70# asphalt, and the additive is the rubber-plastic composite additive R&P produced by Beijing Zhongtian Road Technology Co., Ltd.

[0058] The grading table of AC-20C is as follows:

[0059]

[0060] The mixture is mixed in a "direct addition, dry mixing" way. First, various grades of aggregate and R&P high modulus agent are added and dry mixed for 10 seconds, and then asphalt and mineral powder are added. The single-plate mixing cycle is 45 seconds, of which R&P and aggregate are dry mixed for more than 10 seconds. The discharge temperature of the mixture is 185°C, and the performance is shown in the following table.

[0061] Technical indicators unit result Technical requirements Gross volume relative density / 2.357 Measured Void ratio % 3.5 Measured Dynamic stability (60℃, 0.7MPa) Times / mm 12486 ≥8000 Stability kN 14.27 ≥10 Stream Value 0.1mm 35 15-40 Residual stability % 88 ≥85 Freeze-thaw splitting residual strength ratio TSR % 85 ≥80 Low temperature bending failure strain (-10℃) με 3165 ≥2500

[0062] Paving and rolling are carried out according to normal production organization;

[0063] Step 6: Add 1.5-2.5cm ultra-thin cover

[0064] The selected coarse and fine aggregates and fillers all meet the requirements of the specifications. The asphalt used is A70# asphalt, and the additive is the high-elastic and anti-cracking additive VE produced by Beijing Zhongtian Road Technology Co., Ltd.

[0065] The grading of mineral materials adopts ZTS-10, and the grading table is as follows

[0066]

[0067]

[0068] The mixture is mixed in a "direct addition, dry mixing" manner. First, various aggregates and VE are added and dry mixed for 10 seconds, followed by the addition of asphalt and mineral powder. The mixing cycle of a single plate is 50 seconds, and the discharge temperature of the mixture is 165°C. The performance is shown in the following table.

[0069] Technical indicators unit result Technical requirements Theoretical maximum relative density <![CDATA[g / cm 3 ]]> 2.495 Measured Void ratio % 3.5 3~5 Stability KN 9.9 ≥8 Residual stability % 92.9 ≥85 Freeze-thaw splitting residual strength ratio % 87.1 ≥80 Kentucky Fort scattered losses % 1.5 ≤5 Rutting dynamic stability (60℃) Times / mm 3665 ≥3000 Low temperature bending test (-10℃) failure strain με 3247 ≥3000

[0070] Paving and rolling are carried out according to normal production organization.

[0071] The white-to-black pavement structure and implementation method provided by the present invention fully utilize the original strength of the old cement pavement, do not need to crush or remove the old cement slab, utilize the characteristic of large crushed stones with sufficient strength under boundary constraints, and solve the problem of reflective cracks in the white-to-black pavement through the combination of materials and structures. It reduces asphalt mixing process, saves energy and reduces emissions, has low cost, and has good market promotion value.

[0072] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the attached claims rather than the above description. Therefore, it is intended to include all changes within the meaning and scope of the equivalent elements of the claims in the present invention, and any figure marks in the claims should not be regarded as limiting the claims involved.

[0073] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A white-to-black pavement structure for resisting reflective cracks, comprising an old cement pavement (1), a modified asphalt waterproof bonding layer (2), a large-size crushed stone layer (3), a high-viscosity asphalt crushed stone layer (4), a high-modulus asphalt concrete layer (5) and a wear layer (6), characterized in that: The modified asphalt waterproof bonding layer (2) is arranged on the upper end of the old cement pavement (1), the large-size crushed stone layer (3) is arranged on the upper end of the modified asphalt waterproof bonding layer (2), the high-viscosity asphalt crushed stone layer (4) is arranged on the upper end of the large-size crushed stone layer (3), the high-modulus asphalt concrete layer (5) is arranged on the upper end of the high-viscosity asphalt crushed stone layer (4), and the wear layer (6) is arranged on the upper end of the high-modulus asphalt concrete layer (5).

2. A white-to-black pavement structure for resisting reflective cracks according to claim 1, characterized in that: The old cement pavement (1) is an old cement concrete pavement that has been treated to have hollowed-out bottoms, and surface damage, cracks, and broken boards are allowed to exist.

3. The white-to-black pavement structure for resisting reflective cracks according to claim 1, characterized in that: The modified asphalt waterproof bonding layer (2) is sprinkled with 2.0-2.4 kg / m of modified asphalt. 2 .

4. The white-to-black pavement structure for resisting reflective cracks according to claim 1, characterized in that: The large-size crushed stone layer (3) is crushed stone with a particle size of 20-30 mm and a thickness of 5-15 cm. The crushed stone index meets the technical requirements for coarse aggregate in the highway asphalt pavement construction specifications.

5. The white-to-black pavement structure for resisting reflective cracks according to claim 1, characterized in that: The high-viscosity asphalt gravel layer (4) is made of 3-5 mm gravel and high-viscosity modified asphalt, the dynamic viscosity of the high-viscosity modified asphalt at 60° C. is greater than 20000 Pa·s, and the asphalt dosage is 2-4 kg / m 2 The crushed stone index meets the technical requirements for coarse aggregate in the highway asphalt pavement construction specifications.

6. A white-to-black pavement structure for resisting reflective cracks according to claim 5, characterized in that: The high-viscosity modified asphalt is poured into the upper 2-5 cm of the lower large-diameter crushed stone layer to form a gradual connection structure.

7. The white-to-black pavement structure for resisting reflective cracks according to claim 1, characterized in that: The high modulus asphalt concrete layer (5) has a thickness of 4-9 cm, and the dynamic stability of the mixture is higher than 8000 times / mm.

8. The white-to-black pavement structure for resisting reflective cracks according to claim 1, characterized in that: The wear layer (6) is made of wear-resistant aggregate and high-performance binder, and has a thickness of 1.5-2.5 cm.

9. A method for implementing a white-to-black road surface structure that resists reflective cracking as claimed in any one of claims 1 to 8, characterized in that: The specific steps of the implementation method are as follows: Step 1: Roughen the original road surface to ensure the surface roughness and treat the old cement road surface for defects, mainly including grouting the original cement road surface for mud pumping and the bottom of the board to ensure the balanced bearing capacity of the road surface; Step 2: Spread modified asphalt, 2.0-2.4kg / m 2 ; Step 3: Pave large-size gravel with a particle size of 20-30mm and a thickness of 5-15cm, and vibrate and compact it with a heavy-duty roller; Step 4: Spread high-viscosity modified asphalt on the surface of the large-size gravel layer, and simultaneously spread gravel with a size of 3-5mm. The gravel coverage rate is 60-80%, the less the better. It only needs to be rolled by a heavy-duty rubber-wheeled roller after the gravel is spread. After the rubber-wheeled roller is rolled, the excess gravel should be cleaned and recycled; Step 5: Spread emulsified asphalt on the surface of the high-viscosity asphalt gravel layer after construction, and pave a high-modulus asphalt concrete layer with a thickness of 4-9cm; Step 6: Sprinkle modified emulsified asphalt on the surface of high modulus asphalt concrete and lay the wearing course.