Nickel-based alloy blade overheating structure evaluation method
Through sampling, inlay, polishing and corrosion treatment of nickel-based alloy blades, combined with microscopic observation, it quickly determines whether the blades are overheated due to overheating, solving the problems that are difficult to assess in the existing technology, and achieving rapid assessment and life extension of the blades , improves the safety and efficiency of aircraft engines.
Patent Information
- Application Number
- CN202411116750.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art has failed to effectively assess whether high-temperature alloy blades are overheated due to overheating, resulting in blade failure, affecting the safety and efficiency of aircraft engines.
The overheating structure evaluation method of nickel-based alloy blades is used to determine whether the blades have γ' phase resolvation, rafting, cracks and grain boundary creep through sampling, inlay, polishing and corrosion treatment, combined with optical microscope observations. Fast judge whether the blade can continue to be used.
A rapid assessment of the overheating structure of nickel-based alloy blades is achieved, and whether the blades can continue to be in service is determined, early failure caused by overtemperature is avoided, the service life of the blades is extended, and the safety and reliability of the engine are improved.
Smart Images

Figure HDA0004993845700000011 
Figure HDA0004993845700000012 
Figure HDA0004993845700000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of blade microstructure assessment, and in particular relates to a method for assessing the overheated structure of a nickel-based alloy blade. Background Art
[0002] Nickel-based high-temperature alloys are based on nickel and are fully strengthened by adding a certain amount of chromium, as well as solid solution strengthening, precipitation strengthening and grain boundary strengthening elements. They are mainly used in industrial fields such as aviation, aerospace, ships and power generation. They are the most widely used, with the most brands, the largest usage and the most important status. In the entire field of high-temperature alloys, nickel-based high-temperature alloys occupy a particularly important position. Compared with iron-based and cobalt-based alloys, nickel-based alloys have better high-temperature properties, good oxidation resistance and corrosion resistance. It can be said that the development of nickel-based high-temperature alloys has laid the foundation for the development of aviation turbine engines and also determined the development of the aviation industry.
[0003] In aircraft engines, nickel-based high-temperature alloys are mainly used to make hot-end components, such as turbine blades, guide vanes, turbine disks, combustion chambers and other parts. As the most important and critical parts of the engine, turbine blades are also the parts with the most demanding service environment. They work in high temperature, high pressure and thermal corrosion environments for a long time. The main reasons for their failure are fatigue, overheating, creep, foreign object damage and thermal corrosion, among which the failure caused by overheating also reaches 6.87%. Generally speaking, during the use of the engine, engine surge, inlet distortion, poor fuel regulation, poor nozzle atomization and operational errors will cause the blades to overheat. Overheating can cause serious damage to turbine blades, resulting in premature failure and even major accidents.
[0004] Nickel-based cast high-temperature alloys use γ phase as the matrix, and add aluminum, titanium, niobium, tantalum, etc. to form γ′ phase for strengthening. The amount of γ′ phase is relatively large, even reaching more than 60%. The best strengthening effect of γ′ phase should be regular in morphology, uniform in distribution and size. Overheating will cause changes in the morphology, amount and size of the γ′ strengthening phase, and the strengthening effect will also be weakened.
[0005] How to quickly determine whether an overheated blade can continue to serve is something worthy of study, and there is currently no relevant public report on how to evaluate the overheated structure of high-temperature alloys. Summary of the invention
[0006] The present invention provides a method for evaluating the overheated structure of a nickel-based alloy blade, which can quickly determine whether an overheated blade can continue to serve.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] The invention discloses a method for evaluating overheated structure of a nickel-based alloy blade, comprising the following steps:
[0009] Take samples for metallographic analysis on the blades, wherein for solid blades, the samples include a longitudinal section sample and a high temperature zone cross section sample, and the longitudinal section sample of the blade with a crown should include the crown part; for hollow blades, the samples include three cross section samples including the high temperature zone and the high stress zone and one longitudinal section sample;
[0010] Using a resin material to inlay the sample to obtain an inlaid part;
[0011] polishing the inlay and etching the inlay in a manner that can reveal the γ′ phase;
[0012] The inlay is magnified and observed, and the microstructure of the tenon in the longitudinal section sample is used as the standard for comparison with the leading edge, mid-chord and trailing edge microstructures in the cross-sectional sample. If any of the following five conditions exist: cracks outside the blade tip, grain boundary creep voids perpendicular to the main axis of the blade, γ' phase re-dissolution with a volume fraction less than 45%, γ' phase re-dissolution and γ' phase rafting, and matrix initial dissolution, the blade is judged to be unusable.
[0013] Compared with the prior art, the present invention has at least the following advantages and beneficial effects:
[0014] The present invention takes samples of the overheated blade and then magnifies and observes them, and uses the tenon tissue as a reference to judge the degradation of the leading edge, mid-chord and trailing edge tissues, so as to quickly judge whether the blade can continue to serve. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0016] Figure 1 This is the microstructure diagram of the cross-section sample of the high temperature zone of the nickel-based alloy blade of a certain engine in Example 1 after it is magnified 5000 times;
[0017] Figure 2 This is the microstructure diagram of the cross-section sample of the high temperature zone of the nickel-based alloy blade of a certain engine in Example 1 after it is magnified 1000 times;
[0018] Figure 3 This is the microstructure diagram of the cross-section sample of the high stress area of the nickel-based alloy blade of a certain engine in Example 1 after it is magnified 5000 times;
[0019] Figure 4This is the microstructure diagram of the cross-section sample of the high stress area of the nickel-based alloy blade of a certain engine in Example 1 after it is magnified 1000 times;
[0020] Figure 5 This is the microstructure diagram of the tenon part of the longitudinal section sample of the nickel-based alloy blade of a certain engine in Example 1 after being magnified 5000 times;
[0021] Figure 6 This is the microstructure diagram of the tenon part of the longitudinal section sample of the nickel-based alloy blade of a certain engine in Example 1 after being magnified 1000 times;
[0022] Figure 7 This is the microstructure diagram of the cross-section sample of the high temperature zone of the nickel-based alloy blade of a certain engine in Example 2 after it was magnified 5000 times;
[0023] Figure 8 This is the microstructure diagram of the cross-section sample of the high temperature zone of the nickel-based alloy blade of a certain engine in Example 2 after it is magnified 1000 times;
[0024] Fig. 9 This is the microstructure diagram of the cross-section sample of the high stress area of the nickel-based alloy blade of a certain engine in Example 2 after being magnified 5000 times;
[0025] Fig.10 This is the microstructure diagram of the cross-section sample of the high stress area of the nickel-based alloy blade of a certain engine in Example 2 after it is magnified 1000 times;
[0026] Fig.11 This is the microstructure diagram of the tenon part of the longitudinal section sample of the nickel-based alloy blade of a certain engine in Example 2 after being magnified 5000 times;
[0027] Fig.12 This is the microstructure diagram of the tenon part of the longitudinal section sample of the nickel-based alloy blade of a certain engine in Example 2 after being magnified 1000 times;
[0028] Fig.13 This is a schematic diagram of the sampling position of solid leaf specimens without crowns;
[0029] Fig.14 This is a schematic diagram of the sampling position of the crowned solid leaf specimen;
[0030] Fig.15 This is a schematic diagram of the sampling position of the hollow blade sample;
[0031] Fig.16 is a schematic diagram of a sample and an inlay mold, wherein the sample is a sample of a hollow blade;
[0032] Fig.17 It is a schematic diagram of the specimen and the inlay mold, where the specimen is 2 groups of specimens with crowned solid leaves. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0034] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.
[0036] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0037] In the description of the present invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, or the positions or positional relationships in which the invented product is usually placed when in use, or the positions or positional relationships commonly understood by those skilled in the art, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0038] The invention discloses a method for evaluating overheated structure of a nickel-based alloy blade, which comprises steps S01 to S04.
[0039] Step S01, taking samples for metallographic analysis on the blade, wherein, for a solid blade, the samples include a longitudinal section sample and a high temperature zone cross-sectional sample 41, and the longitudinal section sample 42 of a crowned blade must include a crown portion 421; for a hollow blade, the samples include three cross-sectional samples including a high temperature zone and a high stress zone and one longitudinal section sample.
[0040] For leaves with different structures, the sampling positions are also different. The specific sampling positions are as follows: Figures 13 to 15 As shown in the figure, the sampling position of the longitudinal section sample is shown in Figures 13 to 15 The AA position in the figure, the sampling position of the cross-section specimen is as shown in Figures 13 to 15 When sampling, the distance between the longitudinal section sample and the exhaust edge 1 is 3.2mm to 6.4mm, leaving enough thickness for metallographic sample preparation.
[0041] When sampling, use an automatic cutting machine, manual cutting machine or wire cutting machine. The blade clamp should not cause blade deformation or cracking of the surface coating. The cutting blade can be made of aluminum / diamond. When cutting, use commercial coolant to cool, control the feed rate to 0.02mm / s~0.04mm / s, and the speed to 2000rpm~2500rpm to ensure that the cutting surface is not damaged or overheated, so as to improve the accuracy of overheated structure assessment.
[0042] Step S02: Inlay the sample with a resin material to obtain an inlaid part.
[0043] When mounting, a mounting machine is used to mount the sample. Specifically, the mounting machine can be a hot pressure mounting machine or a cold vacuum mounting machine. The resin material is phenolic resin, transparent synthetic resin or epoxy resin.
[0044] The mounting parameters of the mounting machine are pressure 140 bar to 180 bar, temperature 150° C. to 180° C. and time 5 min to 8 min to prevent gaps between the sample and the mounting material and to prevent cracks in the coating.
[0045] The distance between the specimen and the edge of the inlay mold 3 is greater than 1.27 mm to prevent the inlay material from cracking. Fig.16 , 17 shown.
[0046] Step S03, polishing the inlay and etching the inlay in a manner that can reveal the γ′ phase.
[0047] In this step, the inlay is polished to obtain an acceptable mirror finish. Specifically, manual polishing or automatic polishing equipment can be used to remove the material on the cut surface, with the removal amount not less than 0.25mm, to obtain an acceptable mirror finish and improve the accuracy of subsequent overheating organization assessment. During polishing, the polishing parameters are pressure 12N~16N, speed 350rpm~450rpm, time 2min~4min, and the polishing agent is generally a suspension composed of water-based diamond and cooling lubricant to prevent coating cracking, sample rounding, overheating, over-polishing, and separation of the sample and the inlay.
[0048] After polishing, the inlay should be etched as soon as possible until the sample surface is golden yellow. The corrosion treatment can adopt a variety of existing corrosion methods that can show the γ′ phase. The copper sulfate wiping method is preferred. This method is relatively simple and convenient. The components and their volume ratios in the etchant are CuSO4:HCl:H2O=1:5:5. Etch the cotton in the etchant and wipe it on the surface of the polished inlay for 3 to 5 times. The sample surface will obviously change color until the sample surface is golden yellow.
[0049] Scratches, stains, under-corrosion and over-corrosion are not allowed on the surface of the inlay.
[0050] Step S04, magnify and observe the inlay, and compare the tissue of the tenon part in the longitudinal section sample with the tissue of the leading edge, mid-chord, and trailing edge in the cross-sectional sample. If there is any of the following five situations: cracks in the area outside the blade tip, grain boundary creep cavities perpendicular to the main axis of the blade, γ' phase re-dissolution with a volume fraction less than 45%, γ' phase re-dissolution and γ' phase rafting, and matrix initial dissolution, the blade is determined to be unusable.
[0051] During observation, use an optical microscope or scanning electron microscope that can magnify 1000 to 5000 times. The observation area should avoid the coating and the coating diffusion area, and the observation point should be about 0.25 mm away from the coating diffusion area.
[0052] During the observation, the tenon structure in the longitudinal section sample is used as the standard, because during the operation of the engine, the temperature of the blade tenon is relatively low, and the microstructure of its cross section is usually not obviously degraded. The microstructure of the tenon can be used as a benchmark for judging the high temperature area of the blade to judge its degradation.
[0053] The typical characteristics of the microstructure of nickel-based alloys are as follows:
[0054] 1. There are a large number of γ' precipitates in the γ matrix. Most alloys usually have cubic γ' precipitates, and some other alloys have non-cubic γ' precipitates.
[0055] 2. Some alloys contain a small amount of island γ eutectics and blocky MC-type carbides, which are mainly located at grain boundaries and interdendritic regions.
[0056] 3. Borides, nitrides and other types of carbides can exist in chain form along the grain boundaries. Other types of carbides such as M6C and M 23 C6.
[0057] The effect of high temperature on microstructure is mainly the change of morphology, content, size and distribution of γ' precipitated phase in matrix caused by high temperature, which is specifically manifested as follows:
[0058] 1. γ' phase coarsening
[0059] Among them, the manifestation of γ' phase coarsening is:
[0060] a. The size of the γ' phase is larger than that of the original microstructure, but the volume fraction is similar.
[0061] b. The shape of the γ' phase is slightly spherical.
[0062] c. Eutectics, carbides, borides and nitrides are not affected.
[0063] 2. γ' phase re-dissolution
[0064] Among them, the manifestation of γ' phase dissolution is:
[0065] a. The size and volume fraction of the γ' phase are reduced.
[0066] b. The shape of the γ' phase is significantly more irregular.
[0067] 3. γ' phase rafting
[0068] Among them, the manifestation of γ' phase rafting is:
[0069] a. The shape of the γ' phase is mainly elongated in one direction.
[0070] b. The volume fraction of γ' phase is similar to that of the original microstructure.
[0071] c. The elongation of the γ' phase is always perpendicular to the direction of local stress.
[0072] Blades in service may have a mixed structure of γ' phase coarsening + rafting or γ' phase dissolution + rafting. Creep voids may also exist in blades in long-term service, mainly near grain boundaries and phase boundaries. Grain boundary voids related to creep preferentially extend in the direction perpendicular to the main axis of the blade body.
[0073] In this regard, when judging whether the blade can continue to be used, if it meets any of the following five conditions, it cannot be used any further; otherwise, it can be used any further.
[0074] The following are the five situations where you cannot continue to use the system:
[0075] 1. There are cracks outside the blade tip;
[0076] 2. Grain boundary creep cavities perpendicular to the main axis of the blade;
[0077] 3. The γ' phase dissolves back and the volume fraction is less than 45%;
[0078] 4. The γ' phase dissolves back and the γ' phase rafts
[0079] 5. Initial dissolution of the matrix.
[0080] Example 1: Taking a nickel-based alloy blade of a certain type of engine as an example, the engine experienced an instantaneous overtemperature of 2°C for 2 seconds. The above method was used to analyze the gas turbine blade sample. The microstructure of the high temperature area, high stress area and tenon part is as follows: Figure 1 to Figure 6 As shown in the figure. Among them, the enlarged image of the sample structure in the cross section of the high temperature zone after magnification 5000 times is shown in the figure Figure 1 As shown in the figure, the high temperature zone cross section sample structure is magnified 1000 times as shown in the figure Figure 2 As shown; the cross-sectional sample structure of the high stress area is magnified 5000 times as shown in Figure 3 The cross-sectional structure of the high stress area is magnified 1000 times as shown in Figure 4 As shown in the figure, the enlarged image of the tenon part of the longitudinal section sample after magnification 5000 times is as follows Figure 5 As shown in the figure, the enlarged image of the tenon part of the longitudinal section sample after magnification 1000 times is as follows Figure 6 Observation comparison Figures 1 to 6 It can be judged that the blade body tissue has degraded, but no overheating tissue characteristics have appeared. The blade can continue to serve. The blade has been used for 900 hours.
[0081] Example 2: Take the nickel-based alloy blade of a certain type of engine as an example. The engine overheated to 300°C. The above method was used to analyze the microstructure of its turbine blade. The microstructures of the high temperature area, high stress area and tenon part are as follows: Figure 7 to Figure 12 As shown in the figure. Among them, the enlarged image of the sample structure in the cross section of the high temperature zone after magnification 5000 times is shown in the figure Figure 7 As shown in the figure, the high temperature zone cross section sample structure is magnified 1000 times as shown in the figure Figure 8 As shown; the cross-sectional sample structure of the high stress area is magnified 5000 times as shown in Fig. 9 The cross-section of the high stress area is magnified 1000 times as shown in the figure. Fig.10 As shown in the figure, the enlarged picture of the tenon part of the longitudinal section specimen after magnification 5000 times is as follows Fig.11 As shown in the figure, the enlarged picture of the tenon part of the longitudinal section specimen after magnification 1000 times is as follows Fig.12 Observation comparison Figure 7 to Figure 12 It can be judged that the tissue in the high-temperature area of the blade has completely dissolved, and the tissue in the high-stress area has shown dissolution and rafting characteristics, showing typical overheating tissue characteristics, and the blade cannot continue to be used.
[0082] The above method only requires metallographic sample preparation materials and equipment and an optical microscope or scanning electron microscope. It can quickly and easily realize the overheating tissue analysis and tissue degradation judgment of nickel-based alloy blades, provide support for the evaluation of whether the blades can continue to be used or the extension of the blade life, and can save a large number of turbine blades and realize the reuse of blades that have reached the end of their service life.
[0083] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for evaluating the overheated structure of nickel-based alloy blades. It is characterized in that The following steps are involved: Take samples for metallographic analysis on the blades, wherein for solid blades, the samples include a longitudinal section sample and a high temperature zone cross section sample, and the longitudinal section sample of the blade with a crown should include the crown part; for hollow blades, the samples include three cross section samples including the high temperature zone and the high stress zone and one longitudinal section sample; Using a resin material to inlay the sample to obtain an inlaid part; polishing the inlay and etching the inlay in a manner that can reveal the γ′ phase; The inlay is magnified and observed, and the microstructure of the tenon in the longitudinal section sample is used as the standard for comparison with the leading edge, mid-chord and trailing edge microstructures in the cross-sectional sample. If any of the following five conditions exist: cracks outside the blade tip, grain boundary creep voids perpendicular to the main axis of the blade, γ' phase re-dissolution with a volume fraction less than 45%, γ' phase re-dissolution and γ' phase rafting, and matrix initial dissolution, the blade is judged to be unusable.
2. A method for evaluating the overheated structure of a nickel-based alloy blade according to claim 1, Features: When taking samples from the blade for metallographic analysis, the distance between the longitudinal section sample and the exhaust edge is 3.2mm to 6.4mm.
3. A method for evaluating the overheated structure of a nickel-based alloy blade according to claim 1, Features: When taking samples for metallographic analysis on the blade, a cutting machine is used for cutting while cooling with a coolant, and the feed rate of the cutting machine is controlled to be 0.02 mm / s to 0.04 mm / s and the rotation speed to be 2000 rpm to 2500 rpm.
4. A method for evaluating the overheated structure of a nickel-based alloy blade according to claim 1, Features: The adopting resin material to embed the sample comprises: The sample is inlaid with an inlay machine, wherein the resin material is phenolic resin, transparent synthetic resin or epoxy resin, and the distance between the sample and the edge of the inlay mold is greater than 1.27 mm.
5. A method for evaluating the overheated structure of a nickel-based alloy blade according to claim 1, Features: When the sample is inlaid with a resin material, an inlay machine is used to inlay the sample, and the inlay parameters of the inlay machine are a pressure of 140 bar to 180 bar, a temperature of 150° C. to 180° C., and a time of 5 min to 8 min.
6. A method for evaluating overheated structure of a nickel-based alloy blade according to claim 1, Features: When the inlay is polished, the removal amount is greater than or equal to 0.25 mm.
7. A method for evaluating the overheated structure of a nickel-based alloy blade according to claim 1, Features: The inlay is polished by a polishing machine, the polishing parameters of the polishing machine are pressure 12N-16N, rotation speed 350rpm-450rpm, and time 2min-4min; the polishing agent of the polishing machine is a suspension composed of water-based diamond and cooling lubricant.
8. A method for evaluating overheated structure of a nickel-based alloy blade according to claim 1, Features: When the inlay is corroded by the etching method that can show the γ′ phase, cotton is corroded in the corrosive agent and wiped on the surface of the polished inlay for 3 to 5 times, wherein the components in the corrosive agent and their volume ratio are CuSO 4 :HCl:H 2 O=1:5:5.